Environmentally friendly waterproofing agent and preparation method thereof
By using environmentally friendly waterproofing agents in alkyd resin coatings, combined with reasonable proportions of drying agents, the problem of rapid drying of drying agents resulting in uneven distribution of waterproofing agents is solved, and rapid drying of alkyd resin coatings is achieved and excellent waterproofing is achieved Take into account both performance.
Patent Information
- Application Number
- CN202410633797.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-05-21
AI Technical Summary
During the construction of alkyd resin coating, the drying agent accelerates the drying speed, but may lead to uneven distribution of the waterproofing agent, affecting the waterproof performance of the coating.
A method of preparing an environmentally friendly waterproofing agent is adopted to form a hydrophobic polymer chain through copolymerization of butyl acrylate, isooctyl acrylate and styrene, and combine vinyl triethoxysilane and methacryloyloxyethyl tri Methyl ammonium chloride, azobisylhydrogen hydrochloride and acidic silica sol form a dense three-dimensional network structure, and a reasonable proportion of drying agents ensures that the alkyd resin coating is quickly dry and hard, while also having excellent waterproof performance.
It realizes that alkyd resin coatings maintain excellent waterproof performance while drying quickly, ensuring that the waterproof performance of the coating does not decrease.
Smart Images

Figure CN118359778B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and particularly relates to an environmentally friendly waterproofing agent and a preparation method thereof. Background Art
[0002] Alkyd resin coating is a synthetic resin coating with alkyd resin as the main film-forming substance. Alkyd resin is a resin formed by the reaction of fatty acids (or their corresponding vegetable oils), dibasic acids and polyols. Commonly used polyols for producing alkyd resins include glycerol, pentaerythritol, trimethylolpropane, etc.; commonly used dibasic acids include phthalic anhydride (i.e. phthalic anhydride), isophthalic acid, etc. Alkyd resin coating has the characteristics of weather resistance, good adhesion, brightness, fullness, etc., and is easy to apply. At the same time, the coating film is soft and has poor waterproof properties, so it is necessary to add a waterproofing agent.
[0003] On the other hand, because alkyd resin itself dries slowly, in order to speed up the drying speed of the coating and shorten the construction time, a drying agent needs to be added to the alkyd resin coating to accelerate the evaporation of the solvent in the coating and / or promote the curing process of the coating.
[0004] However, during the construction of alkyd resin coatings, the accelerated drying effect brought about by the use of driers may negatively affect the performance of waterproofing agents. For example, metal salt driers such as zinc, cobalt, and manganese can accelerate the oxidative polymerization process of oil in the coating, thereby accelerating the drying of the coating film. At the same time, it may cause the waterproofing agent to be unevenly distributed in the coating, unable to form a continuous and uniform waterproof layer, which may lead to a decrease in the overall waterproof performance of the coating. Summary of the invention
[0005] In order to solve the problems existing in the background technology, the present invention provides an environmentally friendly waterproofing agent and a preparation method thereof. When the prepared environmentally friendly waterproofing agent is used together with a metal salt drying agent, it ensures that the prepared alkyd resin coating can quickly dry on the surface and dry thoroughly, while having excellent waterproof performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing an environmentally friendly waterproofing agent comprises the following steps:
[0008] S1, put 45g of butyl acrylate, 24g of isooctyl acrylate, 20g of styrene, 1g of vinyl triethoxysilane, 5g of methacryloyloxyethyl trimethyl ammonium chloride, 60g of 4% polyvinyl alcohol aqueous solution and 10g of 8% acrylamide aqueous solution into a homogenizer for homogenization and ultrasonication to obtain a pre-emulsion;
[0009] S2, take 3 mL of methacryloyloxypropyltrimethoxysilane, 15 mL of deionized water and 8 mL of ethanol, mix them, stir and hydrolyze them at 40°C and pH=3 for 1 h, add 30 mL of acidic silica sol, and react to obtain modified silica sol;
[0010] S3. Pour the pre-emulsion obtained in S1 and the modified silica sol obtained in S2 into a three-necked flask, add 1 g of azobisisobutylimidazole hydrochloride and 276 g of deionized water, and react at 65°C for 6.5 h under nitrogen protection to obtain an environmentally friendly waterproofing agent.
[0011] Furthermore, in S1, at room temperature, the homogenizer is used for homogenization at 5000 r / min for 45-60 min; and the ultrasonic dispersion is performed at 50 Hz for 30 min.
[0012] Furthermore, in S2, 1 M hydrochloric acid solution is used to adjust the pH to 3.
[0013] An environmentally friendly waterproofing agent is prepared by adopting the preparation method.
[0014] Furthermore, the environmentally friendly waterproofing agent is used to prepare a quick-drying waterproof coating; the quick-drying waterproof coating comprises the following raw material components by weight: 45-55 parts of alkyd resin, 10-15 parts of titanium dioxide, 8-12 parts of talcum powder, 0.8-1 part of drying agent, 0.5-0.8 part of dispersant, 0.1-0.2 part of anti-skinning agent, 0.2-0.3 part of environmentally friendly waterproofing agent and 4-7 parts of solvent.
[0015] Furthermore, the drying agent comprises the following raw material components by weight: 2-4 parts of 10% cobalt isooctanoate, 2-4 parts of 12% rare earth isooctanoate, 10-12 parts of 5% calcium isooctanoate, 12-14 parts of 6% iron isooctanoate and 13-15 parts of 9% zinc isooctanoate.
[0016] Furthermore, the titanium dioxide includes rutile titanium dioxide and / or anatase titanium dioxide.
[0017] Furthermore, the particle size of the talcum powder is 1000-1500 mesh, and the oil absorption is 30-35g / 100g.
[0018] Furthermore, the solvent includes xylene and / or 200# solvent oil.
[0019] Furthermore, the preparation method of the quick-drying waterproof coating is as follows: add alkyd resin into a disperser, control the stirring speed at 800-1000rpm / min, then add titanium dioxide, talcum powder, drying agent, dispersant, anti-skinning agent, waterproofing agent and solvent, continue to maintain the stirring speed of 800-1000rpm / min, stir for 10-15min, and obtain a mixture; put the mixture into a grinder and grind it to a fineness of no more than 25μm to obtain a quick-drying waterproof coating.
[0020] This application has the following beneficial effects:
[0021] 1. In the preparation of the environmentally friendly waterproofing agent of the present invention, butyl acrylate, isooctyl acrylate and styrene are used as main monomers to participate in copolymerization reaction to form hydrophobic polymer chains; vinyl triethoxysilane and methacryloyloxyethyl trimethyl ammonium chloride are used as functional additives to provide additional cross-linking sites, thereby improving the compactness and waterproofness of the coating in the subsequent coating formation; polyvinyl alcohol aqueous solution and acrylamide aqueous solution are used as dispersants and stabilizers to help form a stable pre-emulsion system; azobisisobutylimidazole hydrochloride is used as an initiator to initiate the polymerization reaction; methacryloyloxypropyl trimethoxysilane can be hydrolyzed to generate silanol groups, which can undergo cross-linking reaction with the polymer chains in the pre-emulsion system to form a denser three-dimensional network structure; and the participation of acidic silica sol provides silicate species, which can further react with polymer chains and silanol groups to subsequently enhance the cross-linking density and waterproof performance of the coating.
[0022] 2. In the preparation of the drying agent of the present invention, 10% cobalt isooctanoate, 12% rare earth isooctanoate, 5% calcium isooctanoate, 6% iron isooctanoate and 9% zinc isooctanoate are reasonably proportioned to ensure that the quick-drying waterproof coating can quickly dry on the surface and dry completely; experimental verification shows that there is neither an obvious positive correlation nor an obvious negative correlation between the drying speed of the coating film and the waterproof performance of the environmentally friendly waterproof agent of the present invention; and there is a positive correlation between the time difference between the surface drying time and the actual drying time of the coating film and the waterproof performance of the environmentally friendly waterproof agent of the present invention; the drying agent of the present invention is used in combination with the environmentally friendly waterproof agent of the present invention to ensure that the prepared quick-drying waterproof coating can quickly dry on the surface and dry completely while having excellent waterproof performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 , comparative trend diagram of surface drying time, actual drying time and time difference between the two obtained by brushing the quick-drying waterproof coating on the board of Examples 1-7 of the present invention and Comparative Examples 1-4;
[0024] Figure 2 , a comparative trend chart of the water contact angle test data of the quick-drying waterproof coatings prepared in Examples 1-7 of the present invention and Comparative Examples 1-4 after the coatings are completely dried. DETAILED DESCRIPTION
[0025] The present application is further described in detail below with reference to the embodiments.
[0026] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0027] Example 1: A method for preparing a quick-drying waterproof coating: 50 parts of alkyd resin are put into a disperser by weight, and the stirring speed is controlled at 900 rpm / min, and then 12 parts of titanium dioxide, 10 parts of talcum powder, 0.9 parts of drying agent, 0.7 parts of dispersant, 0.15 parts of anti-skinning agent, 0.25 parts of environmentally friendly waterproof agent and 6 parts of solvent are added, and the stirring speed is maintained at 900 rpm / min, and stirred for 13 minutes to obtain a mixture. Then the mixture is put into a grinder and ground to a fineness of no more than 25 μm to obtain a quick-drying waterproof coating.
[0028] Among them, the alkyd resin is industrial grade 389-9A alkyd resin, purchased from Huazhang New Materials (Shandong) Co., Ltd. The titanium dioxide is rutile titanium dioxide R-930, purchased from Hebei Weicai Pigment Co., Ltd. The talc powder is GT-202 superfine talc powder with a fineness of 1250 mesh and an oil absorption test data of 30-35g / 100g. The dispersant is BYK-161. The anti-skinning agent KL-841 was purchased from Zhejiang Shengan Chemical Co., Ltd. The solvent is 200# solvent oil.
[0029] The drying agent includes the following raw material components by weight: 3 parts of 10% cobalt isooctanoate, 3 parts of 12% rare earth isooctanoate, 11 parts of 5% calcium isooctanoate, 13 parts of 6% iron isooctanoate and 14 parts of 9% zinc isooctanoate. 10% cobalt isooctanoate, 12% rare earth isooctanoate, 5% calcium isooctanoate, 6% iron isooctanoate and 9% zinc isooctanoate were purchased from Zhengzhou Zhongyue Coating Additive Co., Ltd., and the solvent was 200# solvent oil, as shown in Table 1.
[0030] Table 1. Content standards of each component of the drier
[0031] name Appearance Metal content (%) Solution stability Cobalt 2-ethylhexanoate Purple liquid 10±0.2 Transparent without precipitates Calcium 2-ethylhexanoate Light yellow liquid 5±0.2 Transparent without precipitates Zinc 2-ethylhexanoate Yellow liquid 9±0.2 Transparent without precipitates Rare Earth 2-Ethylhexanoate Light yellow liquid 12±0.2 Transparent without precipitates Iron 2-octanoate Dark brown liquid 6±0.3 Transparent without precipitates
[0032] The preparation method of the environmentally friendly waterproofing agent is as follows:
[0033] S1. Put 45g of butyl acrylate, 24g of isooctyl acrylate, 20g of styrene, 1g of vinyl triethoxysilane, 5g of methacryloyloxyethyl trimethyl ammonium chloride, 60g of 4% polyvinyl alcohol aqueous solution and 10g of 8% acrylamide aqueous solution into a homogenizer. At room temperature, homogenize at 5000r / min for 50min, and then ultrasonically disperse at 50Hz for 30min to obtain a pre-emulsion.
[0034] S2. Mix 3 mL of methacryloyloxypropyltrimethoxysilane, 15 mL of deionized water and 8 mL of ethanol, adjust the pH to 3 at 40°C using 1 M hydrochloric acid solution as a regulator, stir and hydrolyze for 1 hour, add 30 mL of commercially available acidic silica sol, and react to obtain modified silica sol.
[0035] When adjusting the pH, first use a pH meter to measure the initial pH of the solution to determine how much adjuster needs to be added. Slowly add the hydrochloric acid solution while stirring continuously to ensure uniform mixing. Be careful not to add too much at one time to avoid exceeding the target pH. During the process of adding the hydrochloric acid solution, continue to monitor the pH changes of the solution, slow down the dripping speed when approaching the target value, and carefully control the dosage. Once the pH value of the solution reaches 3, stop adding the hydrochloric acid solution and continue stirring for a while to ensure that the pH value is stable. If the pH value is accidentally too low, you can choose to use NaOH solution to adjust it back to the desired pH value.
[0036] The commercially available acidic silica sol is chemical nano-grade acidic silica sol with a content of 30%, purchased from Guangzhou Changhao Chemical Co., Ltd.
[0037] S3. Pour the pre-emulsion obtained in S1 and the modified silica sol obtained in S2 into a three-necked flask, add 1 g of azobisisobutylimidazole hydrochloride and 276 g of deionized water, and react at 65°C for 6.5 h under nitrogen protection to obtain an environmentally friendly waterproofing agent.
[0038] Azobisisobutylimidazole hydrochloride is azo initiator V50, which was purchased from Zhongshan Yuanda New Materials Co., Ltd.
[0039] Embodiment 2: This embodiment differs from Embodiment 1 in that the raw material components of the quick-drying waterproof coating are used in different amounts.
[0040] Specifically, a method for preparing a quick-drying waterproof coating is as follows: 45 parts of alkyd resin are put into a disperser by weight, the stirring speed is controlled at 900 rpm / min, and then 10 parts of titanium dioxide, 8 parts of talcum powder, 0.8 parts of a drying agent, 0.5 parts of a dispersant, 0.1 parts of an anti-skinning agent, 0.2 parts of an environmentally friendly waterproof agent and 4 parts of a solvent are added, and the stirring speed is maintained at 900 rpm / min, and stirred for 13 minutes to obtain a mixture. The mixture is then put into a grinder and ground to a fineness of no more than 25 μm to obtain a quick-drying waterproof coating.
[0041] Embodiment 3: This embodiment differs from Embodiment 1 in that the raw material components of the quick-drying waterproof coating are used in different amounts.
[0042] Specifically, a method for preparing a quick-drying waterproof coating is as follows: 55 parts of alkyd resin are put into a disperser by weight, the stirring speed is controlled at 900 rpm / min, and then 15 parts of titanium dioxide, 12 parts of talcum powder, 1 part of a drying agent, 0.8 parts of a dispersant, 0.2 parts of an anti-skinning agent, 0.3 parts of an environmentally friendly waterproof agent and 7 parts of a solvent are added, and the stirring speed is maintained at 900 rpm / min, and stirred for 13 minutes to obtain a mixture. The mixture is then put into a grinder and ground to a fineness of no more than 25 μm to obtain a quick-drying waterproof coating.
[0043] Embodiment 4: This embodiment differs from Embodiment 1 in that the raw material components of the quick-drying waterproof coating are used in different amounts.
[0044] Specifically, a method for preparing a quick-drying waterproof coating is as follows: 55 parts of alkyd resin are put into a disperser by weight, the stirring speed is controlled at 900 rpm / min, and then 15 parts of titanium dioxide, 12 parts of talcum powder, 0.8 parts of a drying agent, 0.5 parts of a dispersant, 0.1 parts of an anti-skinning agent, 0.2 parts of an environmentally friendly waterproof agent and 4 parts of a solvent are added, and the stirring speed is maintained at 900 rpm / min, and stirred for 13 minutes to obtain a mixture. Then the mixture is put into a grinder and ground to a fineness of no more than 25 μm to obtain a quick-drying waterproof coating.
[0045] Embodiment 5: This embodiment differs from Embodiment 1 in that the dosage of the raw material components of the drying agent is different.
[0046] Specifically, the drying agent includes the following raw material components by weight: 3 parts of 10% cobalt isooctanoate, 3 parts of 12% rare earth isooctanoate, 10 parts of 5% calcium isooctanoate, 14 parts of 6% iron isooctanoate and 13 parts of 9% zinc isooctanoate.
[0047] Embodiment 6: This embodiment differs from Embodiment 1 in that the dosage of the raw material components of the drying agent is different.
[0048] Specifically, the drying agent includes the following raw material components by weight: 2 parts of 10% cobalt isooctanoate, 2 parts of 12% rare earth isooctanoate, 10 parts of 5% calcium isooctanoate, 12 parts of 6% iron isooctanoate and 13 parts of 9% zinc isooctanoate.
[0049] Embodiment 7: This embodiment differs from Embodiment 1 in that the dosage of the raw material components of the drying agent is different.
[0050] Specifically, the drying agent includes the following raw material components by weight: 4 parts of 10% cobalt isooctanoate, 4 parts of 12% rare earth isooctanoate, 12 parts of 5% calcium isooctanoate, 14 parts of 6% iron isooctanoate and 15 parts of 9% zinc isooctanoate.
[0051] Comparative Example 1: The difference between this comparative example and Example 1 is that in the preparation of the environmentally friendly waterproofing agent, the modified silica sol is replaced by commercially available acidic silica sol.
[0052] Specifically, the preparation method of the environmentally friendly waterproofing agent is as follows:
[0053] S1. Put 45g of butyl acrylate, 24g of isooctyl acrylate, 20g of styrene, 1g of vinyl triethoxysilane, 5g of methacryloyloxyethyl trimethyl ammonium chloride, 60g of 4% polyvinyl alcohol aqueous solution and 10g of 8% acrylamide aqueous solution into a homogenizer. At room temperature, homogenize at 5000r / min for 50min, and then ultrasonically disperse at 50Hz for 30min to obtain a pre-emulsion.
[0054] S2. Pour the pre-emulsion obtained in S1 and 30 mL of commercially available acidic silica sol into a three-necked flask, add 1 g of azobisisobutylimidazole hydrochloride and 276 g of deionized water, and react at 65°C for 6.5 h under nitrogen protection to obtain an environmentally friendly waterproofing agent.
[0055] Comparative Example 2: The difference between this comparative example and Example 1 is that in the preparation of the environmentally friendly waterproofing agent, the modified silica sol is deleted.
[0056] Specifically, the preparation method of the environmentally friendly waterproofing agent is as follows:
[0057] S1. Put 45g of butyl acrylate, 24g of isooctyl acrylate, 20g of styrene, 1g of vinyl triethoxysilane, 5g of methacryloyloxyethyl trimethyl ammonium chloride, 60g of 4% polyvinyl alcohol aqueous solution and 10g of 8% acrylamide aqueous solution into a homogenizer. At room temperature, homogenize at 5000r / min for 50min, and then ultrasonically disperse at 50Hz for 30min to obtain a pre-emulsion.
[0058] S2. Pour the pre-emulsion obtained in S1 and 30 mL of deionized water into a three-necked flask, add 1 g of azobisisobutylimidazole hydrochloride and 276 g of deionized water, and react at 65°C for 6.5 h under nitrogen protection to obtain an environmentally friendly waterproofing agent.
[0059] Comparative Example 3: The difference between this comparative example and Example 1 is that in the preparation of the drying agent, 5% calcium isooctanoate is replaced by 5% rare earth isooctanoate; 5% rare earth isooctanoate is obtained by diluting 12% rare earth isooctanoate with 200# solvent oil.
[0060] Specifically, the drying agent includes the following raw material components by weight: 3 parts of 10% cobalt isooctanoate, 3 parts of 12% rare earth isooctanoate, 11 parts of 5% rare earth isooctanoate, 13 parts of 6% iron isooctanoate and 14 parts of 9% zinc isooctanoate.
[0061] Comparative Example 4: The difference between this comparative example and Example 1 is that 10% of cobalt isooctanoate is deleted in the preparation of the drying agent.
[0062] Specifically, the drying agent includes the following raw material components by weight: 3 parts of 12% rare earth isooctanoate, 11 parts of 5% calcium isooctanoate, 13 parts of 6% iron isooctanoate and 14 parts of 9% zinc isooctanoate.
[0063] Test Example 1: Test items: surface dry and through dry.
[0064] Test object: Examples 1-7 and Comparative Examples 1-4 prepared quick-drying waterproof coatings.
[0065] Test method: brushing board, surface drying is tested by blowing cotton ball method, which means gently placing a cotton ball on the surface of the coating and blowing the cotton ball with your mouth. If it can be blown away and no cotton is left on the surface of the paint film, it is considered surface drying; real drying is tested by pressing filter paper method, which means placing a piece of filter paper on the surface of the coating, and then pressing a drying tester (200g weight), removing the weight after 30s, and then turning the test board over. If the filter paper can fall freely, it is considered real drying; time difference = real drying time - surface drying time. Drying environment after brushing board: carried out in a constant temperature and humidity chamber, with a constant temperature of 45℃ and a constant humidity of 55%.
[0066] Test results: See Table 2.
[0067] Test example 2: Test item: water resistance-water contact angle.
[0068] Test object: The quick-drying waterproof coatings prepared in Examples 1-7 and Comparative Examples 1-4 were brushed on the board to test the coating after it was completely dried in Test Example 1.
[0069] Test basis: DB44 / T 1232-2013.
[0070] Test results: See Table 2.
[0071] Table 2. Test results of test examples 1 and 2
[0072]
[0073]
[0074] Test conclusion: Analyze Examples 1-7 and combine the data in Table 2 and Figure 1-2 It can be seen that the quick-drying waterproof coating prepared by the present invention takes as little as 4.47 hours to dry on the surface of the board in a constant temperature of 45°C and a constant humidity of 55%, and as little as 6.23 hours to dry completely; the water contact angle of the coating film after complete drying is measured to be as high as 159°, and the waterproof performance is excellent.
[0075] Analyze Example 1 and Comparative Examples 1-2 and combine the data in Table 2 and Figure 1-2It can be seen that the surface drying and actual drying time of the coatings of Comparative Examples 1 and 2 are basically consistent with those of Example 1, indicating that changes in the environmentally friendly waterproofing agent will not directly affect the drying speed of the coating; the water contact angle of the coating of Comparative Example 1 after actual drying is 144°, which is significantly lower than that of Example 1, and the water contact angle of the coating of Comparative Example 2 after actual drying is 131°, which is further reduced, indicating that in the preparation of the environmentally friendly waterproofing agent, the addition of acidic silica sol can improve the waterproof performance of the environmentally friendly waterproofing agent, and the modification of the acidic silica sol can further improve the waterproof performance of the environmentally friendly waterproofing agent.
[0076] Analyze Example 1 and Comparative Example 3 and combine the data in Table 2 and Figure 1-2 It can be seen that the surface drying time of the coating in Comparative Example 3 is basically consistent with that in Example 1, while the actual drying time is significantly lower than that in Example 1, and the time difference between the surface drying time and the actual drying time is significantly lower than that in Example 1, indicating that in the preparation of the drying agent, 5% calcium isooctanoate is replaced by 5% rare earth isooctanoate, which has almost no effect on the surface drying speed, but can accelerate the actual drying speed, thereby shortening the time difference between the surface drying time and the actual drying time; when the environmentally friendly waterproofing agent used remains unchanged, the water contact angle of the coating in Comparative Example 3 after actual drying is 136°, which is significantly lower than that in Example 1.
[0077] Analyze Example 1 and Comparative Example 4 and combine the data in Table 2 and Figure 1-2 It can be seen that compared with Example 1, the surface drying time and actual drying time of the coating of Comparative Example 4 are significantly higher than those of Example 1, and the time difference between the surface drying time and the actual drying time is significantly lower than that of Example 1, indicating that in the preparation of the drying agent, deleting 10% of cobalt isooctanoate will slow down both the surface drying speed and the actual drying speed, but the degree of slowing down the surface drying speed is greater, which shortens the time difference between the surface drying time and the actual drying time; when the environmentally friendly waterproofing agent used remains unchanged, the water contact angle of the coating of Comparative Example 4 after actual drying is 130°, which is significantly lower than that of Example 2.
[0078] In summary, whether the coating drying speed is accelerated (Comparative Example 3) or slowed down (Comparative Example 4), the water contact angle measured data of the actual dry coating film are all reduced when the same environmentally friendly waterproofing agent of the present invention is used, indicating that the coating drying speed is neither significantly positively correlated nor significantly negatively correlated with the waterproof performance of the environmentally friendly waterproofing agent of the present invention. However, compared with Example 1, the time difference between the surface drying time and the actual drying time of the coating films of Comparative Examples 3 and 4 is shortened. As a result, when the same environmentally friendly waterproofing agent of the present invention is used, the water contact angle measured data of the actual dry coating films of Comparative Examples 3 and 4 are all reduced, indicating that there is a positive correlation between the time difference between the surface drying time and the actual drying time of the coating film and the waterproof performance of the environmentally friendly waterproofing agent of the present invention.
[0079] The drying agent of the present invention is used in combination with the environmentally friendly waterproofing agent to ensure that the prepared quick-drying waterproof coating can quickly dry on the surface and dry thoroughly while having excellent waterproof performance.
[0080] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0081] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing an environmentally friendly waterproofing agent, It is characterized in that The steps include: S1, put 45g of butyl acrylate, 24g of isooctyl acrylate, 20g of styrene, 1g of vinyl triethoxysilane, 5g of methacryloyloxyethyl trimethyl ammonium chloride, 60g of 4% polyvinyl alcohol aqueous solution and 10g of 8% acrylamide aqueous solution into a homogenizer for homogenization and ultrasonication to obtain a pre-emulsion; S2, take 3 mL of methacryloyloxypropyltrimethoxysilane, 15 mL of deionized water and 8 mL of ethanol, mix them, stir and hydrolyze them at 40°C and pH=3 for 1 h, add 30 mL of acidic silica sol, and react to obtain modified silica sol; S3, pour the pre-emulsion obtained in S1 and the modified silica sol obtained in S2 into a three-necked flask, add 1g of azobisisobutylimidazole hydrochloride and 276g of deionized water, and react at 65°C for 6.5h under nitrogen protection to obtain an environmentally friendly waterproofing agent; The environmentally friendly waterproofing agent is used to prepare a quick-drying waterproof coating; The quick-drying waterproof coating comprises the following raw material components by weight: 45-55 parts of alkyd resin, 10-15 parts of titanium dioxide, 8-12 parts of talcum powder, 0.8-1 parts of drying agent, 0.5-0.8 parts of dispersant, 0.1-0.2 parts of anti-skinning agent, 0.2-0.3 parts of environmentally friendly waterproof agent and 4-7 parts of solvent; The drying agent comprises the following raw material components by weight: 2-4 parts of 10% cobalt isooctanoate, 2-4 parts of 12% rare earth isooctanoate, 10-12 parts of 5% calcium isooctanoate, 12-14 parts of 6% iron isooctanoate and 13-15 parts of 9% zinc isooctanoate.
2. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that In S1, at room temperature, the homogenizer was used for homogenization at 5000 r / min for 45-60 min; and 50 Hz ultrasonic dispersion was performed for 30 min.
3. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that In S2, 1 M hydrochloric acid solution was used to adjust pH=3.
4. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that The titanium dioxide includes rutile titanium dioxide and / or anatase titanium dioxide.
5. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that The particle size of the talcum powder is 1000-1500 meshes, and the oil absorption is 30-35g / 100g.
6. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that The solvent includes xylene and / or 200# solvent oil.
7. The method for preparing the environmentally friendly waterproofing agent according to claim 1, It is characterized in that The preparation method of the quick-drying waterproof coating is as follows: adding alkyd resin into a disperser, controlling the stirring speed at 800-1000r / min, then adding titanium dioxide, talcum powder, a drying agent, a dispersant, an anti-skinning agent, a waterproofing agent and a solvent, continuing to maintain the stirring speed of 800-1000r / min, stirring for 10-15min to obtain a mixture; putting the mixture into a grinder, grinding it to a fineness of no more than 25μm, and obtaining a quick-drying waterproof coating.