A high-performance glass fiber reinforced plastic composite material and preparation method thereof
By using phenolic resin, epoxy resin, alkyd resin and specific fiber combination in fiberglass materials, combined with nano-silica fillers, the problem of degradation of performance of fiberglass materials in harsh environments is solved, and high tensile strength and excellent Aging resistance.
Patent Information
- Application Number
- CN202410612077.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-16
AI Technical Summary
FRP materials are prone to internal pores and defects in environments such as high temperature and high humidity, strong ultraviolet rays, and high salinity seawater, resulting in reduced performance and shortened service life, affecting safety.
Phenolic resin, epoxy resin, and alkyd resin are used as resin matrix, combining scientifically proportioned glass fiber, basalt fiber, and silicon fiber, and feldspar powder and nano-silica as fillers, through crosslinking agents and curing agents and the role of accelerator, high-performance fiberglass composite materials are prepared to reduce internal microscopic defects and improve aging resistance.
The tensile strength and anti-aging properties of fiberglass composite materials are significantly improved. The tensile strength retention rate after aging can reach 99.4%, which is significantly better than the comparison group and shows excellent durability and aging resistance.
Smart Images

Figure BDA0004843948780000081 
Figure BDA0004843948780000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass fiber reinforced plastic composite materials, and in particular to a high-performance glass fiber reinforced plastic composite material and a preparation method thereof. Background Art
[0002] The scientific name of FRP is fiber reinforced plastic, which is fiber reinforced composite plastic. According to the different fibers used, it can be divided into glass fiber reinforced composite plastic, carbon fiber reinforced composite plastic, boron fiber reinforced composite plastic, etc. According to the different types of resins used, there are polyester FRP, epoxy FRP, and phenolic FRP. FRP materials are widely used in lifeboats, fan blades, corrosive liquid pipelines, high temperature and high pressure reaction vessels, instrument panels, propellers, hulls and other products because of their light weight, hardness, non-conductivity, stable performance, high mechanical strength, less recycling, and corrosion resistance, showing a huge market prospect.
[0003] Affected by the process, type of polymer material, and fiber type, FRP materials may form pores and defects of varying degrees inside. Under the influence of high temperature, high humidity, strong ultraviolet rays, high-salinity seawater and other factors, microscopic material defects will be aggravated, causing macroscopic aging and performance degradation, resulting in a decrease in the service life of the material and affecting the safety of material use. Therefore, it is very necessary to develop new high-performance FRP composite materials. Summary of the invention
[0004] The purpose of the present invention is to provide a high-performance glass fiber reinforced plastic composite material and a preparation method thereof. By using phenolic resin, epoxy resin and alkyd resin as a resin matrix, using glass fiber, basalt fiber and silicon fiber in a scientific ratio as reinforcing materials, and using feldspar powder and nano-silicon dioxide as fillers, and in the presence of auxiliary agents such as a cross-linking agent, a curing agent and a accelerator, a high-performance glass fiber reinforced plastic composite material is prepared. The glass fiber reinforced plastic composite material has lower internal microscopic defects, better aging resistance and better durability in the external environment.
[0005] To this end, the present invention adopts the following technical solutions:
[0006] On the one hand, the present invention provides a high-performance glass fiber reinforced plastic composite material, comprising the following components in parts by weight: 50-80 parts of phenolic resin, 15-30 parts of epoxy resin, 10-20 parts of alkyd resin, 10-20 parts of glass fiber, 20-40 parts of basalt fiber, 10-20 parts of silicon fiber, 3-10 parts of feldspar powder, 5-15 parts of nano silicon dioxide, 1-9 parts of cross-linking agent, 0.1-3 parts of antioxidant, 0.5-3 parts of curing agent and 0.5-3 parts of accelerator.
[0007] Preferably, the epoxy resin is a phenolic epoxy resin.
[0008] Preferably, the weight ratio of the glass fiber:basalt fiber:silicon fiber is 1-2:1.5-3:1-2.
[0009] Preferably, the particle size of the nano-silicon dioxide is 30-60 nm.
[0010] Preferably, the feldspar powder is potassium feldspar powder with a particle size of 50-100 nm.
[0011] Preferably, the silicon fiber includes at least one of silicon carbide fiber and silicon nitride fiber.
[0012] Preferably, the crosslinking agent includes one or more of a silicate crosslinking agent, an aminosilane crosslinking agent, a methoxysilane crosslinking agent, and a styrene silane crosslinking agent.
[0013] Preferably, the curing agent includes one or more of an organic amine curing agent, a modified amine curing agent, and an organic acid anhydride curing agent.
[0014] Preferably, the promoter includes one or more of isooctyl cobalt organic acid, cycloalkane cobalt organic acid, N,N-dimethylaniline, and N,N-diethylaniline.
[0015] Another aspect of the present invention provides a method for preparing a high-performance glass fiber reinforced plastic composite material, comprising the following steps:
[0016] S1, mixing phenolic resin, epoxy resin, alkyd resin, feldspar powder and nano-silicon dioxide to obtain a mixed resin;
[0017] S2, mixing glass fiber, basalt fiber, silicon fiber and 1 / 3 weight of a cross-linking agent, stirring to obtain mixed fiber;
[0018] S3, mixing the above mixed resin, mixed fiber, the remaining 2 / 3 of the cross-linking agent, antioxidant, curing agent and accelerator, stirring, pouring into a corresponding mold, cooling and molding, and obtaining a high-performance glass fiber reinforced plastic composite material.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The matrix resin of the present invention adopts phenolic resin, epoxy resin and alkyd resin, and the reinforcing fiber adopts glass fiber, basalt fiber and silicon fiber with scientific proportion, and feldspar powder and nano-silicon dioxide are preferably used as reinforcing fillers. The resin and the filler are first compounded, the reinforcing fiber is mixed with part of the cross-linking agent in advance, and then the resin and the reinforcing fiber are mixed to prepare a glass fiber reinforced plastic composite material with excellent tensile strength and anti-aging performance. DETAILED DESCRIPTION
[0021] The specific implementation methods of the technical solution of this specification are further described below through specific examples. These examples are for the purpose of describing the technical solution in detail, rather than for limiting the technical solution. Based on the examples in this specification, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this specification.
[0022] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art, and the reagents and materials used in the following examples are commercially available.
[0023] Phenolic resin PF1A2-1501, CAS No.: 9003-35-4, purchased from Jinan Huijinchuan Chemical Co., Ltd.;
[0024] Phenolic epoxy resin F44 was purchased from Guangzhou Zeyiyuan Chemical Co., Ltd.;
[0025] Alkyd resin VOK-N36X, purchased from Guangzhou Si Tu Yuan Chemical Co., Ltd.:
[0026] Glass fiber, fiber length 25-300 μm, provided by Shaoguan Haoli Recycling Resources Utilization Co., Ltd.
[0027] Basalt fiber, fiber diameter 7-25um, purchased from Hebei Sanliujiu New Material Technology Co., Ltd.;
[0028] Silicon nitride fibers were purchased from Suzhou Beike Nanotechnology Co., Ltd.
[0029] Example 1
[0030] The present embodiment provides a high-performance glass fiber reinforced plastic composite material, comprising the following components in parts by weight: 70 parts of phenolic resin, 25 parts of phenolic epoxy resin, 15 parts of alkyd resin, 20 parts of glass fiber, 35 parts of basalt fiber, 10 parts of silicon nitride fiber, 5 parts of feldspar powder, 15 parts of nano-silica, 7 parts of cross-linking agent, 0.3 parts of 2,6-di-tert-butyl-p-cresol, 1 part of stearylamide ethyl diethylamine, and 1 part of cobalt cyclohexaneate.
[0031] The particle size of the nano silicon dioxide is 60 nm.
[0032] The feldspar powder is potassium feldspar powder, and the average particle size is 50nm.
[0033] The crosslinking agent is vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 1:1.
[0034] The preparation method of the high-performance glass fiber reinforced plastic composite material of this embodiment comprises the following steps:
[0035] S1, adding phenolic resin, phenolic epoxy resin, alkyd resin, feldspar powder and nano-silica into a high-speed mixer and mixing at a speed of 400 rpm for 20 min to obtain a mixed resin;
[0036] S2, mixing glass fiber, basalt fiber, silicon fiber and 1 / 3 weight of a cross-linking agent, and stirring at a rotation speed of 350 rpm to obtain mixed fibers;
[0037] S3, the mixed resin, mixed fiber, the remaining 2 / 3 of the cross-linking agent, antioxidant, curing agent and accelerator are mixed, stirred at a speed of 300 rpm, poured into a mold and cooled to form, so as to obtain a high-performance fiberglass composite material.
[0038] Example 2
[0039] 80 parts of phenolic resin, 20 parts of phenolic epoxy resin, 10 parts of alkyd resin, 10 parts of glass fiber, 20 parts of basalt fiber, 10 parts of silicon nitride fiber, 10 parts of feldspar powder, 10 parts of nano-silica, 7 parts of cross-linking agent, 0.2 parts of 2,6-di-tert-butyl-p-cresol, 1 part of stearylamide ethyl diethylamine, and 1 part of cobalt cyclohexanecarboxylate.
[0040] The particle size of the nano silicon dioxide is 60 nm.
[0041] The feldspar powder is potassium feldspar powder, and the average particle size is 50nm.
[0042] The crosslinking agent is vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 1:1.
[0043] The preparation method of the high-performance glass fiber reinforced plastic composite material of this embodiment comprises the following steps:
[0044] S1, adding phenolic resin, phenolic epoxy resin, alkyd resin, feldspar powder and nano-silica into a high-speed mixer and mixing and stirring at a speed of 300 rpm for 20 min to obtain a mixed resin;
[0045] S2, mixing glass fiber, basalt fiber, silicon fiber and 1 / 3 weight of a cross-linking agent, and stirring at a rotation speed of 300 rpm to obtain mixed fibers;
[0046] S3, the mixed resin, mixed fiber, the remaining 2 / 3 of the cross-linking agent, antioxidant, curing agent and accelerator are mixed, stirred at a speed of 300 rpm, poured into a mold and cooled to form, so as to obtain a high-performance fiberglass composite material.
[0047] Example 3
[0048] 60 parts of phenolic resin, 30 parts of phenolic epoxy resin, 20 parts of alkyd resin, 15 parts of glass fiber, 30 parts of basalt fiber, 10 parts of silicon nitride fiber, 7 parts of feldspar powder, 10 parts of nano-silica, 6 parts of cross-linking agent, 0.3 parts of 2,6-di-tert-butyl-p-cresol, 1 part of stearylamide ethyl diethylamine, and 1 part of cobalt cyclohexanecarboxylate.
[0049] The particle size of the nano silicon dioxide is 60 nm.
[0050] The feldspar powder is potassium feldspar powder, and the average particle size is 50nm.
[0051] The crosslinking agent is vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 1:1.
[0052] The preparation method of the high-performance glass fiber reinforced plastic composite material of this embodiment comprises the following steps:
[0053] S1, adding phenolic resin, phenolic epoxy resin, alkyd resin, feldspar powder and nano-silica into a high-speed mixer and mixing at a speed of 400 rpm for 20 min to obtain a mixed resin;
[0054] S2, mixing glass fiber, basalt fiber, silicon fiber and 1 / 3 weight of a cross-linking agent, and stirring at a rotation speed of 300 rpm to obtain mixed fibers;
[0055] S3, the mixed resin, mixed fiber, the remaining 2 / 3 of the cross-linking agent, antioxidant, curing agent and accelerator are mixed, stirred at a speed of 300 rpm, poured into a mold and cooled to form, so as to obtain a high-performance fiberglass composite material.
[0056] Comparative Example 1
[0057] The difference between this comparative example and Example 1 is that no phenolic epoxy resin is added, and other components are the same.
[0058] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0059] Comparative Example 2
[0060] The difference between this comparative example and Example 1 is that no alkyd resin is added, and other components are the same.
[0061] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0062] Comparative Example 3
[0063] The difference between this comparative example and Example 1 is that no phenolic epoxy resin and alkyd resin are added, and other components are the same.
[0064] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0065] Comparative Example 4
[0066] The difference between this comparative example and Example 1 is that glass fiber is not added, and other components are the same.
[0067] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0068] Comparative Example 5
[0069] The difference between this comparative example and Example 1 is that basalt fiber is not added, and other components are the same.
[0070] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0071] Comparative Example 6
[0072] The difference between this comparative example and Example 1 is that silicon nitride fiber is not added, and other components are the same.
[0073] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0074] Comparative Example 7
[0075] The difference between this comparative example and Example 1 is that glass fiber and silicon nitride fiber are not added, and other components are the same.
[0076] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0077] Comparative Example 8
[0078] The difference between this comparative example and Example 1 is that basalt fiber and silicon nitride fiber are not added, the weight percentage of glass fiber is, and the other components are the same.
[0079] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0080] Comparative Example 9
[0081] The difference between this comparative example and Example 1 is that the nano silicon dioxide is replaced by calcium carbonate in equal parts by weight, and the other components are the same.
[0082] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0083] Comparative Example 10
[0084] The difference between this comparative example and Example 1 is that the feldspar powder is replaced by an equal weight portion of calcium carbonate, the nano silicon dioxide is replaced by an equal weight portion of 1 um silicon dioxide, and the other components are the same.
[0085] The preparation method of the glass fiber reinforced plastic composite material in this comparative example is the same as that in Example 1.
[0086] Comparative Example 11
[0087] The preparation method of the glass fiber reinforced plastic composite material of the comparative example is as follows: phenolic resin, epoxy resin, alkyd resin, feldspar powder, nano silicon dioxide, crosslinking agent, antioxidant, curing agent and accelerator are mixed and stirred, and extruded to obtain the glass fiber reinforced plastic composite material.
[0088] Performance Test:
[0089] 1. UV aging resistance test
[0090] Refer to "Artificial Weathering and Artificial Radiation Exposure of Paints and Varnishes to Filtered Xenon Arc Radiation" (GB / T1865-2009), the irradiance on the sample surface is 60W / m 2 , the air temperature in the test chamber is 38±3℃, and the aging time is 3000h.
[0091] 2. Tensile strength and retention rate test
[0092] The tensile strength of FRP samples before and after aging was tested according to the "Test Method for Tensile Properties of Fiber Reinforced Plastics" (GB / T 1447-2005). The tensile strength retention rate was the percentage of the tensile strength of the FRP sample after the aging test to the tensile strength before aging.
[0093] The test results are shown in Table 1.
[0094] Table 1 Test results of material tensile strength and tensile strength retention rate
[0095]
[0096]
[0097] It can be seen from Table 1 that the high-performance FRP composite material provided by the embodiment of the present invention has a tensile strength of up to 334 MPa, and a tensile strength retention rate of up to 99.4% after 3000 h of UV irradiation aging treatment, which is significantly higher than the FRP composite materials of Comparative Examples 1-11, and has excellent tensile strength and aging resistance.
[0098] The difference between Comparative Example 1 and Example 1 is that the matrix resin does not contain phenolic epoxy resin; the test results show that the tensile strength before aging is lower than that of Example 1, and the tensile strength retention rate is also reduced after 3000h of UV aging treatment, indicating that the addition of phenolic epoxy resin can enhance the strength and aging resistance of the FRP composite material.
[0099] The difference between Comparative Example 2 and Example 1 is that the base resin does not contain alkyd resin; the test results show that the tensile strength before aging is lower than that of Example 1, and the tensile strength retention rate is also reduced after 3000 hours of UV aging treatment, indicating that the addition of alkyd resin can enhance the strength and aging resistance of the FRP composite material.
[0100] Compared with Example 1, Comparative Example 3 differs in that the matrix resin does not contain phenolic epoxy resin and alkyd resin. The test results show that the tensile strength before aging is lower than that of Example 1. After 3000 hours of UV aging treatment, the tensile strength retention rate is also reduced, indicating that the simultaneous addition of phenolic epoxy resin and alkyd resin can further enhance the strength and aging resistance of the FRP composite material.
[0101] The difference between Comparative Example 4 and Example 1 is that no glass fiber is added; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that glass fiber can significantly improve the tensile strength and aging resistance of the matrix resin.
[0102] The difference between Comparative Example 5 and Example 1 is that no basalt fiber is added; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that basalt fiber can significantly improve the tensile strength and aging resistance of the matrix resin.
[0103] The difference between Comparative Example 6 and Example 1 is that silicon nitride fiber is not added; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that silicon nitride fiber can improve the tensile strength and aging resistance of the matrix resin.
[0104] The difference between Comparative Example 7 and Example 1 is that glass fiber and silicon nitride are not added; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that glass fiber and silicon nitride fiber can synergistically improve the tensile strength and aging resistance of the matrix resin.
[0105] The difference between Comparative Example 8 and Example 1 is that basalt fiber and silicon nitride fiber are not added; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that basalt fiber and silicon nitride fiber can significantly improve the tensile strength and aging resistance of the matrix resin.
[0106] Compared with Example 1, Comparative Example 9 differs in that nano-silica is replaced by an equal weight portion of calcium carbonate; the test results show that the tensile strength before aging is lower than that of Example 1, and the tensile strength retention rate is also reduced after 3000 hours of UV aging treatment, indicating that nano-silica can better improve the performance of fiberglass composite materials than other fillers, such as calcium carbonate.
[0107] Compared with Example 1, Comparative Example 10 differs in that the feldspar powder is replaced by an equal weight portion of calcium carbonate, and the nano-silica is replaced by an equal weight portion of 1 um silica; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and the tensile strength retention rate is also reduced after 3000 hours of UV aging treatment, indicating that the nano-silica particle size and the feldspar filler provided by the present invention can better improve the performance of the glass fiber reinforced plastic composite material.
[0108] The difference between Comparative Example 11 and Example 1 is that the preparation steps of the FRP composite material are different; the test results show that the tensile strength before aging is significantly lower than that of Example 1, and after 3000 hours of UV aging treatment, the tensile strength retention rate is also significantly reduced, indicating that the FRP composite material prepared by the preparation method of the present invention has better performance.
[0109] From the test results of the above embodiments and comparative examples, it can be seen that the high-performance fiberglass composite material provided by the present invention has excellent strength and anti-aging ability.
[0110] Although the embodiments of the present description have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present description, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A high-performance fiberglass composite material, It is characterized in that The invention comprises the following components in parts by weight: 50-80 parts of phenolic resin, 15-30 parts of epoxy resin, 10-20 parts of alkyd resin, 10-20 parts of glass fiber, 20-40 parts of basalt fiber, 10-20 parts of silicon fiber, 3-10 parts of feldspar powder, 5-15 parts of nano silicon dioxide, 1-9 parts of crosslinking agent, 0.1-3 parts of antioxidant, 0.5-3 parts of curing agent and 0.5-3 parts of accelerator; the silicon fiber is silicon nitride fiber; the epoxy resin is phenolic epoxy resin; the high performance glass fiber is 10-20 parts of basalt fiber, 10-20 parts of glass ...; the high performance glass fiber is 10-20 parts of basalt fiber, 10-20 parts of basalt fiber, 10-20 The preparation method of a glass fiber reinforced plastic composite material comprises the following steps: S1, mixing phenolic resin, epoxy resin, alkyd resin, feldspar powder and nano-silicon dioxide to obtain a mixed resin; S2, mixing glass fiber, basalt fiber, silicon fiber and 1 / 3 weight of a cross-linking agent, stirring to obtain a mixed fiber; S3, mixing the mixed resin, the mixed fiber, the remaining 2 / 3 of the cross-linking agent, an antioxidant, a curing agent and an accelerator, stirring, pouring into a corresponding mold for cooling and forming, and obtaining a high-performance glass fiber reinforced plastic composite material.
2. The high performance fiberglass composite material according to claim 1, It is characterized in that The weight ratio of the glass fiber:basalt fiber:silicon fiber is 1-2:1.5-3:1-2.
3. The high performance fiberglass composite material according to claim 1, It is characterized in that The particle size of the nano silicon dioxide is 30-60nm.
4. The high performance fiberglass composite material according to claim 1, It is characterized in that The feldspar powder is potassium feldspar powder with a particle size of 50-100nm.
5. The high performance fiberglass composite material according to claim 1, It is characterized in that The crosslinking agent includes one or more of a silicate crosslinking agent, an aminosilane crosslinking agent, a methoxysilane crosslinking agent, and a styrene silane crosslinking agent.
6. The high performance fiberglass composite material according to claim 1, It is characterized in that The curing agent includes one or more of an organic amine curing agent and an organic acid anhydride curing agent.
7. The high performance fiberglass composite material according to claim 1, It is characterized in that The accelerator includes one or more of isooctyl organic acid cobalt, cycloalkane organic acid cobalt, N,N-dimethylaniline, and N,N-diethylaniline.