Preparation method of light-cured 3D printed alumina ceramics without degreasing treatment
By using silane coupling agents or silicone precursors containing photocurable groups in the photocuring 3D printing process of alumina ceramics, the problem of long degreasing and sintering cycles in the traditional process is solved, and efficient and low-cost oxidation is achieved. Aluminum ceramic preparation improves the mechanical properties and precision of ceramics.
Patent Information
- Application Number
- CN202410815191.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Traditional alumina ceramic manufacturing processes are difficult to meet the complex shape and high-precision needs of modern manufacturing. Moreover, the degreasing and sintering cycles in the light-curing 3D printing process are long, resulting in shrinkage, deformation and large pores in the body, affecting the mechanical properties of the ceramics.
Using a silane coupling agent or a silicone precursor containing a photocurable group as a photocurable cross-linking agent eliminates the need for degreasing, simplifies the preparation process, improves the physical properties of the ceramic, including strength and stability, and maintains low viscosity and high solids. content.
The preparation process has been successfully simplified, the production cycle has been shortened, the cost has been reduced, the dimensional accuracy and density of alumina ceramics have been improved, the shrinkage rate has been reduced, and efficient, low-cost preparation has been achieved.
Smart Images

Figure CN118373670B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of oxide additive manufacturing, and in particular relates to a method for preparing light-cured 3D printed alumina ceramics without degreasing treatment. Background Art
[0002] Alumina (Al2O3) ceramics are the most widely used ceramics due to their excellent comprehensive properties and relatively cheap prices. They play an irreplaceable role in important fields such as high-precision machinery (photolithography machines), metal processing (tools, casting cores), chemical equipment (corrosion-resistant pumps and valves), electronics (substrates, semiconductors, etc.), biomedicine (artificial bones, stents, etc.), and aerospace (rocket nozzles, bearings, etc.). With the progress of the times, the development of complex precision structures and high-performance Al2O3 ceramics has become crucial. However, the traditional oxide ceramic manufacturing process is no longer suitable for the requirements of modern manufacturing for Al2O3 ceramics with increasingly complex shapes, higher precision, and digital and intelligent production. For this reason, ceramic additive manufacturing technology has become a hot topic for research and development in academia and industry in recent years. Digital light processing (DLP) photocuring 3D printing technology has become the most commercialized technology in ceramic additive manufacturing due to its advantages of high molding efficiency and good surface smoothness. At present, most DLP photocuring 3D printing uses solvent-containing slurry as raw material and acrylate monomer as photocuring molding cross-linking agent, among which dispersant and acrylate monomer account for more than 40 vol%. They need to be completely discharged before the green body is sintered, resulting in long drying and degreasing cycles, green body shrinkage, deformation and large pores, which seriously affect the shape, size, precision and mechanical properties of Al2O3 ceramic parts.
[0003] Chinese patent CN115180965B discloses a method for preparing polycarbosilane-enhanced alumina ceramic slurry and a 3D printing light-curing molding process. By adjusting the mass percentage of liquid polycarbosilane in the entire suspension, the silicon carbide content of the Al2O3 composite material and the mullite content generated by chemical reaction are optimized, thereby achieving the purpose of enhancing the mechanical properties of the ceramic. However, its preparation process still requires a long degreasing time, and the polycarbosilane content in the photosensitive resin is relatively low. The large amount of organic matter removed causes a large shrinkage of the alumina ceramic.
[0004] Chinese patent CN115991595B discloses a photocurable 3D printed alumina-based ceramic material and a preparation method thereof, comprising the following steps: ball milling and mixing alumina powder, sintering aid, surface modifier and organic solvent to obtain surface-modified ceramic powder; mixing the surface-modified ceramic powder and photosensitive resin premix to obtain ceramic slurry; photocuring 3D printing the ceramic slurry to obtain a ceramic blank; degreasing and sintering the ceramic blank in sequence to obtain a photocurable 3D printed alumina-based ceramic material. This method can adjust the contradiction between the high porosity and high-temperature creep resistance of photocurable 3D printed alumina-based ceramic materials, avoid the generation of delamination defects in the degreasing and sintering processes, and obtain alumina-based ceramic materials with excellent high-temperature performance. However, the photosensitive resin used is still ordinary acrylate monomers (organic matter), and a long degreasing process is still required in post-processing.
[0005] In order to reduce the shrinkage and degreasing cycle of light-curing 3D printed Al2O3 ceramics and improve the mechanical properties of complex-shaped Al2O3 ceramics, the following two aspects can be improved: (1) the formulation of photosensitive resin; (2) the solid content of alumina ceramic slurry. However, the solid content and viscosity of ceramic slurry are contradictory. When the solid content in the slurry reaches a certain value, the viscosity of the slurry increases sharply, resulting in the slurry no longer being suitable for light-curing 3D printing. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing light-cured 3D printed alumina ceramics that is exempt from degreasing treatment. By adopting a silane coupling agent or an organosilicon precursor containing a photocuring group as a photocuring cross-linking agent, not only the degreasing process is successfully eliminated and the preparation process is simplified, but also the physical properties of the ceramics, including strength and stability, are improved. At the same time, the low viscosity of the slurry is maintained and its solid content is increased, thereby achieving efficient and low-cost preparation of alumina ceramics.
[0007] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to the present invention comprises the following steps:
[0008] 1) Mixing a reactive diluent monomer with one or more of a silane coupling agent or an organosilicon precursor containing a photocurable group to obtain a photosensitive resin, and then adding a photoinitiator, mixing and stirring to obtain a mixed component; the amount of the reactive diluent monomer added is 10-24wt.% of the total amount of the photosensitive resin; the mass ratio of the reactive diluent monomer to the photoinitiator is (3.5-7.5):1;
[0009] 2) Add a dispersant to the mixed components, stir, then add alumina ceramic powder and continue stirring to obtain alumina ceramic slurry; the amount of the alumina ceramic powder added is 70-79wt.% of the total amount of the photosensitive resin and the alumina ceramic powder; the amount of the dispersant added is 3-8wt.% of the total amount of the alumina ceramic powder;
[0010] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0011] 4) Dry the green body in a blast drying oven;
[0012] 5) Place the dried green body in a box-type resistance furnace, heat it from room temperature to 200-300°C at a heating rate of 1-3°C / min, keep it warm for 1-2h, then heat it to 400-600°C at a heating rate of 1-4°C / min and keep it warm for 2-4h, then heat it to 1590-1610°C at a heating rate of 5-8°C / min, keep it warm for 1-2h, and cool it to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0013] In the step 1), the active diluent monomer is one or more of 1,6-hexanediol diacrylate, 1,4-hexanediol diacrylate, tripropylene glycol diacrylate, hydroxyethyl acrylate, trimethylolpropane triacrylate, dipentaerythritol hexaacrylate or pentaerythritol acrylate.
[0014] In the step 1), the photoinitiator is one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide or 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone.
[0015] In the step 1), the silane coupling agent is γ-methacryloxypropyltrimethoxysilane (KH570) or γ-glycidyloxypropyltrimethoxysilane (KH560).
[0016] In the step 1), the organosilicon precursor containing a photocurable group is one of polycarbosilane, polynitrogen silane or polysiloxane.
[0017] In the step 2), the dispersant is one of BYK190, BYK110, KOS110 or BYK111.
[0018] In the step 2), the particle size of the alumina ceramic powder is 0.2-1 μm.
[0019] In the step 1), the mixing and stirring speed is 400-500 r / min and the time is 2-4 h.
[0020] In the step 2), after adding the dispersant, the stirring speed is 400-500 r / min for 1-2 h; after adding the alumina ceramic powder, the stirring speed is continued to be 400-500 r / min for 2-4 h.
[0021] In the step 4), the drying temperature is 50-70°C and the drying time is 4-6 hours.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The method for preparing degreasing-free photocurable 3D printed alumina ceramics of the present invention introduces a silane coupling agent or an organosilicon precursor containing a photocurable group as a photocurable crosslinking agent, which is converted into ceramics during the post-processing process and retained in the sample, thereby successfully eliminating the degreasing and debonding process after the traditional photosensitive resin molding. This not only simplifies the preparation process, but also significantly shortens the production cycle and reduces the production cost;
[0024] (2) The method for preparing light-cured 3D printed alumina ceramics that is free of degreasing treatment described in the present invention uses a silane coupling agent or an organic silicon precursor containing a light-curing group to generate silicon dioxide during the sintering process, which reacts with alumina to form part of mullite, thereby enhancing the strength and stability of the ceramic material. At the same time, these generated substances remain in the system and effectively reduce the shrinkage rate during the sintering process, so that the prepared alumina ceramics have higher dimensional accuracy and lower shrinkage rate, and the shrinkage is more uniform;
[0025] (3) The method for preparing light-cured 3D printed alumina ceramics that is exempt from degreasing treatment described in the present invention increases the solid content of the slurry while maintaining a low viscosity of the slurry by introducing an organic silicon precursor or a silane coupling agent containing a photocuring group. This is not only conducive to the smooth progress of the 3D printing process, but also can improve the density and strength of the final product. The alumina ceramics obtained have excellent properties such as high strength, suitable porosity, high precision, and low and uniform shrinkage. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope image of the alumina ceramic powder used in Example 1;
[0027] Figure 2 This is a scanning electron microscope image of the light-cured 3D printed alumina ceramic exempted from degreasing treatment obtained in Example 1;
[0028] Figure 3 This is an EDS test diagram of the light-cured 3D printed alumina ceramic exempted from degreasing treatment obtained in Example 1, and an O element distribution diagram;
[0029] Figure 4 This is an EDS test image of Al element distribution of the light-cured 3D printed alumina ceramic exempted from degreasing treatment obtained in Example 1;
[0030] Figure 5 This is an EDS test diagram of Si element distribution of the light-cured 3D printed alumina ceramic exempted from degreasing treatment obtained in Example 1;
[0031] Figure 6 XRD test graphs of the degreasing-free light-cured 3D-printed alumina ceramic prepared in Example 1 and the alumina ceramic powder used in Example 1. DETAILED DESCRIPTION
[0032] The present invention will be further described below with reference to the embodiments.
[0033] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0034] Example 1
[0035] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0036] 1) 1 g of 1,6-hexanediol diacrylate, 0.5 g of trimethylolpropane triacrylate and 5 g of γ-methacryloxypropyltrimethoxysilane were mixed to obtain a photosensitive resin, and then 0.2 g of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide was added, and magnetic stirring was performed at a speed of 400 r / min for 4 hours to obtain a mixed component;
[0037] 2) Add 0.73 g of KOS110 to the mixed components, stir magnetically at a speed of 400 r / min for 2 h, then add 23.5 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 3 h at a speed of 400 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 1254 mPa·s and a solid content of 87.9%;
[0038] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0039] 4) Dry the green body in a blast drying oven at a temperature of 50°C for 6 hours;
[0040] 5) Place the dried green body in a box-type resistance furnace, heat it from room temperature to 300°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 500°C at a heating rate of 2°C / min and keep it warm for 2 hours, then heat it to 1600°C at a heating rate of 5°C / min, keep it warm for 2 hours, and cool it to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment. The sintering time is 650 minutes (excluding the time for cooling with the furnace).
[0041] The surface morphology of alumina ceramic powder was observed by scanning electron microscopy. Figure 1 As shown by Figure 1 It can be seen that the alumina ceramic particles are uniform in size.
[0042] The surface morphology of degreasing-free light-cured 3D printed alumina ceramics was observed by scanning electron microscopy. Figure 2 As shown by Figure 2 It can be seen that the grain size of alumina ceramics is uniform and there are no pores.
[0043] The chemical element composition of light-cured 3D printed alumina ceramics without degreasing treatment was obtained by EDS. The results are as follows Figure 3-5 As shown in the figure, the distribution of Si, Al, and O elements can be seen. In particular, the presence of Si proves that after the silane coupling agent is introduced into the photosensitive resin formula, it remains in the matrix during the sintering process, thereby eliminating the degreasing process and reducing the shrinkage of the ceramic sample.
[0044] The diffraction characteristic peaks of alumina ceramic powder and light-cured 3D printed alumina ceramics without degreasing treatment were tested by XRD. The results are as follows Figure 6 As shown, the 3Al2O3·2SiO2 curve is the diffraction characteristic peak of the light-cured 3D printed alumina ceramic exempted from degreasing treatment, and the Al2O3 curve is the diffraction characteristic peak of the alumina ceramic powder. It can be seen from the figure that a new phase of mullite is generated in the light-cured 3D printed alumina ceramic exempted from degreasing treatment prepared in Example 1.
[0045] Example 2
[0046] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0047] 1) 0.5 g of 1,4-hexanediol diacrylate, 0.5 g of dipentaerythritol hexaacrylate and 5.5 g of γ-glycidyloxypropyltrimethoxysilane were mixed to obtain a photosensitive resin, and then 0.2 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate was added, and magnetic stirring was performed at a speed of 500 r / min for 2 h to obtain a mixed component;
[0048] 2) Add 0.73 g of BYK190 to the mixed components, stir magnetically at a speed of 500 r / min for 1 h, then add 15.2 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 2 h at a speed of 500 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 943 mPa·s and a solid content of 82%;
[0049] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0050] 4) Dry the green body in a blast drying oven at 70°C for 4 hours;
[0051] 5) The dried green body is placed in a box-type resistance furnace and heated from room temperature to 300°C at a heating rate of 3°C / min, kept warm for 1 hour, then heated to 600°C at a heating rate of 1°C / min and kept warm for 3 hours, then heated to 1610°C at a heating rate of 8°C / min, kept warm for 1 hour, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0052] Example 3
[0053] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0054] 1) 0.5 g of tripropylene glycol diacrylate and 5.8 g of polynitrosilane were mixed to obtain a photosensitive resin, and then 0.2 g of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added, and magnetic stirring was performed at a speed of 400 r / min for 4 hours to obtain a mixed component;
[0055] 2) Add 1.24 g of BYK110 to the mixed components, stir magnetically at a speed of 400 r / min for 2 h, then add 16.3 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 4 h at a speed of 400 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 976 mPa·s and a solid content of 83%;
[0056] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0057] 4) Dry the green body in a blast drying oven at 60°C for 5 hours;
[0058] 5) The dried green body is placed in a box-type resistance furnace, heated from room temperature to 200°C at a heating rate of 1°C / min, kept warm for 2 hours, then heated to 400°C at a heating rate of 4°C / min and kept warm for 4 hours, then heated to 1590°C at a heating rate of 6°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0059] Example 4
[0060] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0061] 1) 1.5 g of hydroxyethyl acrylate and 5 g of polycarbosilane were mixed to obtain a photosensitive resin, and then 0.2 g of 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone was added, and magnetic stirring was performed at a speed of 400 r / min for 4 hours to obtain a mixed component;
[0062] 2) Add 0.73 g of BYK111 to the mixed components, stir magnetically at a speed of 400 r / min for 2 h, then add 23.5 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 3 h at a speed of 400 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 1205 mPa·s and a solid content of 87.9%;
[0063] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0064] 4) Dry the green body in a blast drying oven at a temperature of 50°C for 6 hours;
[0065] 5) The dried green body is placed in a box-type resistance furnace, heated from room temperature to 300°C at a heating rate of 2°C / min, kept warm for 1 hour, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, then heated to 1600°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0066] Example 5
[0067] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0068] 1) 1.5 g of pentaerythritol acrylate and 5 g of polysiloxane were mixed to obtain a photosensitive resin, and then 0.2 g of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide was added, and magnetic stirring was performed at a speed of 400 r / min for 4 hours to obtain a mixed component;
[0069] 2) Add 0.73 g of KOS110 to the mixed components, stir magnetically at a speed of 400 r / min for 2 h, then add 23.5 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 3 h at a speed of 400 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 1213 mPa·s and a solid content of 87.9%;
[0070] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0071] 4) Dry the green body in a blast drying oven at a temperature of 50°C for 6 hours;
[0072] 5) The dried green body is placed in a box-type resistance furnace, heated from room temperature to 300°C at a heating rate of 2°C / min, kept warm for 1 hour, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, then heated to 1600°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0073] Example 6
[0074] The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment comprises the following steps:
[0075] 1) 1 g of 1,6-hexanediol diacrylate, 0.5 g of trimethylolpropane triacrylate, 3 g of γ-methacryloxypropyltrimethoxysilane and 2 g of polycarbosilane were mixed to obtain a photosensitive resin, and then 0.2 g of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide was added, and magnetic stirring was performed at a speed of 400 r / min for 4 hours to obtain a mixed component;
[0076] 2) Add 0.73 g of KOS110 to the mixed components, stir magnetically at a speed of 400 r / min for 2 h, then add 23.5 g of alumina ceramic powder with a particle size of 0.6±0.4 μm and continue stirring for 3 h at a speed of 400 r / min, and then stir homogenously for 10 min to obtain a uniformly dispersed alumina ceramic slurry without bubbles, with a viscosity of 1238 mPa·s and a solid content of 87.9%;
[0077] 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device;
[0078] 4) Dry the green body in a blast drying oven at a temperature of 50°C for 6 hours;
[0079] 5) The dried green body is placed in a box-type resistance furnace, heated from room temperature to 300°C at a heating rate of 2°C / min, kept warm for 1 hour, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, then heated to 1600°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment.
[0080] Comparative Example 1
[0081] The difference from Example 1 is:
[0082] In step 1) of the method for preparing light-cured 3D printed alumina ceramics without degreasing treatment, no silane coupling agent is added, and the rest is the same as in Example 1.
[0083] Comparative Example 2
[0084] The difference from Example 1 is:
[0085] In step 5) of the method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment, the temperature is heated from room temperature to 300°C at a heating rate of 0.5°C / min, kept warm for 2 hours, then heated to 500°C at a heating rate of 0.5°C / min and kept warm for 2 hours, then heated to 1600°C at a heating rate of 2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain light-cured 3D printed alumina ceramics exempted from degreasing treatment. The rest is the same as in Example 1, and the sintering time is 1910 minutes (excluding the time for cooling with the furnace).
[0086] Comparative Example 3
[0087] The difference from Example 4 is:
[0088] In step 1) of the method for preparing light-cured 3D printed alumina ceramics without degreasing treatment, polycarbosilane is not added, and the rest is the same as in Example 4.
[0089] Comparative Example 4
[0090] The difference from Example 1 is:
[0091] In step 5) of the preparation method of the light-cured 3D printed alumina ceramic exempted from degreasing treatment, the dried green body is placed in a box-type resistance furnace, heated from room temperature to 300°C at a heating rate of 2°C / min, kept warm for 1 hour, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, then heated to 1550°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramic exempted from degreasing treatment. The rest is the same as Example 1.
[0092] Comparative Example 5
[0093] The difference from Example 1 is:
[0094] In step 5) of the preparation method of the light-cured 3D printed alumina ceramic exempted from degreasing treatment, the dried green body is placed in a box-type resistance furnace, heated from room temperature to 300°C at a heating rate of 2°C / min, kept warm for 1 hour, then heated to 500°C at a heating rate of 2°C / min and kept warm for 2 hours, then heated to 1650°C at a heating rate of 5°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramic exempted from degreasing treatment. The rest is the same as Example 1.
[0095] Comparative Example 6
[0096] The difference from Example 1 is:
[0097] In step 2) of the method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment, the amount of alumina ceramic powder added is 4.89 g, the amount of KOS110 added is 0.15 g, and the rest is the same as in Example 1.
[0098] The performance of the alumina ceramics obtained in Examples 1-6 and Comparative Examples 1-6 was tested, and the test method was as follows:
[0099] Bending strength (MPa), tested in accordance with GB / T 6569-2006;
[0100] The test methods for linear shrinkage and porosity are conventional test methods in the art.
[0101] The test results are shown in Table 1.
[0102] Table 1
[0103]
[0104] It can be seen from Table 1 that the introduction of silane coupling agent or organosilicon precursor containing photocurable group can effectively improve the mechanical properties of photocurable 3D printed alumina ceramics and reduce the linear shrinkage. Among them, the photosensitive resin in Examples 1-6 can generate silicon dioxide during the sintering process, and then react with alumina to form mullite, which enhances the strength of the alumina ceramics and reduces its linear shrinkage; while the photosensitive resin prepared in Comparative Examples 1 and 3 does not contain silane coupling agent or organosilicon precursor containing photocurable group, and the organic matter generated by the alumina ceramics during the sintering process is completely eliminated, and no substance remains in the matrix, resulting in a large linear shrinkage and porosity, thereby affecting the mechanical properties of the alumina ceramics. In Comparative Example 2, conventional degreasing and sintering steps are used to degrease the alumina ceramics. From the experimental results, it can be found that compared with Example 1, its sintering cycle is longer, the cost is higher, and the performance of the alumina ceramics is not greatly affected. This also shows that the preparation method of light-cured 3D printed alumina ceramics exempted from degreasing treatment described in the present invention can exempt the degreasing process, shorten the cycle, and not affect the performance of the alumina ceramics, thereby obtaining high-performance alumina ceramics with complex shapes. In Comparative Example 4, the sintering temperature is too low to achieve densification, resulting in low performance of the alumina ceramics. In Comparative Example 5, the sintering temperature is too high to cause the alumina ceramics to be over-burned, which also reduces the performance of the alumina ceramics. In Comparative Example 6, the reduction in the content of alumina ceramic powder has a greater impact on the mechanical properties of the alumina ceramics. At the same time, due to the low solid content, its linear shrinkage and porosity are higher.
Claims
1. A method for preparing light-cured 3D printed alumina ceramics without degreasing treatment, characterized in that: The following steps are involved: 1) Mixing a reactive diluent monomer with one or more of a silane coupling agent or an organosilicon precursor containing a photocurable group to obtain a photosensitive resin, and then adding a photoinitiator, mixing and stirring to obtain a mixed component; the amount of the reactive diluent monomer added is 10-24wt.% of the total amount of the photosensitive resin; the mass ratio of the reactive diluent monomer to the photoinitiator is (3.5-7.5):1; 2) Add a dispersant to the mixed components, stir, then add alumina ceramic powder and continue stirring to obtain alumina ceramic slurry; the amount of the alumina ceramic powder added is 70-79wt.% of the total amount of the photosensitive resin and the alumina ceramic powder; the amount of the dispersant added is 3-8wt.% of the total amount of the alumina ceramic powder; 3) Printing the obtained alumina ceramic slurry into a green body using a light-curing 3D printing device; 4) Dry the green body in a blast drying oven; 5) Place the dried green body in a box-type resistance furnace, heat it from room temperature to 200-300°C at a heating rate of 1-3°C / min, keep it warm for 1-2h, then heat it to 400-600°C at a heating rate of 1-4°C / min and keep it warm for 2-4h, then heat it to 1590-1610°C at a heating rate of 5-8°C / min, keep it warm for 1-2h, and cool it to room temperature with the furnace to obtain the light-cured 3D printed alumina ceramics exempted from degreasing treatment; In the step 1), the silane coupling agent is γ-methacryloxypropyltrimethoxysilane or γ-glycidyloxypropyltrimethoxysilane; In the step 1), the organosilicon precursor containing a photocurable group is one of polycarbosilane, polynitrogen silane or polysiloxane.
2. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 1), the active diluent monomer is one or more of 1,6-hexanediol diacrylate, 1,4-hexanediol diacrylate, tripropylene glycol diacrylate, hydroxyethyl acrylate, trimethylolpropane triacrylate, dipentaerythritol hexaacrylate or pentaerythritol acrylate.
3. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 1), the photoinitiator is one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide or 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone.
4. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 2), the dispersant is one of BYK190, BYK110, KOS110 or BYK111.
5. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 2), the particle size of the alumina ceramic powder is 0.2-1 μm.
6. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 1), the mixing and stirring speed is 400-500 r / min and the time is 2-4 h.
7. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 2), after adding the dispersant, the stirring speed is 400-500 r / min for 1-2 h; after adding the alumina ceramic powder, the stirring speed is continued to be 400-500 r / min for 2-4 h.
8. The method for preparing light-cured 3D printed alumina ceramics exempted from degreasing treatment according to claim 1, characterized in that: In the step 4), the drying temperature is 50-70°C and the drying time is 4-6 hours.