A high-rate graphite negative electrode material and its preparation process

By using microwave treatment and polyethylene oxide bonding, the interlayer spacing of natural graphite was widened and the pores were filled, which solved the problem of low lithium-ion conductivity of natural graphite and improved the rate performance and cycle stability of lithium-ion batteries.

CN118380572BActive Publication Date: 2024-11-12SHANGHAI BACUS SUPERCONDUCTING NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410822251.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-12
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Natural graphite anode materials have poor rate performance during charge and discharge processes due to their low lithium-ion conductivity.

Method used

By microwave treatment of natural graphite and the bonding effect of polyethylene oxide, the interlayer spacing is widened and the pores are filled, enhancing the lithium-ion transport capacity. At the same time, natural spherical graphite materials with appropriate particle size and OI value range are selected to ensure structural stability.

Benefits of technology

It significantly improves the rate performance and cycle stability of lithium-ion batteries, reduces the loss of active lithium, and enhances the first coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of negative electrode materials for lithium ion batteries. More specifically, it relates to a high-rate graphite negative electrode material and a preparation process thereof. The present invention comprises: mixing natural graphite and an acid solution, heating and stirring the reaction, filtering, washing and drying to obtain acid-treated natural graphite; dispersing the obtained acid-treated natural graphite in an emulsifier aqueous solution, ultrasonically dispersing it uniformly, centrifuging it, and drying it to a moisture content of 2%-5% to obtain pre-treated natural graphite; then treating the obtained pre-treated natural graphite under a microwave condition of 300-600W for 2-4h to obtain microwave-treated natural graphite; stirring and mixing the microwave-treated natural graphite and a polyethylene oxide N-methylpyrrolidone solution to obtain a mixture; then grinding the mixture for more than 10min to obtain a rubber abrasive; S3: subjecting the rubber abrasive to ultrasonic shearing, drying, and refining to obtain a natural graphite negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of negative electrode materials for lithium ion batteries, and more specifically, relates to a high-rate graphite negative electrode material and a preparation process thereof. Background Art

[0002] It has become a recognized fact that the development of high-performance lithium-ion batteries is highly dependent on the selection and preparation process of positive and negative electrode materials. At present, the most widely used positive electrode materials are mainly lithium iron phosphate positive electrode materials and nickel-cobalt-manganese ternary positive electrode materials, while negative electrode materials are mainly divided into carbon materials and non-carbon materials. Carbon materials mainly include: graphite, graphene and disordered carbon. At present, graphite negative electrode materials occupy the leading position in the application of lithium-ion batteries, such as artificial graphite and natural graphite. Non-carbon materials mainly include: silicon-based negative electrode materials and lithium titanate negative electrode materials. Silicon-based negative electrode materials are the future development direction of lithium batteries due to their high unit theoretical capacity and abundant reserves. However, in the process of forming silicon-lithium alloy compounds, the volume expansion reaches more than 300%, resulting in the separation of silicon negative electrode materials and conductive agents, reducing conductivity, causing rapid attenuation of battery capacity and shortening cycle life; huge expansion changes will cause active materials to fall off from the current collector, resulting in increased internal resistance of the battery, increased heat generation, and serious threats to battery safety. Lithium titanate anode materials have advantages such as wide working environment temperature range, strong rapid charge and discharge capability and excellent cycle stability, but they also face problems such as low energy density, high cost and flatulence. Therefore, for a long time in the future, graphite anode materials will continue to occupy the leading position in the lithium-ion battery anode material application market.

[0003] Cheap natural graphite anode materials have become one of the anode materials for lithium-ion batteries due to their high theoretical specific capacity, excellent electronic conductivity, and high reversibility of charge and discharge. However, natural graphite anodes have low lithium ion conductivity, and have problems such as poor rate performance and long-cycle stability during charge and discharge, and are prone to lithium dendrites, which limits their further application as high-performance electrochemical energy storage materials. Summary of the invention

[0004] The technical problem to be solved by the present invention is to solve the disadvantage that natural graphite has low lithium ion conductivity due to its own structural problems, which ultimately leads to poor rate performance during the charge and discharge process. A high-rate graphite negative electrode material and a preparation process thereof are provided.

[0005] One of the purposes of the present invention is to provide a process for preparing a high-rate graphite negative electrode material.

[0006] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0007] A preparation process of a high-rate graphite negative electrode material, the specific preparation process comprises the following steps:

[0008] S1: treating natural graphite under microwave conditions with a power of 300-600 W for 2-4 h to obtain microwave-treated natural graphite;

[0009] S2: stirring and mixing the microwave-treated natural graphite and the N-methylpyrrolidone solution of polyethylene oxide to obtain a mixture; then subjecting the mixture to a rubber grinding treatment for more than 10 minutes to obtain a rubber abrasive;

[0010] Wherein, in the polyethylene oxide N-methylpyrrolidone solution, the mass fraction of polyethylene oxide is 15%-20%; and the mass ratio of the microwave-treated natural graphite to the polyethylene oxide N-methylpyrrolidone solution is 1:(10-12);

[0011] S3: subjecting the rubber abrasive to ultrasonic shearing, drying and refining to obtain a natural graphite negative electrode material.

[0012] The above technical solution uses microwaves of a certain power to treat natural graphite. During this process, the interlayer spacing of natural graphite is widened, holes are formed in some areas, and some disordered structures inside are eliminated. After microwave treatment, the specific surface area of ​​the inner and outer interfaces of natural graphite is increased, and the ion diffusion capacity is significantly improved. However, the problem is that during the formation of the SEI film, the expanded specific surface area requires more SEI films to cover, resulting in the loss of active lithium, and the first coulomb efficiency and cycle life of the product cannot be effectively guaranteed; the inventor uses the bonding effect of polyethylene oxide, and with the cooperation of the solvent, it diffuses and penetrates into the interlayer of natural graphite, fixes the physical structure of natural graphite after microwave treatment, and fills some holes, thereby regulating its specific surface area. At the same time, because polyethylene oxide can still exert relatively excellent lithium ion transmission capacity under the synergistic effect of the electrolyte, the rate performance of the product will not be significantly reduced due to the introduction of polyethylene oxide.

[0013] Furthermore, the natural graphite is natural spherical graphite, and the D50 of the natural spherical graphite is 8-15 μm and the OI value is 8-15.

[0014] By selecting natural spherical graphite and materials of corresponding size, if the particle size is too small, then during the above microwave treatment process, the particle's own structural stability will be lost. The smaller the particle size, the more unstable its own structure, so during high-rate charge and discharge, the structure is prone to collapse; if the particle size is too large, the resistance of polyethylene oxide to diffuse and penetrate into the particle will increase, resulting in a large difference in the ion diffusion capacity inside and outside the particle, and greater polarization. The powder OI value represents the orientation of the graphite sheet structure in the particle. Selecting raw materials within the above OI value range will not easily cause the material to collapse when the distance between layers is expanded during microwave treatment.

[0015] Furthermore, the step S1 further includes:

[0016] After mixing natural graphite and acid solution, heating and stirring to react, filtering, washing and drying, acid-treated natural graphite is obtained;

[0017] The obtained acid-treated natural graphite is dispersed in an emulsifier aqueous solution, dispersed uniformly by ultrasonication, centrifuged, and dried to a moisture content of 2% to 5% to obtain pretreated natural graphite;

[0018] The obtained pretreated natural graphite is then treated under microwave conditions with a power of 300-600 W for 2-4 hours to obtain microwave-treated natural graphite.

[0019] First, acid treatment is used to change the surface polarity of natural graphite, making it easily wetted. Then, under the action of emulsifier and the control of drying conditions, a small amount of moisture is retained inside the natural graphite. In the subsequent microwave treatment process, the high energy of microwaves causes the internal water molecules to vaporize rapidly, thereby effectively widening the interlayer spacing of the product. At the same time, during the gas diffusion process, holes are formed inside the product, increasing the lithium ion diffusion channel.

[0020] Further, the acid solution is selected from any one of concentrated sulfuric acid, concentrated nitric acid or hydrofluoric acid;

[0021] Wherein, the concentrated sulfuric acid is concentrated sulfuric acid with a mass fraction of 96% or more;

[0022] The concentrated nitric acid is concentrated nitric acid with a mass fraction of 55% or more;

[0023] The hydrofluoric acid has a mass fraction of more than 50%.

[0024] Further, the heating and stirring reaction comprises:

[0025] The mixture was stirred at 95-100°C and 600-800 r / min for 3-5 h.

[0026] Furthermore, the emulsifier is selected from any one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, span-60, span-80, and emulsifier OP-10.

[0027] Another object of the present invention is to provide a high-rate graphite negative electrode material.

[0028] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0029] A high-rate graphite negative electrode material is prepared by the above-mentioned preparation process.

[0030] Another object of the present invention is to provide a negative electrode plate for a lithium ion battery.

[0031] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0032] A negative electrode plate for a lithium ion battery comprises a negative electrode current collector and a negative electrode active material coating adhered to at least one surface of the negative electrode current collector, wherein the negative electrode active material coating comprises the above-mentioned high-rate graphite negative electrode material, a binder and a conductive agent.

[0033] Another object of the present invention is to provide a lithium ion battery.

[0034] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0035] A lithium-ion battery comprises the above-mentioned negative electrode plate.

[0036] Beneficial effects:

[0037] (1) The present invention uses microwaves of a certain power to treat natural graphite. During this process, the interlayer spacing of natural graphite is widened, pores are formed in some areas, and some disordered structures inside the natural graphite are eliminated. After microwave treatment, the specific surface area of ​​the internal and external interfaces of natural graphite is increased, and the ion diffusion capacity is significantly improved. However, the problem is that in the process of SEI film formation, the enlarged specific surface area requires more SEI film to cover, which leads to the loss of active lithium, and the first coulomb efficiency and cycle life of the product cannot be effectively guaranteed. The inventors use the bonding effect of polyethylene oxide, and with the cooperation of solvent, make it diffuse and penetrate into the interlayer of natural graphite, fix the physical structure of natural graphite after microwave treatment, and fill some pores, thereby regulating its specific surface area. At the same time, because polyethylene oxide can still exert relatively excellent lithium ion transmission capacity under the synergistic effect of electrolyte, the rate performance of the product will not be significantly reduced due to the introduction of polyethylene oxide.

[0038] (2) Secondly, by selecting natural spherical graphite and materials of corresponding size, if the particle size is too small, then during the above microwave treatment, the particle's own structural stability will be lost. The smaller the particle size, the more unstable its own structure, so during high-rate charge and discharge, the structure is prone to collapse; if the particle size is too large, the resistance of polyethylene oxide to diffuse and penetrate into the particle will increase, resulting in a large difference in the ion diffusion capacity inside and outside the particle and greater polarization. The powder OI value represents the orientation of the graphite sheet structure in the particle. Selecting raw materials within the above OI value range will not easily cause the material to collapse when the distance between layers is expanded during microwave treatment. DETAILED DESCRIPTION

[0039] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0040] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0041] Example 1

[0042] The natural graphite and the acid solution were mixed in a mass ratio of 1:5 and poured into a stainless steel reactor lined with polytetrafluoroethylene. The mixture was stirred at 95°C and a stirring speed of 600 r / min for 3 hours. The mixture was naturally cooled to room temperature, discharged, filtered, and the filter cake was collected. The filter cake was washed with deionized water until the washing liquid was neutral, thereby obtaining acid-treated natural graphite.

[0043] The natural graphite is selected from natural spherical graphite, and the D50 of the natural spherical graphite is 8 μm and the OI value is 8;

[0044] The acid solution is selected from concentrated sulfuric acid;

[0045] The concentrated sulfuric acid is 96.5% by mass;

[0046] The acid-treated natural graphite and the aqueous solution of the emulsifier were mixed in a mass ratio of 1:8 and poured into a reactor. The mixture was ultrasonically dispersed for 45 minutes at an ultrasonic frequency of 80 kHz, and then centrifuged to obtain a filter cake. The filter cake was transferred to an oven and dried at a temperature of 85°C to a moisture content of 2%, thereby obtaining pretreated natural graphite.

[0047] Wherein, the mass fraction of the aqueous solution of the emulsifier is 3%; the emulsifier is selected from sodium dodecylbenzene sulfonate;

[0048] In the above drying process, the controlled moisture content is actually the moisture content at the corresponding drying temperature; for example, when the above drying temperature is selected as 85°C, the moisture content at this time is that the product is completely dried at 85°C until constant weight, which is used as the basis for calculation;

[0049] The obtained pretreated natural graphite was subjected to microwave treatment for 2 h in a nitrogen atmosphere at a microwave power of 300 W, and then naturally cooled to room temperature and discharged to obtain microwave-treated natural graphite;

[0050] The microwave-treated natural graphite and the N-methylpyrrolidone solution of polyethylene oxide are stirred and mixed for 60 minutes at a rotation speed of 300 r / min to obtain a mixture; then the mixture is subjected to a rubber grinding treatment for 12 minutes to obtain a rubber abrasive;

[0051] Wherein, the mass fraction of polyethylene oxide in the polyethylene oxide N-methylpyrrolidone solution is 15%; and the mass ratio of the microwave-treated natural graphite to the polyethylene oxide N-methylpyrrolidone solution is 1:10;

[0052] The obtained rubber abrasive was transferred to a shearing machine, and sheared for 1 hour at a rotation speed of 2500 r / min, then the shearing was stopped, and ultrasonic treatment was performed for 10 hours at an ultrasonic frequency of 100 kHz, and then sheared for 1 hour at a rotation speed of 2500 r / min, filtered, and the filter cake was collected. The obtained filter cake was transferred to an oven, dried to constant weight at a temperature of 100° C., and finally ground and refined to obtain a natural graphite negative electrode material;

[0053] Preparation of negative electrode sheet:

[0054] The natural graphite negative electrode material, the conductive agent and the binder are mixed in a mass ratio of 96:2.5:1.5 to prepare a negative electrode slurry, wherein the binder is first mixed and dissolved with a solvent to obtain a glue solution, which is then mixed evenly with the natural graphite negative electrode material and the conductive agent, and then extruded and coated on the surface of the negative electrode current collector by a coating machine, and after drying, rolled to a compaction density of 1.65 g / cm 3 , so as to form a negative electrode active material coating on the surface of the negative electrode current collector, and then slitting, die-cutting, and winding to obtain a negative electrode sheet;

[0055] The conductive agent is super P, the binder is CMC, and the negative electrode current collector is a copper foil with a thickness of 6 μm;

[0056] Preparation of positive electrode:

[0057] Lithium iron phosphate was selected as the positive electrode material. The mass ratio of the positive electrode material, the conductive agent and the binder was 97:2:1. The binder was first mixed and dissolved with the solvent to obtain a glue solution, which was then mixed evenly with the positive electrode material and the conductive agent, and then extruded and coated on the surface of the positive electrode current collector to form a positive electrode active material coating. After drying, it was rolled to a compaction density of 3.6 g / cm 3 , slitting, die-cutting, and winding to obtain the positive electrode sheet;

[0058] Among them, the conductive agent is selected with a mass ratio of acetylene black and CNT of 4:1, the binder is selected with PVDF, and the positive electrode current collector is selected with a thickness of 12 μm.

[0059] The diaphragm is selected with a base film of 7μm PP and a 2μm single-sided ceramic diaphragm;

[0060] The electrolyte solution is prepared by mixing ethylene carbonate and ethyl methyl carbonate in a mass ratio of 2:3 to form a solvent, and lithium hexafluorophosphate is used as a lithium salt and added into the solvent to form an electrolyte solution with a concentration of 1 mol / L;

[0061] After assembling the positive electrode plate, negative electrode plate and separator to form a single battery, inject the electrolyte with an injection coefficient of 1.4; after the injection is completed, stand it at a temperature of 45°C for 8 hours to obtain a lithium battery product.

[0062] Example 2

[0063] The natural graphite and the acid solution were mixed in a mass ratio of 1:6 and poured into a stainless steel reactor lined with polytetrafluoroethylene. The mixture was stirred at 98°C and a stirring speed of 700 r / min for 4 hours. The mixture was naturally cooled to room temperature, discharged, filtered, and the filter cake was collected. The filter cake was washed with deionized water until the washing liquid was neutral, thereby obtaining acid-treated natural graphite.

[0064] The natural graphite is natural spherical graphite, and the D50 of the natural spherical graphite is 12 μm and the OI value is 10;

[0065] The acid solution is selected from concentrated nitric acid;

[0066] The concentrated nitric acid is 56% by mass.

[0067] The acid-treated natural graphite and the aqueous solution of the emulsifier were mixed in a mass ratio of 1:9 and poured into a reactor. The mixture was ultrasonically dispersed for 55 minutes at an ultrasonic frequency of 90 kHz, and then centrifuged to obtain a filter cake. The filter cake was transferred to an oven and dried at a temperature of 88°C to a moisture content of 3%, thereby obtaining pretreated natural graphite.

[0068] Wherein, the mass fraction of the aqueous solution of the emulsifier is 4.5%; the emulsifier is selected from hexadecyltrimethylammonium bromide;

[0069] In the above drying process, the controlled moisture content is actually the moisture content at the corresponding drying temperature; for example, when the above drying temperature is selected as 88°C, the moisture content at this time is that the product is completely dried at 88°C until constant weight, which is used as the basis for calculation;

[0070] The obtained pretreated natural graphite was subjected to microwave treatment for 3 h in a nitrogen atmosphere at a microwave power of 500 W, and then naturally cooled to room temperature and discharged to obtain microwave-treated natural graphite;

[0071] The microwave-treated natural graphite and the N-methylpyrrolidone solution of polyethylene oxide are stirred and mixed for 70 minutes at a rotation speed of 400 r / min to obtain a mixture; then the mixture is subjected to a rubber grinding treatment for 15 minutes to obtain a rubber abrasive;

[0072] Wherein, the mass fraction of polyethylene oxide in the polyethylene oxide N-methylpyrrolidone solution is 18%; and the mass ratio of the microwave-treated natural graphite to the polyethylene oxide N-methylpyrrolidone solution is 1:11;

[0073] The obtained rubber abrasive was transferred to a shearing machine, and sheared for 1 hour at a rotation speed of 2800 r / min, then the shearing was stopped, and ultrasonic treatment was performed for 10 hours at an ultrasonic frequency of 110 kHz, and then sheared for 1 hour at a rotation speed of 2800 r / min, filtered, and the filter cake was collected. The obtained filter cake was transferred to an oven, dried to constant weight at a temperature of 100° C., and finally ground and refined to obtain a natural graphite negative electrode material;

[0074] Preparation of negative electrode sheet:

[0075] The natural graphite negative electrode material, the conductive agent and the binder are mixed in a mass ratio of 96:2.5:1.5 to prepare a negative electrode slurry, wherein the binder is first mixed and dissolved with a solvent to obtain a glue solution, which is then mixed evenly with the natural graphite negative electrode material and the conductive agent, and then extruded and coated on the surface of the negative electrode current collector by a coating machine, and after drying, rolled to a compaction density of 1.65 g / cm 3 , so as to form a negative electrode active material coating on the surface of the negative electrode current collector, and then slitting, die-cutting, and winding to obtain a negative electrode sheet;

[0076] The conductive agent is super P, the binder is CMC, and the negative electrode current collector is a copper foil with a thickness of 6 μm;

[0077] Preparation of positive electrode:

[0078] Lithium iron phosphate was selected as the positive electrode material. The mass ratio of the positive electrode material, the conductive agent and the binder was 97:2:1. The binder was first mixed and dissolved with the solvent to obtain a glue solution, which was then mixed evenly with the positive electrode material and the conductive agent, and then extruded and coated on the surface of the positive electrode current collector to form a positive electrode active material coating. After drying, it was rolled to a compaction density of 3.6 g / cm 3 , slitting, die-cutting, and winding to obtain the positive electrode sheet;

[0079] Among them, the conductive agent is selected with a mass ratio of acetylene black and CNT of 4:1, the binder is selected with PVDF, and the positive electrode current collector is selected with a thickness of 12 μm.

[0080] The diaphragm is selected with a base film of 7μm PP and a 2μm single-sided ceramic diaphragm;

[0081] The electrolyte solution is prepared by mixing ethylene carbonate and ethyl methyl carbonate in a mass ratio of 2:3 to form a solvent, and lithium hexafluorophosphate is used as a lithium salt and added into the solvent to form an electrolyte solution with a concentration of 1 mol / L;

[0082] After assembling the positive electrode plate, negative electrode plate and separator to form a single battery, inject the electrolyte with an injection coefficient of 1.4; after the injection is completed, stand it at a temperature of 45°C for 8 hours to obtain a lithium battery product.

[0083] Example 3

[0084] The natural graphite and the acid solution were mixed in a mass ratio of 1:8 and poured into a stainless steel reactor lined with polytetrafluoroethylene. The mixture was stirred at 100°C and a stirring speed of 800 r / min for 5 hours. The mixture was naturally cooled to room temperature, discharged, filtered, and the filter cake was collected. The filter cake was washed with deionized water until the washing liquid was neutral, thereby obtaining acid-treated natural graphite.

[0085] The natural graphite is natural spherical graphite, and the D50 of the natural spherical graphite is 15 μm and the OI value is 15;

[0086] The acid solution is selected from hydrofluoric acid;

[0087] The hydrofluoric acid is hydrofluoric acid with a mass fraction of 52%;

[0088] The acid-treated natural graphite and the aqueous solution of the emulsifier were mixed in a mass ratio of 1:10 and poured into a reactor. The mixture was ultrasonically dispersed for 60 minutes at an ultrasonic frequency of 100 kHz, and then centrifuged to obtain a filter cake. The filter cake was transferred to an oven and dried at a temperature of 90°C to a moisture content of 5%, thereby obtaining pretreated natural graphite.

[0089] Wherein, the mass fraction of the aqueous solution of the emulsifier is 5%; the emulsifier is selected from span-60;

[0090] In the above drying process, the controlled moisture content is actually the moisture content at the corresponding drying temperature; for example, if the drying temperature is selected as 90°C, the moisture content at this time is that the product is completely dried at 90°C until constant weight, which is used as the basis for calculation;

[0091] The obtained pretreated natural graphite was subjected to microwave treatment for 4 h in a nitrogen atmosphere at a microwave power of 600 W, and then naturally cooled to room temperature and discharged to obtain microwave-treated natural graphite;

[0092] The microwave-treated natural graphite and the N-methylpyrrolidone solution of polyethylene oxide are stirred and mixed for 80 minutes at a rotation speed of 500 r / min to obtain a mixture; then the mixture is subjected to a rubber grinding treatment for 16 minutes to obtain a rubber abrasive;

[0093] Wherein, the mass fraction of polyethylene oxide in the polyethylene oxide N-methylpyrrolidone solution is 20%; and the mass ratio of the microwave-treated natural graphite to the polyethylene oxide N-methylpyrrolidone solution is 1:12;

[0094] The obtained rubber abrasive was transferred to a shearing machine, and sheared for 1 hour at a rotation speed of 3000 r / min, then the shearing was stopped, and ultrasonic treatment was performed for 10 hours at an ultrasonic frequency of 120 kHz, and then sheared for 1 hour at a rotation speed of 3000 r / min, filtered, and the filter cake was collected. The obtained filter cake was transferred to an oven, dried to constant weight at a temperature of 105° C., and finally ground and refined to obtain a natural graphite negative electrode material;

[0095] Preparation of negative electrode sheet:

[0096] The natural graphite negative electrode material, the conductive agent and the binder are mixed in a mass ratio of 96:2.5:1.5 to prepare a negative electrode slurry, wherein the binder is first mixed and dissolved with a solvent to obtain a glue solution, which is then mixed evenly with the natural graphite negative electrode material and the conductive agent, and then extruded and coated on the surface of the negative electrode current collector by a coating machine, and after drying, rolled to a compaction density of 1.65 g / cm 3 , so as to form a negative electrode active material coating on the surface of the negative electrode current collector, and then slitting, die-cutting, and winding to obtain a negative electrode sheet;

[0097] The conductive agent is super P, the binder is CMC, and the negative electrode current collector is a copper foil with a thickness of 6 μm;

[0098] Preparation of positive electrode:

[0099] Lithium iron phosphate was selected as the positive electrode material. The mass ratio of the positive electrode material, the conductive agent and the binder was 97:2:1. The binder was first mixed and dissolved with the solvent to obtain a glue solution, which was then mixed evenly with the positive electrode material and the conductive agent, and then extruded and coated on the surface of the positive electrode current collector to form a positive electrode active material coating. After drying, it was rolled to a compaction density of 3.6 g / cm 3 , slitting, die-cutting, and winding to obtain the positive electrode sheet;

[0100] Among them, the conductive agent is selected with a mass ratio of acetylene black and CNT of 4:1, the binder is selected with PVDF, and the positive electrode current collector is selected with a thickness of 12 μm.

[0101] The diaphragm is selected with a base film of 7μm PP and a 2μm single-sided ceramic diaphragm;

[0102] The electrolyte solution is prepared by mixing ethylene carbonate and ethyl methyl carbonate in a mass ratio of 2:3 to form a solvent, and lithium hexafluorophosphate is used as a lithium salt and added into the solvent to form an electrolyte solution with a concentration of 1 mol / L;

[0103] After assembling the positive electrode plate, negative electrode plate and separator to form a single battery, inject the electrolyte with an injection coefficient of 1.4; after the injection is completed, stand it at a temperature of 45°C for 8 hours to obtain a lithium battery product.

[0104] Example 4

[0105] The difference between this embodiment and embodiment 1 is that the D50 of the natural graphite is 3.5 μm, and the other conditions remain unchanged.

[0106] Example 5

[0107] The difference between this embodiment and embodiment 1 is that the D50 of the natural graphite is 25 μm, and the other conditions remain unchanged.

[0108] Example 6

[0109] Compared with Example 1, the present embodiment differs in that the OI value of the natural graphite is 4, and the other conditions remain unchanged.

[0110] Example 7

[0111] Compared with Example 1, this embodiment is different in that the OI value of the natural graphite is 22, and the other conditions remain unchanged.

[0112] Example 8

[0113] The present embodiment differs from the embodiment 1 in that the acid solution is replaced by deionized water of equal mass, and the other conditions remain unchanged.

[0114] Example 9

[0115] The present embodiment is different from the embodiment 1 in that the emulsifier aqueous solution is replaced by deionized water of equal mass, and the other conditions remain unchanged.

[0116] Comparative Example 1

[0117] The difference between this comparative example and Example 1 is that an equal amount of N-methylpyrrolidone is used to replace the N-methylpyrrolidone solution of polyethylene oxide, and the other conditions remain unchanged.

[0118] The performance of the lithium battery products obtained in Examples 1-9 and Comparative Example 1 was tested. The specific test methods and test results are as follows:

[0119] Rate performance test:

[0120] At 25°C, the battery capacity was calibrated, and then at 25°C, the battery was charged at a rate of 2.5C and discharged at a rate of 1C, and a full charge and discharge cycle test was performed until the battery capacity decayed to 80% of the initial capacity. The charge and discharge were stopped, and the cycle number was recorded. The specific test results are shown in Table 1.

[0121] Among them, during the full charge process, first charge at a constant current rate of 2.5C. After reaching the cut-off voltage (3.75V), continue to charge at a constant voltage until the current is lower than 0.025C, then stop charging and it is considered fully charged; during the full discharge process, discharge at a discharge rate of 1C until the cut-off voltage is 2.7V, and then let it stand for 30 minutes;

[0122] At 25°C, the battery capacity was calibrated, and then at 25°C, the battery was charged at a rate of 3.0C and discharged at a rate of 1C, and a full charge and discharge cycle test was performed until the battery capacity decayed to 80% of the initial capacity. The charge and discharge were stopped, and the number of cycles was recorded. The specific test results are shown in Table 1.

[0123] Among them, during the full charge process, first charge at a constant current rate of 3.0C. After reaching the cut-off voltage (3.75V), continue to charge at a constant voltage until the current is lower than 0.025C, then stop charging and it is considered fully charged; during the full discharge process, discharge at a discharge rate of 1C until the cut-off voltage is 2.7V, and then let it stand for 30 minutes;

[0124] Table 1: Product performance test results

[0125]

[0126] It can be seen from the test results in Table 1 that the product obtained by the present invention can still maintain relatively excellent cycle performance under high rate charge and discharge conditions.

[0127] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A preparation process of high-rate graphite negative electrode material, It is characterized in that The specific preparation process includes the following steps: S1: mixing natural graphite and an acid solution, heating and stirring to react, and then filtering, washing and drying to obtain acid-treated natural graphite; The obtained acid-treated natural graphite is dispersed in an emulsifier aqueous solution, dispersed uniformly by ultrasonication, centrifuged, and dried to a moisture content of 2% to 5% to obtain pretreated natural graphite; The obtained pretreated natural graphite is then treated under microwave conditions with a power of 300-600 W for 2-4 hours to obtain microwave-treated natural graphite; S2: stirring and mixing the microwave-treated natural graphite and the N-methylpyrrolidone solution of polyethylene oxide to obtain a mixture; then subjecting the mixture to a rubber grinding treatment for more than 10 minutes to obtain a rubber abrasive; Wherein, in the polyethylene oxide N-methylpyrrolidone solution, the mass fraction of polyethylene oxide is 15%-20%; and the mass ratio of the microwave-treated natural graphite to the polyethylene oxide N-methylpyrrolidone solution is 1:(10-12); S3: subjecting the rubber abrasive to ultrasonic shearing, drying, and refining to obtain a natural graphite negative electrode material; The natural graphite is natural spherical graphite, and the D50 of the natural spherical graphite is 8-15 μm and the OI value is 8-15; The acid solution is selected from any one of concentrated sulfuric acid, concentrated nitric acid or hydrofluoric acid; Wherein, the concentrated sulfuric acid is concentrated sulfuric acid with a mass fraction of 96% or more; The concentrated nitric acid is concentrated nitric acid with a mass fraction of 55% or more; The hydrofluoric acid has a mass fraction of more than 50%.

2. A process for preparing a high-rate graphite negative electrode material according to claim 1, It is characterized in that The heating and stirring reaction comprises: The reaction was carried out under the conditions of 95-100°C and 600-800 r / min of stirring, and the mixture was stirred and reacted for 3-5 hours.

3. A process for preparing a high-rate graphite negative electrode material according to claim 1, It is characterized in that The emulsifier is selected from any one of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, span-60, span-80, and emulsifier OP-10.

4. A high-rate graphite negative electrode material, It is characterized in that The method is prepared by the preparation process described in any one of claims 1 to 3.

5. A negative electrode sheet for a lithium-ion battery, It is characterized in that It comprises a negative electrode current collector and a negative electrode active material coating adhered to at least one surface of the negative electrode current collector, wherein the negative electrode active material coating comprises the high-rate graphite negative electrode material according to claim 4, a binder and a conductive agent.

6. A lithium ion battery, It is characterized in that Including the negative electrode sheet as described in claim 5.

Citation Information

Patent Citations

  • Lithium ion battery with high capacity and high circulation frequency

    CN107910519A

  • All-solid secondary battery, particles for all-solid secondary batteries, solid electrolyte composition for all-solid secondary batteries, electrode sheet for all-solid secondary batteries, and production methods therefor

    CN108370062A

  • Preparation process of composite material of artificial graphite and carbon-coated natural graphite

    CN117800335A

  • Lithium ion battery graphite negative electrode material and preparation method thereof

    US20140302394A1

  • Artificial graphite negative electrode material for high-rate lithium ion battery and preparation method therefor

    WO2022121136A1