A method for preparing a laminated aluminum oxide film based on ALD process
Through the improved ALD process, a multi-layer aluminum oxide film is constructed to regulate the H2O and TMA sources on the bottom and top layers, solving the problem of insufficient thickness of the aluminum oxide film in solar cells, improving the electrical performance and efficiency of the cell, and reducing the cost.
Patent Information
- Application Number
- CN202410804183.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-21
AI Technical Summary
It is difficult to prepare a thick enough aluminum oxide film in solar cells with the existing technology, resulting in substandard UV test indicators, which in turn affects the performance attenuation speed and power generation of the cell. In addition, the traditional process cannot print the slurry well due to the dense film layer. Ohmic contact reduces cell efficiency.
Using an improved ALD process, by constructing a multi-layer aluminum oxide film, the bottom layer has a small amount of H2O source and a large amount of TMA source, and the top layer has a large amount of H2O source and a small amount of TMA source. The amount and time of TMA and water vapor are controlled to form a laminated aluminum oxide film. layer to ensure film thickness and performance.
It has improved the electrical performance of the battery, increased the open circuit voltage (Voc) and fill factor (FF), enhanced the conversion efficiency of the battery, and reduced the cost, avoiding low conversion efficiency and thin film strips caused by the thickness of the aluminum oxide film. Here comes the question of UV testing.
Smart Images

Figure CN118380510B_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for preparing a laminated aluminum oxide film layer based on an ALD process, and belongs to the field of solar cell technology and semiconductor technology. Background Art
[0002] Aluminum oxide is deposited on the front of the Topcon battery. The film is dense and the sintering window is narrow, which makes it impossible for the aluminum oxide film to be thicker. The thickness of the aluminum oxide will affect the UV test indicators at the component end (downstream of the battery) (simulating ultraviolet radiation from sunlight to accelerate the efficiency decay of the battery cell, thereby testing the performance decay rate of the battery cell in a short period of time). If the thickness is not enough, the UV test attenuation is large, which will directly lead to the decay of the battery's power generation over time.
[0003] Due to the requirements of UV test indicators, related tests on indicators of different aluminum oxide film thicknesses such as 1~5nm were conducted. It was found that aluminum oxide films above 4nm can easily pass the test, while the battery performance of low-thickness cells is greatly attenuated, which is inversely proportional to the film thickness. In addition, battery performance tracking and verification was carried out for aluminum oxide cells with different film thicknesses. It was found that the battery efficiency was better when the film thickness was 2-3nm, while both low and high film thicknesses showed a downward trend in FF (fill factor). Under current technology, only 2-3nm aluminum oxide films can be made, which does not meet the UV test requirements of the component end. If thicker aluminum oxide films are continued to grow, the printed slurry cannot have good ohmic contact due to the dense film layer, which leads to reduced efficiency of the battery cell. Summary of the invention
[0004] In order to solve the above problems, the present invention improves the atomic layer deposition (ALD) process, changing the traditional single aluminum oxide film into a multi-layer aluminum oxide film; specifically, the process is changed into a bottom layer with a small amount of H2O source and a large amount of TMA (trimethylaluminum) source, and a top layer with a large amount of H2O source and a small amount of TMA source (the traditional process is a single aluminum oxide layer, and the amounts of H2O and TMA sources are moderate).
[0005] The specific plan is as follows:
[0006] A method for preparing a laminated aluminum oxide film layer based on an ALD process comprises the following steps:
[0007] S1. Placing the substrate in an atomic layer deposition chamber, and performing vacuuming, leak detection, and temperature and pressure regulation on the chamber;
[0008] S2, continuously introducing water vapor into the atomic layer deposition chamber to pre-treat the silicon wafer;
[0009] S3, constructing a bottom film: introducing TMA to deposit on the surface of the silicon wafer, then introducing an inert gas to purge away excess TMA; then introducing water vapor to deposit on the surface of the silicon wafer to react with the previously deposited TMA to form an Al2O3 film on the surface of the silicon wafer, and finally introducing an inert gas to purge away excess water; repeating the above process to obtain a bottom film;
[0010] S4, constructing a top film: introducing TMA to deposit on the surface of the silicon wafer, then introducing an inert gas to purge away excess TMA; then introducing water vapor to deposit on the surface of the silicon wafer to react with the previously deposited TMA to form an Al2O3 film on the surface of the silicon wafer, and finally introducing an inert gas to purge away excess water; repeating the above process to obtain a top film;
[0011] S5, evacuating and purging the remaining gas in the reaction chamber, and filling the chamber with nitrogen to back-pressure, thereby obtaining a laminated aluminum oxide film layer;
[0012] Moreover, the amount of TMA introduced into S3 is higher than that introduced into S4.
[0013] And / or, the amount of water vapor introduced into S3 is lower than the amount of water vapor introduced into S4.
[0014] In one embodiment of the present invention, in S3, the amount of TMA introduced is 20-70 torr for 3-10 seconds. It can further be selected that 20-70 torr is introduced for 4-10 seconds. Preferably, 20-70 torr is introduced for 7-10 seconds.
[0015] In one embodiment of the present invention, in S3, the amount of water vapor introduced is 20-70 torr, and the time is 3-6 seconds.
[0016] In one embodiment of the present invention, in S3, the number of repetitions is 5-15 times.
[0017] In one embodiment of the present invention, in S4, the amount of TMA introduced is 20-70 torr, and the time is 3-6 s.
[0018] In one embodiment of the present invention, in S4, the amount of water vapor introduced is 20-70 torr for 3-10 seconds, and further, 20-70 torr can be introduced for 8-10 seconds.
[0019] In one embodiment of the present invention, in S4, the number of repetitions is 10-30 times.
[0020] In one embodiment of the present invention, the method for preparing a stacked aluminum oxide film layer based on the ALD process satisfies at least one of the following conditions: the amount of TMA contained in the bottom film in the multilayer aluminum oxide film is higher than the amount of TMA contained in the top film, and / or the amount of H2O contained in the bottom film in the multilayer aluminum oxide film is lower than the amount of H2O contained in the top film.
[0021] In one embodiment of the present invention, there are three specific situations as follows:
[0022] a. The amount of TMA introduced into S3 is 20-70 torr, the time is 3-10 s, and the amount of water vapor introduced is 20-70 torr, the time is 3-6 s; the amount of TMA introduced into S4 is 20-70 torr, the time is 3-6 s, and the amount of water vapor introduced is 20-70 torr, the time is 3-10 s; and the amount of TMA introduced into S3 is higher than the amount of TMA introduced into S4.
[0023] b. The amount of TMA introduced into S3 is 20-70 torr, the time is 3-10 s, and the amount of water vapor introduced is 20-70 torr, the time is 3-6 s; the amount of TMA introduced into S4 is 20-70 torr, the time is 3-6 s, and the amount of water vapor introduced is 20-70 torr, the time is 3-10 s; and the amount of water vapor introduced into S3 is lower than the amount of water vapor introduced into S4.
[0024] c. The amount of TMA introduced into S3 is 20-70 torr, the time is 3-10 s, and the amount of water vapor introduced is 20-70 torr, and the time is 3-6 s; the amount of TMA introduced into S4 is 20-70 torr, the time is 3-6 s, and the amount of water vapor introduced is 20-70 torr, and the time is 3-10 s; and the amount of TMA introduced into S3 is higher than the amount of TMA introduced into S4, and the amount of water vapor introduced into S3 is lower than the amount of water vapor introduced into S4.
[0025] In one embodiment of the present invention, further, the amount of TMA introduced into S3 is 40-70 torr, and the time is 7-10 s; the amount of TMA introduced into S4 is 40 torr, and the time is 5 s.
[0026] In one embodiment of the present invention, further, the amount of water vapor introduced into S3 is 55 torr, and the time is 5 s; the amount of water vapor introduced into S4 is 20-70 torr, and the time is 3-10 s.
[0027] In one embodiment of the present invention, more preferably, the amount of water vapor introduced into S3 is 55 torr, and the time is 5 s; the amount of water vapor introduced into S4 is 55-70 torr, and the time is 8-10 s.
[0028] In one embodiment of the present invention, in S3 and S4, the inert gas may be N2. The inert gas is introduced at a flow rate of 10-30 L / min for 3-15 s.
[0029] In one embodiment of the present invention, in S1, the temperature and pressure adjustment process refers to adjusting the pressure to 0.05-0.5 torr and the temperature to 200-350°C.
[0030] In one embodiment of the present invention, the pretreatment conditions in S1 are a water vapor introduction rate of 20-70 torr and a time of 30-120 seconds.
[0031] In one embodiment of the present invention, a method for preparing a laminated aluminum oxide film layer based on an ALD process specifically comprises the following steps:
[0032] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.05-0.5 torr and a temperature of 200-350°C;
[0033] S2: Continuously introduce water (steam) into the reaction chamber to pre-treat the silicon wafer, with the amount of water vapor introduced being 20-70 torr for 30-120 seconds;
[0034] S3. Building the top membrane:
[0035] TMA (trimethylaluminum) is introduced and deposited on the surface of the silicon wafer. The TMA amount is 20-70 torr and the time is 3-10 seconds. Then an inert gas such as N2 is introduced to purge the excess TMA. The N2 flow rate is 10-30 L / min and the time is 3-15 seconds.
[0036] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form AL2O3 on the surface of the silicon wafer. The amount of H2O is 20-70torr and the time is 3-6s. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 10-30L / min and the time is 3-15s.
[0037] Repeat the above process 5-15 times;
[0038] S4. Construction of top membrane:
[0039] TMA (trimethylaluminum) is introduced and deposited on the surface of the silicon wafer. The TMA amount is 20-70 torr and the time is 3-6 seconds. Then an inert gas such as N2 is introduced to purge the excess TMA. The N2 flow rate is 10-30 L / min and the time is 3-15 seconds.
[0040] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form AL2O3 on the surface of the silicon wafer. The amount of H2O is 20-70torr and the time is 4-10s. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 10-30L / min and the time is 3-15s.
[0041] Repeat the above process 10-30 times;
[0042] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0043] The present invention prepares and improves a laminated aluminum oxide film layer based on the above method.
[0044] The present invention also provides application of the laminated aluminum oxide film layer in the battery field.
[0045] The present invention also provides a battery manufacturing process, comprising the following steps:
[0046] The original silicon wafer is alkali-textured to prepare the texture surface; boron diffusion is used to prepare the PN junction; the silicon wafer is cleaned to remove the borosilicate glass, etc.; LPCVD is used to prepare the tunneling oxide layer and the amorphous silicon thin layer; phosphorus diffusion is used to dope the back of the battery with phosphorus; and the silicon wafer is cleaned;
[0047] According to the above method, a front Al2O3 film is prepared to increase the passivation effect; a front and back silicon nitride film is prepared; and electrodes are screen printed, sintered and tested.
[0048] The present invention also provides a battery product manufactured based on the battery manufacturing process.
[0049] Beneficial effects of the present invention:
[0050] The process of the present invention has been verified by mature large samples, and has relative advantages in the electrical performance of the battery cell, because Voc (open circuit voltage) and FF (fill factor) have gains, thereby improving the conversion efficiency of the battery.
[0051] The process advantages of the present invention include:
[0052] Cost advantage: The existing method uses plate ALD, the film quality can be relatively loose, and the film can grow to the required thickness, but the plate ALD capacity is half of the tubular ALD, and the price is about twice that of the tubular ALD; the process of the present invention has a cost advantage over the process based on plate ALD equipment;
[0053] Product performance advantages: Based on the battery performance improvement obtained by the process of the present invention, there is no need to worry about the low conversion efficiency caused by thick aluminum oxide or the UV testing problems caused by thin aluminum oxide film. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a process flow chart of preparing a laminated aluminum oxide film layer based on the ALD process of the present invention.
[0055] Figure 2 The performance test results of the Al2O3 films obtained in various embodiments and comparative examples are shown in FIG. DETAILED DESCRIPTION
[0056] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are partial embodiments of the present invention, rather than all embodiments.
[0057] Example 1
[0058] An ALD stacked film process comprises the following steps:
[0059] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0060] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55 torr, and the time is 60s;
[0061] S3. Preparation of bottom film:
[0062] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer, with a TMA amount of 40 torr and a time of 7 seconds; then an inert gas, such as N2, is introduced to purge the excess TMA, with a N2 flow rate of 30 L / min and a time of 7 seconds;
[0063] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0064] Repeat the above process 10 times;
[0065] S4. Preparation of top film:
[0066] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0067] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 8s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30 L / min and the time is 7s.
[0068] Repeat the above process 20 times;
[0069] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, complete the process, and obtain the front-side AL2O3 film passivated silicon wafer.
[0070] Example 2
[0071] Referring to Example 1, the amount of TMA in S3 was adjusted to 70 torr and the time was 10 s; and the amount of H2O in S4 was adjusted to 20 torr and the time was 3 s; and the rest remained unchanged.
[0072] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0073] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55 torr, and the time is 60s;
[0074] S3. Preparation of bottom film:
[0075] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer, with a TMA amount of 70 torr and a time of 10 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA, with a N2 flow rate of 30 L / min and a time of 7 seconds.
[0076] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0077] Repeat the above process 10 times;
[0078] S4. Preparation of top film:
[0079] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0080] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 20 torr and the time is 3s. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 30 L / min and the time is 7s.
[0081] Repeat the above process 20 times;
[0082] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, complete the process, and obtain the front-side AL2O3 film passivated silicon wafer.
[0083] Example 3
[0084] Referring to Example 1, the amount of TMA in S3 was adjusted to 20 torr and the time was 3 s; and the amount of H2O in S4 was adjusted to 70 torr and the time was 10 s; and the rest remained unchanged.
[0085] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0086] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55 torr, and the time is 60s;
[0087] S3. Preparation of bottom film:
[0088] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer, with a TMA amount of 20 torr and a time of 3 seconds; then an inert gas, such as N2, is introduced to purge the excess TMA, with a N2 flow rate of 30 L / min and a time of 7 seconds;
[0089] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0090] Repeat the above process 10 times;
[0091] S4. Preparation of top film:
[0092] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0093] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 70 torr and the time is 10s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30 L / min and the time is 7s.
[0094] Repeat the above process 20 times;
[0095] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, complete the process, and obtain the front-side AL2O3 film passivated silicon wafer.
[0096] Example 4
[0097] Referring to Example 1, the amount of TMA in S3 was adjusted to 70 torr and the time was 10 s; and the amount of H2O in S4 was adjusted to 70 torr and the time was 10 s; and the rest remained unchanged.
[0098] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0099] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55 torr, and the time is 60s;
[0100] S3. Preparation of bottom film:
[0101] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer, with a TMA amount of 70 torr and a time of 10 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA, with a N2 flow rate of 30 L / min and a time of 7 seconds.
[0102] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0103] Repeat the above process 10 times;
[0104] S4. Preparation of top film:
[0105] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0106] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 70 torr and the time is 10s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30 L / min and the time is 7s.
[0107] Repeat the above process 20 times;
[0108] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, complete the process, and obtain the front-side AL2O3 film passivated silicon wafer.
[0109] Example 5
[0110] Referring to Example 1, the amount of TMA in S3 was adjusted to 20 torr and the time was 3 s; and the amount of H2O in S4 was adjusted to 20 torr and the time was 3 s; and the rest remained unchanged.
[0111] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0112] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55 torr, and the time is 60s;
[0113] S3. Preparation of bottom film:
[0114] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer, with a TMA amount of 20 torr and a time of 3 seconds; then an inert gas, such as N2, is introduced to purge the excess TMA, with a N2 flow rate of 30 L / min and a time of 7 seconds;
[0115] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55 torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0116] Repeat the above process 10 times;
[0117] S4. Preparation of top film:
[0118] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0119] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 20 torr and the time is 3s. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 30 L / min and the time is 7s.
[0120] Repeat the above process 20 times;
[0121] S5: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, complete the process, and obtain the front-side AL2O3 film passivated silicon wafer.
[0122] Comparative Example 1
[0123] Traditional process (single-layer film):
[0124] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0125] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55torr, the time is 60s;
[0126] S3. Preparation of aluminum oxide film:
[0127] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas such as N2 is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0128] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0129] Repeat the above process 30 times;
[0130] S4: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0131] Comparative Example 2
[0132] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0133] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55torr, the time is 60s;
[0134] S3. Preparation of aluminum oxide film:
[0135] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 70 torr for 10 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0136] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 55torr and the time is 5s. Then an inert gas such as N2 is introduced to purge the excess water. The N2 flow rate is 30L / min and the time is 7s.
[0137] Repeat the above process 30 times;
[0138] S4: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0139] Comparative Example 3
[0140] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0141] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55torr, the time is 60s;
[0142] S3. Preparation of aluminum oxide film:
[0143] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 40 torr for 5 seconds. Then an inert gas such as N2 is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0144] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 70 torr and the time is 10 seconds. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 30 L / min and the time is 7 seconds.
[0145] Repeat the above process 30 times;
[0146] S4: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0147] Comparative Example 4
[0148] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0149] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55torr, the time is 60s;
[0150] S3. Preparation of aluminum oxide film:
[0151] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 70 torr for 10 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0152] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 70 torr and the time is 10 seconds. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 30 L / min and the time is 7 seconds.
[0153] Repeat the above process 30 times;
[0154] S4: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0155] Comparative Example 5
[0156] S1: Place the substrate (silicon wafer) in the reaction chamber (atomic layer deposition chamber), and evacuate, leak test and heat the reaction chamber at a pressure of 0.1 torr and a temperature of 280°C.
[0157] S2, pretreatment: continuously introduce water (steam) into the reaction chamber to pretreat the silicon wafer, the water vapor volume is 55torr, the time is 60s;
[0158] S3. Preparation of aluminum oxide film:
[0159] TMA (trimethylaluminum) is introduced to deposit on the surface of the silicon wafer at a TMA amount of 20 torr for 3 seconds. Then an inert gas, such as N2, is introduced to purge the excess TMA at a N2 flow rate of 30 L / min for 7 seconds.
[0160] Then water (steam) is introduced to deposit on the surface of the silicon wafer and react with the previous TMA to form Al2O3 on the surface of the silicon wafer. The amount of H2O is 20 torr and the time is 3s. Then an inert gas such as N2 is introduced to purge excess water. The N2 flow rate is 30L / min and the time is 7s.
[0161] Repeat the above process 30 times;
[0162] S4: Evacuate and purge the remaining gas in the reaction chamber; fill the chamber with nitrogen to back-pressure, take out the wafer, and complete the process.
[0163] Application Example 1 Battery Preparation
[0164] The original silicon wafer is alkali-textured to prepare the texture surface; boron diffusion is used to prepare the PN junction; the silicon wafer is cleaned to remove the borosilicate glass, etc.; LPCVD is used to prepare the tunneling oxide layer and the amorphous silicon thin layer; phosphorus diffusion is used to dope the back of the battery with phosphorus; and the silicon wafer is cleaned;
[0165] According to the above method, a front Al2O3 film is prepared to increase the passivation effect; a front and back silicon nitride film is prepared; and electrodes are screen printed, sintered and tested.
[0166] The Al2O3 films of the embodiments and comparative examples were tested for performance; and the Al2O3 films of the embodiments and comparative examples were applied to solar cells of the same type, and then the performance of the solar cells was tested. The corresponding test results are shown in FIG. Figure 2 shown.
[0167] Figure 2 The electrical performance test results involved in the test were all statistically analyzed for confidence (p-value analysis), and the test samples and reference samples obtained were significantly different (p<0.05), thus eliminating the differences caused by test errors. In addition, the photoelectric conversion efficiency has been improved by 0.1~0.2% per year for more than ten years, so an absolute efficiency improvement of 0.1% is a huge improvement.
[0168] from Figure 2 It is known that compared with comparative example 1 (traditional process), Eta of Example 1 is greatly improved, which is mainly reflected in the obvious improvement of Voc and FF, indicating that changing the aluminum and oxygen ratio of the bottom membrane and the top membrane has obvious benefits on battery performance; compared with other examples, the battery performance of Example 1 is the best, indicating that there is room for improvement in battery performance when the bottom membrane is rich in aluminum and the top membrane is rich in oxygen, while the battery performance of Example 3 is also obviously reduced when the bottom membrane is less in aluminum and the top membrane is more in oxygen.
[0169] It can be seen that if the bottom layer uses a small amount of H2O source and a large amount of TMA source, there will be a lot of aluminum bonding during the film growth process. This type of bonding will promote the battery sintering contact and promote the sintering of the battery printed grid line and the silicon wafer to achieve good ohmic contact. The corresponding battery performance will increase FF (fill factor), which can be concluded by comparing with the traditional process (Comparative Example 1); if the top layer uses a large amount of H2O source and a small amount of TMA source, there will be a lot of oxygen bonding when growing this film, which will increase the field passivation effect of the battery cell, thereby increasing Voc (open circuit voltage).
[0170] Functions and Effects of the Embodiments
[0171] The improved principle of the present invention is as follows: a small amount of H2O source and a large amount of TMA source are used in the bottom layer. During the film growth process, many more aluminum bonds will be produced. Such bonds will promote the sintering contact of the battery, promote the sintering of the battery printed grid line and the silicon wafer to achieve good ohmic contact, and the corresponding battery performance will improve FF (fill factor); a large amount of H2O source and a small amount of TMA source are used in the top layer. When this layer of film is grown, many more oxygen bonds will be produced, which will increase the field passivation effect of the battery cell, thereby improving Voc (open circuit voltage).
[0172] Some other laminated film reports in the prior art, such as CN114420790A and CN117558764A, mainly involve using H-free oxidants (such as ozone) in combination with H-containing oxidants such as H2O to further improve the passivation effect of using H-containing oxidants alone; the corresponding principles are to achieve the performance of the overall laminated film while maintaining the same total aluminum bonding in the multilayer film but with a small proportion of aluminum-hydroxyl in the bottom film.
[0173] It can be seen that the present invention proposes a new improvement idea for the first time. There is no need to introduce a complex oxygen source system. Only H2O is used as the oxygen source. By regulating the amount of H2O source and TMA source in the bottom layer and the top layer of the laminated film, significant performance improvement can be achieved.
[0174] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for preparing a laminated aluminum oxide film based on an ALD process, characterized in that: The steps include: S1. Placing the substrate in an atomic layer deposition chamber, and performing vacuuming, leak detection, and temperature and pressure regulation on the chamber; S2, then continuously introducing water vapor into the atomic layer deposition chamber to pre-treat the silicon wafer; S3, constructing a bottom film: introducing TMA to deposit on the surface of the pretreated silicon wafer, then introducing an inert gas to purge away excess TMA; then introducing water vapor to deposit on the surface of the silicon wafer to react with the previously deposited TMA to form an Al2O3 film on the surface of the silicon wafer, and finally introducing an inert gas to purge away excess water; repeating the above process to obtain a bottom film; S4, constructing a top film: introducing TMA to be deposited on the surface of the silicon wafer with the bottom film, and then introducing an inert gas to purge away excess TMA; introducing water vapor to be deposited on the surface of the silicon wafer to react with the previously deposited TMA to form an Al2O3 film on the surface of the silicon wafer, and finally introducing an inert gas to purge away excess water; repeating the above process to obtain a top film; S5, evacuating and purging the remaining gas in the reaction chamber, and filling the chamber with nitrogen to back-pressure, thereby obtaining a laminated aluminum oxide film layer; Among them, the amount of TMA introduced into S3 is higher than the amount of TMA introduced into S4.
2. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S3, the amount of TMA introduced is 20-70 torr, and the time is 3-10 s.
3. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S3, the amount of water vapor introduced is 20-70 torr, and the time is 3-6 seconds.
4. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S3, the number of repetitions is 5-15 times.
5. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S4, the amount of TMA introduced is 20-70 torr and the time is 3-6 s.
6. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S4, the amount of water vapor introduced is 20-70 torr, and the time is 3-10 seconds.
7. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S4, the number of repetitions is 10-30 times.
8. The method for preparing a laminated aluminum oxide film based on the ALD process according to claim 1, characterized in that: In S3 and S4, the inert gas is specifically N2; the flow rate of the inert gas is 10-30 L / min, and the time is 3-15 s.
9. A laminated aluminum oxide film, characterized in that: The aluminum oxide film is prepared by the method for preparing a laminated aluminum oxide film based on an ALD process as described in any one of claims 1 to 8.
10. A battery product, characterized in that: A laminated aluminum oxide film layer comprising the laminated aluminum oxide film layer according to claim 9.
Citation Information
Patent Citations
Method for preparing laminated aluminum oxide film layer based on ALD (Atomic Layer Deposition) process
CN114420790A
Solar cell, preparation method thereof and photovoltaic module
CN117558764A
Atomic layer deposition method of low-temperature high-growth-rate silicon oxide film
CN112210769A
Method for improving inter-batch uniformity of ALD passive film of TOPCon battery and application
CN116682894A
Method for improving thickness uniformity of ALD (atomic layer deposition) film
CN116949429A