A high-adhesion weather-resistant waterborne polyurethane coating and preparation method thereof
Modification of polyester polyol by hydrophilic polyether-modified MDT silicone resin solves the shortcomings of water-based polyurethane coatings in terms of weather resistance and adhesion, and achieves the improvement of high adhesion, weather resistance and flexibility, and solves the problem of In the prior art, there are problems of narrow selection of ingredients and limited improvement effects.
Patent Information
- Application Number
- CN202410543192.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-04
AI Technical Summary
The existing water-based polyurethane coatings have limited improvements in weather resistance and adhesion, and the composition is complex and the choice is narrow, making it difficult to adjust performance by curing agents.
Hydrophilic polyether modified MDT silicone resin is used to modify the polyester polyol. Through the branching and copolymerization of T-links, water dispersion and compatibility are improved, and the chemical connection between polysiloxane and polyurethane is realized. , prepare high adhesion weatherable water-resistant polyurethane coatings.
It significantly improves the weather resistance, adhesion and flexibility of water-based polyurethane coatings, and combines the excellent characteristics of silicone, polyester polyol and polyether polyol.
Smart Images

Figure BDA0004821587110000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a high-adhesion weather-resistant waterborne polyurethane coating and a preparation method thereof. Background Art
[0002] Polyurethane is a block polymer formed by alternating condensation of polyols as flexible segments and diisocyanates and low molecular weight chain extenders as rigid segments. Among them, polyurethane is divided into water-based polyurethane and oil-based polyurethane. Water-based polyurethane uses abundant water instead of solvent as a dispersant, which can reduce harm to the human body and the environment during production and use, and is an important development direction of the coatings industry.
[0003] Patent CN 115505096 B discloses a polyurethane with strong weather resistance and its preparation method, including raw material polymer diol, carbodiimide modified diphenylmethane diisocyanate, fluorosilicone modified acrylic resin, hydrophilic chain extender, weathering aid and deionized water. By using carbodiimide modified diphenylmethane diisocyanate instead of ordinary diisocyanate, and adding fluorosilicone modified acrylic resin, the water resistance and weather resistance of polyurethane are effectively improved under the synergy of carbodiimide modified diphenylmethane diisocyanate and fluorosilicone modified acrylic resin. Patent CN112876974 B discloses a high-adhesion waterborne polyurethane coating, which uses polytetramethylene ether glycol as the main agent and 4,4-dicyclohexylmethane diisocyanate as the curing agent. The adhesion of the obtained waterborne polyurethane coating is significantly improved under the synergistic effect of jatropha oil and the curing agent. However, the above-mentioned prior art generally has the problem of complex composition or narrow selection of component compatibility. Furthermore, the performance is mainly adjusted through the selection of curing agent, and the improvement effect is limited.
[0004] Polyols used in polyurethane synthesis are mainly divided into polyester polyols and polyether polyols. Polyester polyols have good mechanical properties, chemical resistance, adhesion to various substrates, and good heat resistance. Polyether polyols have limited tolerance to certain chemicals and solvents, low heat resistance, but good hydrolysis stability and low-temperature flexibility. Therefore, the modification of polyols often improves the performance of polyurethane more significantly.
[0005] Patent CN 109180915 B discloses a liquid polyester polyol for polyurethane coating. Considering the small molecular dibasic acid and diol as the raw materials for synthesizing polyester polyol, the small molecular dibasic acid uses a mixed dibasic acid, and the small molecular diol uses two or more diols, and one of them must contain a branched structure. This ensures that the obtained polyester polyol has a high degree of structural irregularity and asymmetry. The obtained polyester is not easy to crystallize or does not crystallize, and is liquid at room temperature or low temperature, maintaining good fluidity, which is conducive to the preparation of the main agent component in the two-component polyurethane coating and meets the basic requirements of stability, fluidity, etc. However, the improvement of weather resistance and adhesion is limited.
[0006] Organic silicon materials contain Si-O bonds with high bond energy (422.2 kJ / mol) and near-zero rotation barriers. Moreover, polysiloxane has a large single molecule volume and low cohesive energy density, so it has excellent properties such as high and low temperature resistance, weather aging resistance, good flexibility, and good processing fluidity. Therefore, it is an ideal material for polyurethane modified products. However, due to the hydrophobic and low surface energy characteristics of polysiloxane, its application effect in waterborne polyurethane is poor. Summary of the invention
[0007] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a high-adhesion weather-resistant waterborne polyurethane coating. The present invention uses a specific hydrophilic polyether-modified MDT silicone resin to modify polyester polyols, thereby improving its water dispersibility and significantly improving the weather resistance, adhesion and flexibility of the resulting waterborne polyurethane coating.
[0008] Another object of the present invention is to provide a method for preparing the above-mentioned high-adhesion weather-resistant waterborne polyurethane coating.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] A high-adhesion weather-resistant waterborne polyurethane coating comprises the following components in parts by weight:
[0011] 15-30 parts of polyether polyol, 15-30 parts of polyester polyol, 20-40 parts of polyisocyanate curing agent, 0-5 parts of hydrophilic chain extender, 0-10 parts of filler, 0-30 parts of cosolvent, 50-150 parts of water;
[0012] The polyester polyol is a hydrophilic MDT silicone resin modified polyester polyol, which is prepared by the following method:
[0013] (1) adding hydrogen-containing MDT silicone resin and allyl polyether into an organic solvent and mixing them evenly, then adding chloroplatinic acid catalyst, heating to 60-90° C. for addition reaction, and obtaining polyether-modified MDT silicone resin;
[0014] (2) Adding polyether-modified MDT silicone resin, dibasic acid and small molecule diol into a reaction kettle, heating and stirring to mix, adding titanate catalyst under nitrogen protection, heating to 180-240° C. to keep the temperature for reaction, and obtaining hydrophilic MDT silicone resin-modified polyester polyol.
[0015] Furthermore, the hydrogen-containing MDT silicone resin in step (1) has a weight average molecular weight (Mw) of 3000 to 8000 g / mol and an active hydrogen content of 0.1% to 0.8% (wt%). It can be prepared by the following method:
[0016] Add dialkoxysilane (D), trialkoxysilane (T) and acid catalyst solution into the reaction kettle, heat to 30-60°C for hydrolysis reaction; then add end-capping agent tetramethyl disiloxane (MM H ), and the temperature is raised to 60-80° C. to carry out copolymerization equilibrium reaction to obtain hydrogenated MDT silicone resin.
[0017] Preferably, the mass ratio of the dialkoxysilane, trialkoxysilane and the end-capping agent tetramethyldisiloxane is 100:10 to 30:10 to 40. The dialkoxysilane can be selected from methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane; the trialkoxysilane can be selected from methyltrimethoxysilane or methyltriethoxysilane.
[0018] Preferably, the acid catalyst solution is hydrochloric acid or sulfuric acid solution, and the hydrolysis reaction time is 1 to 4 hours.
[0019] Preferably, the copolymerization equilibrium reaction time is 2 to 6 hours; after the copolymerization equilibrium reaction is completed, the reaction is allowed to stand for stratification, and the oil phase is vacuum dried at 100 to 140° C. to remove water and low-boiling impurities to obtain a hydrogenated MDT silicone resin.
[0020] Furthermore, the allyl polyether in step (1) is allyl polyethylene glycol with a molecular weight of 500 to 2000 and a hydroxyl value of 25 to 120 mgKOH / g.
[0021] Furthermore, the molar ratio of the amount of the allyl polyether added in step (1) to the active hydrogen content in the hydrogen-containing MDT silicone resin is 0.05 to 0.4:1.
[0022] Furthermore, the organic solvent in step (1) is toluene.
[0023] Furthermore, the addition reaction time in step (1) is 2 to 6 hours, and after the reaction is completed, the organic solvent is removed in vacuo to obtain a polyether-modified MDT silicone resin.
[0024] Furthermore, the dibasic acid in step (2) is an aliphatic dicarboxylic acid or an aromatic dicarboxylic acid. Aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, etc.; aromatic dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, etc.; the small molecule diol is an aliphatic diol having 2 to 6 carbon atoms, such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol or 1,6-hexanediol.
[0025] Furthermore, in step (2), the molar ratio of the dibasic acid to the small molecule diol is 1:1-1.2; and the added amount of the polyether-modified MDT silicone resin is 10%-80% of the total mass of the dibasic acid and the small molecule diol.
[0026] Furthermore, the heat preservation reaction in step (2) refers to firstly heat preservation reaction under closed conditions until the acid value is less than 5 mgKOH / g, and then dehydration reaction by reduced pressure distillation until the acid value is less than 1 mgKOH / g and the hydroxyl value is 40 to 120 mgKOH / g, thereby obtaining a hydrophilic MDT silicone resin modified polyester polyol.
[0027] Furthermore, the polyether polyol is at least one of polyethylene glycol, polypropylene glycol and polybutylene glycol with a molecular weight of 400 to 2000.
[0028] Furthermore, the polyisocyanate curing agent is at least one of HDI (hexamethylene diisocyanate), HDI trimer, HDI-TMP (trimethylolpropane) adduct, TDI (toluene diisocyanate), TDI trimer, TDI-TMP adduct, IPDI (isophorone diisocyanate), IPDI trimer, IPDI-TMP adduct, MDI (diphenylmethane diisocyanate), MDI trimer, and MDI-TMP adduct.
[0029] Furthermore, the hydrophilic chain extender is at least one of ethylenediamine, diethylenetriamine, triethylenetetramine, diethanolamine, triethanolamine, and N-methyldiethanolamine.
[0030] Furthermore, the filler is at least one of calcium carbonate, barium sulfate, talc, kaolin, quartz powder, white carbon black, mica powder, wollastonite, and bentonite.
[0031] Furthermore, the co-solvent is at least one of isopropanol and tert-butanol.
[0032] The preparation method of the above-mentioned high-adhesion weather-resistant waterborne polyurethane coating comprises the following preparation steps:
[0033] Add polyether polyol, polyester polyol and cosolvent into water, heat to 50-100°C, stir and dissolve evenly, then add filler, stir and disperse evenly, cool to room temperature, add polyisocyanate curing agent and hydrophilic chain extender, stir and dissolve evenly, and obtain high adhesion and weather-resistant waterborne polyurethane coating.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The present invention adopts hydrophilic MDT silicone resin to modify polyester polyol, which contains a large number of branched and blocked hydrophilic polyether chains through the branching of T segments and the use of hydrophilic polyether end-capping, thereby improving the water solubility of silicone resin and the compatibility with polyether polyol and polyisocyanate curing agent. Through further copolymerization and curing reactions, chemical connection between polysiloxane and polyurethane is achieved, and effective modification of waterborne polyurethane system by polysiloxane is achieved.
[0036] (2) The hydrophilic MDT silicone resin modified polyester polyol used in the present invention has the advantages of silicone, polyester polyol and polyether polyol. The prepared waterborne polyurethane coating has the characteristics of high adhesion, high strength, good weather resistance and flexibility. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0038] Example 1
[0039] A high-adhesion weather-resistant waterborne polyurethane coating comprises the following components in parts by weight:
[0040] 20 parts of polyethylene glycol-600, 20 parts of hydrophilic MDT silicone resin modified polyester polyol, 30 parts of HDI-TMP adduct, 2 parts of triethanolamine, 5 parts of white carbon black, 15 parts of isopropanol, and 100 parts of water.
[0041] The hydrophilic MDT silicone resin modified polyester polyol is prepared by the following method:
[0042] (1) 10 kg of dimethyldiethoxysilane, 2 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor and heated to 45 °C for hydrolysis reaction for 2 h; then 3 kg of end-capping agent tetramethyldisiloxane (MM H ), the temperature was raised to 75°C for copolymerization equilibrium reaction for 4 hours, and after the reaction was completed, the phase was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.28wt.% by sampling titration method, and the weight average molecular weight was 5520g / mol by GPC.
[0043] (2) Take 5 kg of hydrogenated MDT silicone resin and 2.5 kg of allyl polyether APEG-800 (hydroxyl value 71 mgKOH / g) and add them to 5 kg of toluene solvent, stir and dissolve them, then add 40 ml of 3 wt% chloroplatinic acid isopropanol solution as catalyst, heat to 85°C for addition reaction for 3 hours, take samples to detect the olefin content, and the reaction is complete. Then remove the organic solvent in vacuo to obtain polyether-modified MDT silicone resin.
[0044] (3) 2kg of polyether-modified MDT silicone resin, 1.18kg of succinic acid, 2.02kg of sebacic acid and 1.98kg of 1,4-butanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1wt% of n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220°C and sealed for reaction for 4 hours, during the reaction, the acid value of the mixture was tested every half an hour until the acid value of the mixture was less than 5mgKOH / g. Then, the mixture was subjected to reduced pressure distillation and dehydration reaction at 220-240°C until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1 hour. The hydroxyl value of the product was 87.4mgKOH / g after sampling and testing, and a hydrophilic MDT silicone resin modified polyester polyol was obtained.
[0045] The high-adhesion weather-resistant waterborne polyurethane coating is prepared by the following method:
[0046] Weigh each raw material by weight, add polyethylene glycol-600, hydrophilic MDT silicone resin modified polyester polyol and isopropyl alcohol into water, heat to 80-85°C, stir and dissolve evenly, then add white carbon black, stir and disperse evenly, cool to room temperature, then add HDI-TMP adduct and triethanolamine, stir and dissolve evenly, to obtain a high adhesion and weather-resistant water-based polyurethane coating.
[0047] Example 2
[0048] A high-adhesion weather-resistant waterborne polyurethane coating comprises the following components in parts by weight:
[0049] 15 parts of polypropylene glycol-400, 30 parts of hydrophilic MDT silicone resin modified polyester polyol, 40 parts of HDI-TMP adduct, 5 parts of diethylenetriamine, 30 parts of tert-butyl alcohol, and 50 parts of water.
[0050] The hydrophilic MDT silicone resin modified polyester polyol is prepared by the following method:
[0051] (1) 10 kg of methyldiethoxysilane, 3 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor and heated to 55 °C for hydrolysis reaction for 2 h; then 4 kg of end-capping agent tetramethyldisiloxane (MM H), the temperature was raised to 80°C for copolymerization equilibrium reaction for 4 hours, and after the reaction was completed, the mixture was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.63wt.% by sampling titration method, and the weight average molecular weight was 3850g / mol by GPC.
[0052] (2) Take 5 kg of hydrogenated MDT silicone resin and 1.5 kg of allyl polyether APEG-500 (hydroxyl value 105 mgKOH / g) and add them to 5 kg of toluene solvent, stir and dissolve them, then add 40 ml of 3 wt% chloroplatinic acid isopropanol solution as catalyst, heat to 80°C for addition reaction for 4 hours, take samples to detect the olefin content, and the reaction is complete. Then remove the organic solvent in vacuo to obtain polyether-modified MDT silicone resin.
[0053] (3) 1 kg of polyether-modified MDT silicone resin, 1.18 kg of succinic acid, 1.88 kg of azelaic acid and 2.45 kg of 1,6-hexanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1 wt% of n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220°C and sealed for reaction for 4 hours, during the reaction, the acid value of the mixture was tested every half an hour until the acid value of the mixture was less than 5 mgKOH / g. Then, the mixture was subjected to reduced pressure distillation and dehydration reaction at 220-240°C until the acid value was less than 1 mgKOH / g, and the vacuum insulation reaction was continued for 1 hour. The hydroxyl value of the product was 105.6 mgKOH / g after sampling and testing, and a hydrophilic MDT silicone resin-modified polyester polyol was obtained.
[0054] The high-adhesion weather-resistant waterborne polyurethane coating is prepared by the following method:
[0055] Weigh each raw material by weight, add polypropylene glycol-400, hydrophilic MDT silicone resin modified polyester polyol and tert-butyl alcohol into water, heat to 80-85°C, stir and dissolve evenly, cool to room temperature, then add HDI-TMP adduct and diethylenetriamine, stir and dissolve evenly to obtain a high adhesion and weather-resistant water-based polyurethane coating.
[0056] Example 3
[0057] A high-adhesion weather-resistant waterborne polyurethane coating comprises the following components in parts by weight:
[0058] 30 parts of polyethylene glycol-1200, 15 parts of hydrophilic MDT silicone resin modified polyester polyol, 20 parts of HDI-TMP adduct, 5 parts of white carbon black, 15 parts of tert-butyl alcohol, and 150 parts of water.
[0059] The hydrophilic MDT silicone resin modified polyester polyol is prepared by the following method:
[0060] (1) 10 kg of dimethyldiethoxysilane, 1 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor and heated to 45 °C for hydrolysis reaction for 2 h; then 1 kg of end-capping agent tetramethyldisiloxane (MM H ), the temperature was raised to 75°C for copolymerization equilibrium reaction for 3 hours, and after the reaction was completed, the phase was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.12wt.% by sampling titration method, and the weight average molecular weight was 7680g / mol by GPC.
[0061] (2) Take 5 kg of hydrogenated MDT silicone resin and 2 kg of allyl polyether APEG-1000 (hydroxyl value 52 mgKOH / g) and add them to 5 kg of toluene solvent, stir and dissolve them, then add 40 ml of 3 wt% chloroplatinic acid isopropanol solution as catalyst, heat to 85°C for addition reaction for 5 hours, take samples to detect the olefin content, and the reaction is complete. Then remove the organic solvent in vacuo to obtain polyether-modified MDT silicone resin.
[0062] (3) 4 kg of polyether-modified MDT silicone resin, 2.92 kg of adipic acid, 0.83 kg of phthalic acid, 1.52 kg of 1,3-propylene glycol, and 0.45 kg of 1,4-butanediol were added to a high-pressure reactor, heated, stirred, dissolved, and mixed. A 0.1 wt% concentration of n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220° C. and sealed for reaction for 4 hours. During the reaction, the acid value of the mixture was tested every half an hour until the acid value of the mixture was less than 5 mgKOH / g. Then, the mixture was subjected to reduced pressure distillation and dehydration reaction at 220-240° C. until the acid value was less than 1 mgKOH / g. The reaction was continued under vacuum for 1 hour. The hydroxyl value of the product was 66.5 mgKOH / g, and a hydrophilic MDT silicone resin-modified polyester polyol was obtained.
[0063] The high-adhesion weather-resistant waterborne polyurethane coating is prepared by the following method:
[0064] Weigh each raw material by weight, add polyethylene glycol-1200, hydrophilic MDT silicone resin modified polyester polyol and tert-butyl alcohol into water, heat to 80-85°C, stir and dissolve evenly, then add white carbon black, stir and disperse evenly, cool to room temperature, add HDI-TMP adduct, stir and dissolve evenly, and obtain a high adhesion and weather-resistant water-based polyurethane coating.
[0065] Comparative Example 1
[0066] A waterborne polyurethane coating, compared with Example 1, the polyester polyol is not modified with the hydrophilic MDT silicone resin, and the rest is the same. The polyester polyol is prepared by the following method:
[0067] 1.18kg succinic acid, 2.02kg sebacic acid and 1.98kg 1,4-butanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 110.6mgKOH / g when the sample was tested to obtain polyester polyol.
[0068] Comparative Example 2
[0069] A waterborne polyurethane coating, compared with Example 2, the polyester polyol is not modified with the hydrophilic MDT silicone resin, and the rest is the same. The polyester polyol is prepared by the following method:
[0070] 1.18kg succinic acid, 1.88kg azelaic acid and 2.45kg 1,6-hexanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220℃ and sealed for 4h, during the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 122.5mgKOH / g when the sample was tested to obtain polyester polyol.
[0071] Comparative Example 3
[0072] A waterborne polyurethane coating, compared with Example 3, the polyester polyol is not modified with the hydrophilic MDT silicone resin, and the rest is the same. The polyester polyol is prepared by the following method:
[0073] 2.92kg adipic acid, 0.83kg phthalic acid, 1.52kg 1,3-propylene glycol and 0.45kg 1,4-butanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 120.3mgKOH / g, and polyester polyol was obtained.
[0074] Comparative Example 4
[0075] A waterborne polyurethane coating, compared with Example 1, is modified by using the linear hydroxy silicone oil PDMS disclosed in the literature (Preparation of silicone-modified waterborne polyurethane coating and its antifouling performance [J], Journal of Functional Polymers, 2021, 34(4): 397-385) instead of the hydrophilic MDT silicone resin, and the rest is the same. The polyester polyol is prepared by the following method:
[0076] 2kg of hydroxy silicone oil PDMS, 1.18kg of succinic acid, 2.02kg of sebacic acid and 1.98kg of 1,4-butanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1wt% of n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220℃ and sealed for reaction for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 90.2mgKOH / g when the sample was tested to obtain polyester polyol.
[0077] The performance of the waterborne polyurethane coatings obtained in the above Examples 1 to 3 and Comparative Examples 1 to 4 was tested. The test method is: the obtained waterborne polyurethane coating is dried and heat-cured at 70 to 75°C, and then the performance of the corresponding coating or standard test sample is tested. Among them, the adhesion test refers to the standard GB / T 5210-2006, and the adhesion substrate adopts a hard steel plate; the tensile strength and elongation at break test refer to the standard GB / T 528-2009; the low-temperature flexibility test refers to the standard GB / T 6742-2007, and before the test, it is adjusted for 24 hours at a low temperature of (-30±2)°C and a relative humidity of (50±5)%; the weather resistance test refers to the standard GB / T 14522-2, and the light source is a UVA-340 fluorescent ultraviolet lamp with an irradiance of 0.89W / m 2 , the tensile strength retention rate and elongation at break retention rate after 600h artificial weathering were tested. The test results are shown in Table 1 below.
[0078] Table 1
[0079]
[0080] From the comparison results of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be seen that the polyurethane coating prepared by the present invention using hydrophilic MDT silicone resin to modify polyester polyol has significantly improved adhesion, strength, flexibility and weather resistance compared to conventional polyester polyol. From the comparison results of Example 1 and Comparative Example 4, it can be seen that after using linear hydroxy silicone oil PDMS to replace hydrophilic MDT silicone resin, the adhesion, strength, flexibility and weather resistance of the obtained waterborne polyurethane coating are significantly reduced. The reason is that the hydrophilicity and compatibility of linear hydroxy silicone oil PDMS are poor, and it is not suitable for improving the performance of waterborne polyurethane systems.
[0081] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high-adhesion weather-resistant waterborne polyurethane coating, characterized in that: The composition comprises the following components by weight: 15-30 parts of polyether polyol, 15-30 parts of polyester polyol, 20-40 parts of polyisocyanate curing agent, 0-5 parts of hydrophilic chain extender, 0-10 parts of filler, 0-30 parts of cosolvent, 50-150 parts of water; The polyester polyol is a hydrophilic MDT silicone resin modified polyester polyol, which is prepared by the following method: (1) adding hydrogen-containing MDT silicone resin and allyl polyether into an organic solvent and mixing them evenly, then adding chloroplatinic acid catalyst, heating to 60-90°C for addition reaction, and obtaining polyether-modified MDT silicone resin; (2) adding the polyether-modified MDT silicone resin, the dibasic acid and the small molecule diol into a reaction kettle, heating and stirring to mix, adding a titanate catalyst under nitrogen protection, heating to 180-240°C for heat preservation and reaction, and obtaining a hydrophilic MDT silicone resin-modified polyester polyol; The hydrogen-containing MDT silicone resin in step (1) has a weight average molecular weight of 3000-8000 g / mol and an active hydrogen content of 0.1%-0.8%; it is prepared by the following method: Adding dialkoxysilane, trialkoxysilane and acid catalyst solution into a reaction kettle, heating to 30-60°C for hydrolysis reaction; then adding end-capping agent tetramethyldisiloxane, heating to 60-80°C for copolymerization equilibrium reaction, and obtaining hydrogen-containing MDT silicone resin; The allyl polyether in step (1) is an allyl polyethylene glycol with a molecular weight of 500-2000 and a hydroxyl value of 25-120 mgKOH / g; the molar ratio of the amount of the allyl polyether added to the active hydrogen content in the hydrogen-containing MDT silicone resin is 0.05-0.4:1; The molar ratio of the dibasic acid to the small molecule diol in step (2) is 1:1-1.2; the amount of the polyether-modified MDT silicone resin added is 10%-80% of the total mass of the dibasic acid and the small molecule diol.
2. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The mass ratio of the dialkoxysilane, trialkoxysilane and end-capping agent tetramethyldisiloxane added is 100:10~30:10~40; the dialkoxysilane is selected from methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane; the trialkoxysilane is selected from methyltrimethoxysilane or methyltriethoxysilane.
3. The high adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The acid catalyst solution is hydrochloric acid or sulfuric acid solution, the hydrolysis reaction time is 1-4 hours, the copolymerization equilibrium reaction time is 2-6 hours, after the copolymerization equilibrium reaction is completed, the reaction is allowed to stand and the layers are separated, and the oil phase is vacuum dried at 100-140° C. to remove water and low-boiling impurities, thereby obtaining a hydrogenated MDT silicone resin.
4. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The addition reaction time in step (1) is 2 to 6 hours. After the reaction is completed, the organic solvent is removed in vacuo to obtain a polyether-modified MDT silicone resin.
5. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The dibasic acid in step (2) is an aliphatic dicarboxylic acid or an aromatic dicarboxylic acid; and the small molecule diol is an aliphatic diol having 2 to 6 carbon atoms.
6. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The heat preservation reaction in step (2) refers to firstly heat preservation reaction under closed conditions until the acid value is less than 5 mgKOH / g, and then dehydration reaction by reduced pressure distillation until the acid value is less than 1 mgKOH / g and the hydroxyl value is 40-120 mgKOH / g, thereby obtaining a hydrophilic MDT silicone resin modified polyester polyol.
7. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The polyether polyol is at least one of polyethylene glycol, polypropylene glycol, and polybutylene glycol with a molecular weight of 400 to 2000; the polyisocyanate curing agent is at least one of HDI, HDI trimer, HDI-TMP adduct, TDI, TDI trimer, TDI-TMP adduct, IPDI, IPDI trimer, IPDI-TMP adduct, MDI, MDI trimer, and MDI-TMP adduct.
8. The high-adhesion weather-resistant waterborne polyurethane coating according to claim 1, characterized in that: The hydrophilic chain extender is at least one of ethylenediamine, diethylenetriamine, triethylenetetramine, diethanolamine, triethanolamine, and N-methyldiethanolamine; the filler is at least one of calcium carbonate, barium sulfate, talcum powder, kaolin, quartz powder, white carbon black, mica powder, wollastonite, and bentonite; and the cosolvent is at least one of isopropanol and tert-butanol.
9. The method for preparing a high-adhesion weather-resistant waterborne polyurethane coating according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: Add polyether polyol, polyester polyol and cosolvent into water, heat to 50-100°C, stir and dissolve evenly, then add filler, stir and disperse evenly, cool to room temperature, add polyisocyanate curing agent and hydrophilic chain extender, stir and dissolve evenly, to obtain high adhesion and weather-resistant waterborne polyurethane coating.