Preparation method of carbon-based composite negative electrode material of sodium-ion battery

By using covalent bonding method of nanosilicon dioxide and hydroxy Zn-MOF in sodium ion batteries, a carbon-based composite negative electrode material with uniform pore structure was prepared, which solved the problem of uneven pores of hard carbon materials and improved sodium ions adsorption and diffusion capabilities and electrochemical properties of the battery.

CN119092664APending Publication Date: 2024-12-06YANCHENG TEACHERS UNIV

Patent Information

Application Number
CN202411121755.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The pore formation of hard carbon materials in sodium ion batteries is uneven, resulting in poor adsorption and diffusion capabilities of sodium ion and making it difficult to commercialize.

Method used

Carbon-based composite negative electrode material is prepared by dissolving nanosilica polymer and hydroxy Zn-MOF in N,N-dimethylformamide, and covalently combining hydroxy Zn-MOF with nanosilica to form a uniform The porous structure improves the adsorption and diffusion ability of sodium ions.

Benefits of technology

The prepared carbon-based composite negative electrode material has uniform pore distribution, which improves the adsorption and diffusion capacity of sodium ions, improves the storage capacity and Coulomb efficiency of the battery, and enhances the electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995297200000081
    Figure BDA0004995297200000081
Patent Text Reader

Abstract

The invention discloses a preparation method of a sodium-ion battery carbon-based composite negative electrode material, and belongs to the technical field of sodium-ion battery materials, and the preparation method comprises the following steps: step 1, heating a nano silicon dioxide polymer and hydroxyl Zn-MOF in N, N-dimethylformamide in a reaction kettle to prepare a nano silicon dioxide / Zn-MOF polymer; and 2, carrying out high-temperature carbonization on the nano silicon dioxide / Zn-MOF polymer in a tubular furnace under the protection of nitrogen to obtain the carbon-based composite negative electrode material. The carbon-based composite negative electrode material of the sodium-ion battery prepared by the preparation method disclosed by the invention is prepared by carrying out composite high-temperature carbonization on the polyacrylonitrile copolymer and the nano silicon dioxide, and the nano silicon dioxide is uniformly dispersed on the surface of polyacrylonitrile, so that a hard carbon composite material generated by the polyacrylonitrile copolymer is uniform in pore distribution; and the adsorption and diffusion capabilities of the carbon-based composite negative electrode material formed by the hard carbon material on sodium ions are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion battery materials, and in particular relates to a method for preparing a carbon-based composite negative electrode material for a sodium ion battery. Background Art

[0002] Sodium-ion batteries and lithium-ion batteries have similar energy storage mechanisms. Lithium-ion batteries currently have outstanding advantages in the field of energy storage, but the lack of lithium resources, uneven distribution and high costs limit their large-scale application. Sodium ions are abundant in the earth's crust and seawater and are easy to obtain. Therefore, sodium-ion batteries are considered to be one of the most promising alternatives to lithium-ion batteries.

[0003] Sodium ions have heavier atomic mass and larger ionic radius, which results in the energy density of sodium ion batteries being lower than that of lithium ion batteries. The negative electrode material is an important component of sodium ion batteries. Since the capacity of the negative electrode materials of traditional sodium ion batteries is limited, finding suitable negative electrode materials for sodium ion batteries has always been the focus of sodium ion battery research.

[0004] Patent CN106935856A discloses a carbon-based composite negative electrode material for a sodium ion battery and a preparation method thereof. Hard carbon balls are obtained by a hydrothermal method, and an iron source and a carbon source are attached or coated on the surface of the hard carbon balls by a liquid phase method, and then carbonized to obtain a carbon-based composite negative electrode material. However, the hard carbon material with abundant nanopores has a large specific surface area and a low Coulomb efficiency in the first cycle, making it difficult to commercialize.

[0005] Patent CN118039884A discloses a sodium ion battery bamboo charcoal composite negative electrode and a preparation method thereof, wherein the bamboo charcoal material is activated and then hydroxylated, nano-silicate particles are grafted onto the surface of the bamboo charcoal material, and a dense and uniform carbon coating layer is formed on the surface of the prepared sodium ion battery bamboo charcoal composite negative electrode material after carbonization, thereby obtaining a sodium ion battery negative electrode material with rich pore structure and high stability; however, in this scheme, the nano-silicate plays a connecting role with the bamboo charcoal material and the hydroxylated modified polyacrylic acid at the same time, and is greatly affected by the content and dispersibility of the nano-silicate. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a carbon-based composite negative electrode material for a sodium ion battery, so as to solve the problem of uneven pore formation and poor adsorption and diffusion capacity of sodium ions when hard carbon materials are used as sodium ion battery materials.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for preparing a carbon-based composite negative electrode material for a sodium ion battery comprises the following steps:

[0009] Step 1: dissolving the nano-silica polymer in N,N-dimethylformamide in a reaction kettle, dispersing the hydroxy Zn-MOF in N,N-dimethylformamide and adding the mixture into the reaction kettle, heating to 40-50° C., stirring and reacting for 1-1.5 hours, removing the solvent by rotary evaporation, and vacuum drying to obtain the nano-silica / Zn-MOF polymer;

[0010] Step 2: heating the nano-silica / Zn-MOF polymer to 1000-1200° C. in a tube furnace under nitrogen protection for 2-3 hours at a heating rate of 5° C. / min to obtain a carbon-based composite negative electrode material;

[0011] Nano-silicon dioxide polymer is prepared by the following steps:

[0012] In a reaction kettle, polyacrylonitrile and polymethyl methacrylate are dissolved in N-methylpyrrolidone, stirred and reacted at 70-80°C for 4-6 hours, polymethacrylate N,N-dimethylaminoethyl ester is added to the reaction kettle, stirred and reacted for 40-60 minutes, 1,2-bis(2-iodoethoxy)ethane is added, and the polymer template is obtained after standing for 48-72 hours, tetramethoxysilane and anhydrous ethanol are stirred and mixed, and then added to the reaction kettle, ammonia water is added to the reaction kettle, and stirred and reacted for 4-6 hours, the solvent is removed by rotary evaporation, and the insoluble matter is collected, and the insoluble matter is dried in a vacuum to obtain a nano-silica polymer.

[0013] Further, the hydroxy Zn-MOF is prepared by the following steps:

[0014] In a reaction kettle, pamoic acid and 2,5-dihydroxyterephthalic acid were dissolved in N,N-dimethylformamide, and Zn(ClO 4 ) 2 6H 2 O is dissolved in methanol solution and added into the reaction kettle for mixing, and the mixture is sealed and heated to 75-85°C for reaction for 24-36h. After cooling, the mixture is washed with methanol and vacuum dried to obtain hydroxy Zn-MOF.

[0015] Furthermore, the ratio of pamoic acid, 2,5-dihydroxyterephthalic acid and N,N-dimethylformamide is 4-5 g: 2-3 g: 200-250 mL; Zn(C l O 4 ) 2 6H 2 The dosage ratio of O and methanol is: 4-5g:100-125mL.

[0016] Furthermore, in step 1, the ratio of the amount of nano-silica polymer to N,N-dimethylformamide is 10-15 g: 20-30 mL; the ratio of the amount of hydroxy Zn-MOF to N,N-dimethylformamide is 2-3 g: 10-15 mL.

[0017] Furthermore, the usage ratio of polyacrylonitrile, polymethyl methacrylate, N-methylpyrrolidone, poly(N,N-dimethylaminoethyl methacrylate) and 1,2-bis(2-iodoethoxy)ethane is 10-15g:3-5g:80-85g:10-15g:3-4g.

[0018] Furthermore, the usage ratio of tetramethoxysilane, anhydrous ethanol and ammonia water is 3-5 mL: 45-50 mL: 15-20 mL.

[0019] Furthermore, the mass fraction of the ammonia water is 1.5-2%.

[0020] Beneficial effects of the present invention:

[0021] (1) The carbon-based composite negative electrode material for sodium ion batteries prepared by the preparation method of the present invention is prepared by high-temperature carbonization of a polyacrylonitrile copolymer and nano-silicon dioxide. The nano-silicon dioxide is evenly dispersed on the surface of the polyacrylonitrile so that the pore distribution of the hard carbon composite material generated by the polyacrylonitrile copolymer is uniform, thereby enhancing the adsorption and diffusion capacity of the carbon-based composite negative electrode material formed by the hard carbon material for sodium ions.

[0022] (2) The present invention covalently bonds hydroxy Zn-MOF with nano-silica, so that the hydroxy Zn-MOF becomes vitrified and adheres to the surface of the nano-silica when polyacrylonitrile is carbonized. The vitrified hydroxy Zn-MOF can improve the ion transport performance of the carbon-based composite negative electrode material. The ligand of the hydroxy Zn-MOF is also carbonized to form a porous carbon layer attached to the surface of the nano-silica, thereby improving the porous surface area of ​​the carbon-based composite negative electrode material.

[0023] (3) The present invention first grafts hydrophobic polyacrylonitrile and hydrophobic polymethyl methacrylate, and then crosslinks with hydrophilic polymethacrylate N,N-dimethylaminoethyl to form a polymer template, and then deposits nano-silica on the polymer template by a solvent-gel method under the catalytic action of tetramethoxysilane and ammonia water, so that the nano-silica is uniformly deposited on the polymer template, thereby obtaining a carbon-based composite negative electrode material uniformly loaded with nano-silica during high-temperature carbonization, so that the carbon-based composite negative electrode material has uniform pores, and the adsorption and diffusion capacity of the carbon-based composite negative electrode material for sodium ions is improved. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1: A method for preparing a carbon-based composite negative electrode material for a sodium ion battery, comprising the following steps:

[0026] Step 1: Dissolve 4 g of pamoic acid and 2 g of 2,5-dihydroxyterephthalic acid in 200 mL of N,N-dimethylformamide in a polytetrafluoroethylene-lined reactor, and add 4 g of Zn(ClO 4 ) 2 6H 2 O was dissolved in 100 mL of methanol solution and added into the reaction kettle for mixing. The mixture was sealed and heated to 75 °C for reaction for 24 h. After cooling, the mixture was washed twice with methanol and dried under vacuum at 80 °C for 12 h to obtain hydroxy Zn-MOF.

[0027] Step 2: Dissolve 10 g of polyacrylonitrile and 3 g of polymethyl methacrylate in 80 g of N-methylpyrrolidone in a reactor, stir and react at 70° C. for 4 h, then add 10 g of polymethacrylate N,N-dimethylaminoethyl to the reactor, stir and react for 40 min, add 3 g of 1,2-bis(2-iodoethoxy)ethane, and place for 48 h to obtain a polymer template, stir and mix 3 mL of tetramethoxysilane and 45 mL of anhydrous ethanol and add to the reactor, add 15 mL of 1.5 wt% ammonia water to the reactor and stir and react for 4 h, remove the solvent by rotary evaporation, collect insoluble matter, and dry the insoluble matter in vacuo at 50° C. for 18 h to obtain a nano-silica polymer.

[0028] Step 3: Dissolve 10 g of nano-silica polymer in 20 mL of N,N-dimethylformamide in a reactor, disperse 2 g of hydroxy Zn-MOF in 10 mL of N,N-dimethylformamide and add to the reactor, heat to 40 °C and stir to react for 1 h, remove the solvent by rotary evaporation, and vacuum dry at 50 °C for 18 h to obtain nano-silica / Zn-MOF polymer.

[0029] Step 4: Heat the nano-silica / Zn-MOF polymer to 1000° C. in a tubular furnace under nitrogen protection for 2 h at a heating rate of 5° C. / min to obtain a carbon-based composite negative electrode material.

[0030] Example 2: A method for preparing a carbon-based composite negative electrode material for a sodium ion battery, comprising the following steps:

[0031] Step 1: Dissolve 4.5 g of pamoic acid and 2.5 g of 2,5-dihydroxyterephthalic acid in 225 mL of N,N-dimethylformamide in a polytetrafluoroethylene-lined reactor, and add 4.5 g of Zn(ClO 4 ) 2 6H 2O was dissolved in 115 mL of methanol solution and added into the reactor for mixing. The mixture was sealed and heated to 80 °C for reaction for 30 h. After cooling, it was washed twice with methanol and dried in vacuum at 90 °C for 16 h to obtain hydroxy Zn-MOF.

[0032] Step 2: Dissolve 12.5 g of polyacrylonitrile and 4 g of polymethyl methacrylate in 82.5 g of N-methylpyrrolidone in a reactor, stir and react at 75° C. for 5 h, then add 12.5 g of N,N-dimethylaminoethyl polymethacrylate to the reactor, stir and react for 50 min, add 3.5 g of 1,2-bis(2-iodoethoxy)ethane, and place for 54 h to obtain a polymer template, stir and mix 4 mL of tetramethoxysilane and 47.5 mL of anhydrous ethanol and add them to the reactor, add 17.5 mL of 1.75 wt% ammonia water to the reactor and stir and react for 5 h, remove the solvent by rotary evaporation, collect the insoluble matter, and dry the insoluble matter in vacuo at 55° C. for 21 h to obtain a nano-silica polymer.

[0033] Step 3: Dissolve 12.5 g of nano-silica polymer in 25 mL of N,N-dimethylformamide in a reactor, disperse 2.5 g of hydroxy Zn-MOF in 12.5 mL of N,N-dimethylformamide and add the mixture to the reactor. Heat to 45 °C and stir to react for 1.25 h. Rotary evaporate to remove the solvent, and vacuum dry at 55 °C for 21 h to obtain nano-silica / Zn-MOF polymer.

[0034] Step 4: Heat the nano-silica / Zn-MOF polymer to 1100° C. in a tubular furnace under nitrogen protection and react for 2.5 hours at a heating rate of 5° C. / min to obtain a carbon-based composite negative electrode material.

[0035] Example 3: A method for preparing a carbon-based composite negative electrode material for a sodium ion battery, comprising the following steps:

[0036] Step 1: Dissolve 5 g of pamoic acid and 3 g of 2,5-dihydroxyterephthalic acid in 250 mL of N,N-dimethylformamide in a polytetrafluoroethylene-lined reactor, and add 5 g of Zn(ClO 4 ) 2 6H 2 O was dissolved in 125 mL of methanol solution and added into the reaction kettle for mixing. The mixture was sealed and heated to 85 °C for reaction for 36 h. After cooling, the mixture was washed with methanol for 3 times and dried in vacuum at 100 °C for 24 h to obtain hydroxy Zn-MOF.

[0037] Step 2: Dissolve 15 g of polyacrylonitrile and 5 g of polymethyl methacrylate in 85 g of N-methylpyrrolidone in a reactor, stir and react at 80° C. for 6 h, then add 15 g of polymethacrylate N,N-dimethylaminoethyl to the reactor, stir and react for 60 min, add 4 g of 1,2-bis(2-iodoethoxy)ethane, and place for 72 h to obtain a polymer template, stir and mix 5 mL of tetramethoxysilane and 50 mL of anhydrous ethanol and add to the reactor, add 20 mL of 2 wt% ammonia water to the reactor and stir and react for 6 h, remove the solvent by rotary evaporation, collect insoluble matter, and dry the insoluble matter in vacuo at 60° C. for 24 h to obtain a nano-silica polymer.

[0038] Step 3: Dissolve 15 g of nano-silica polymer in 30 mL of N,N-dimethylformamide in a reactor, disperse 3 g of hydroxy Zn-MOF in 15 mL of N,N-dimethylformamide and add to the reactor, heat to 50 °C and stir to react for 1.5 h, remove the solvent by rotary evaporation, and vacuum dry at 60 °C for 24 h to obtain nano-silica / Zn-MOF polymer.

[0039] Step 4: Heat the nano-silica / Zn-MOF polymer to 1200° C. in a tubular furnace under nitrogen protection for 3 hours at a heating rate of 5° C. / min to obtain a carbon-based composite negative electrode material.

[0040] Principle of the invention:

[0041] Hydroxy Zn-MOF is synthesized by using pamoic acid as a ligand, and the hydroxyl group of pamoic acid is used to hydroxylate Zn-MOF; polymethyl methacrylate is first grafted with polyacrylonitrile, and then cross-linked with polymethacrylate N,N-dimethylaminoethyl to form a hydrophilic-hydrophobic polymer template, and the polymer template is partially quaternized by adding a quaternizing agent 1,2-bis(2-iodoethoxy)ethane to form a more stable polymer template, and tetramethoxysilane is used to deposit more stable nano-silica on the polymer template by a solvent-gel method under the catalytic action of ammonia water, so that the nano-silica is uniformly deposited on the polymer template, and then the hydroxyl group in the hydroxyl Zn-MOF ligand and the hydroxyl group on the surface of the nano-silica are condensed to make the hydroxyl Zn-MOF covalently bonded to the nano-silica, and the hydroxyl Zn-MOF is dispersed on the polymer template with the nano-silica, and then the polymer template and the hydroxyl group are heated at high temperature. The ligands in Zn-MOF are carbonized, causing the polyacrylonitrile copolymer in the polymer template to carbonize to form a hard carbon composite material. During the heating process, the hydroxyl Zn-MOF will be vitrified, and the ligands in the hydroxyl Zn-MOF will first be carbonized to form a porous carbon layer coated on the surface of the nano-silica. The evenly distributed nano-silica makes the carbon material formed when the polyacrylonitrile copolymer is carbonized at a higher temperature have a more porous structure, and the pores are evenly distributed. The quaternary ammonium groups in the polymer template will also be doped into the carbon material to form nitrogen-doped porous carbon, thereby improving the stability and electron transport capacity of the carbon material. The carbon layer formed by the hydroxyl Zn-MOF ligands on the surface of the nano-silica also has a porous structure. The vitrified hydroxyl Zn-MOF also improves the ion transport performance of the carbon-based composite negative electrode material, enhances the adsorption and diffusion capacity of the carbon-based composite negative electrode material formed by the hard carbon material for sodium ions, and improves the storage capacity and coulomb efficiency of the carbon-based composite negative electrode material.

[0042] Comparative Example 1: The difference from Example 1 is that the nano-silicon dioxide polymer is prepared by the following steps:

[0043] In a reaction kettle, 10 g of polyacrylonitrile was dispersed in 80 g of N-methylpyrrolidone, 3 mL of tetramethoxysilane was mixed with 45 mL of anhydrous ethanol and added to the reaction kettle, 15 mL of 1.5 wt% ammonia water was added to the reaction kettle and stirred for 4 h, the solvent was removed by rotary evaporation and the insoluble matter was collected, and the insoluble matter was vacuum dried at 50° C. for 18 h to obtain a nano-silica polymer.

[0044] Comparative Example 2: The difference from Example 1 is that the carbon-based composite negative electrode material is prepared by the following steps: the nano-silicon dioxide polymer is heated to 1000°C in a tubular furnace under nitrogen protection for 2 hours, and the heating rate is 5°C / min to obtain a carbon-based composite negative electrode material.

[0045] Comparative Example 3: The difference from Example 1 is that 1,2-bis(2-iodoethoxy)ethane is not added in step 2.

[0046] The sources of some reagents in the embodiments and comparative examples are as follows:

[0047] 1,2-Bis(2-iodoethoxy)ethane and tetramethoxysilane were purchased from MacLean Reagent Co., Ltd.

[0048] Poly(N,N-dimethylaminoethyl methacrylate) was purchased from Hangzhou Xinqiao Biotechnology Co., Ltd.

[0049] Ammonia, polyethylene glycol, polyacrylonitrile, pamoic acid, dihydroxyterephthalic acid, polymethyl methacrylate, and N-methylpyrrolidone were purchased from Sigma-Aldrich.

[0050] The carbon-based composite negative electrode material obtained in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 and acetylene black, styrene butadiene latex, and carboxymethyl cellulose were mixed with deionized water in a ratio of 7:2:0.5:0.5, stirred to form a uniform slurry, and then coated on a copper foil current collector, dried in vacuum at 60°C overnight to remove the solvent, and then cut into 10 mm diameter circular pole pieces. The mass loading of the active material was 0.5-0.8 mg cm -2 , Whatman D (675 μm) glass fiber membrane was used as a separator, 200 μl of 1.0 M NaCF3SO3 in diglyme (100%) was used as an electrolyte solution, and sodium metal foil was used as a counter electrode. CR2032 button-type batteries were assembled in an argon-filled glove box and installed on a CT2001ALAND test system. The charge and discharge current density and battery voltage test range (0.01-3.0 V (vs. Na+ / Na)) were set to test its electrochemical performance. After the battery was assembled and aged for 12 h, a charge and discharge test was performed, activated at 0.1 C for 3 cycles, and then cycled at 2 C for 200 cycles. The results are shown in Table 1:

[0051] Table 1

[0052]

[0053] It can be seen from Table 1 that the carbon-based composite negative electrode material for sodium ion batteries prepared by the preparation method of the present invention has good conductivity, good electrochemical performance, and high capacity retention rate after 200 cycles, indicating that the carbon-based composite negative electrode material for sodium ion batteries has uniform pores, good cycle performance, high battery capacity, and strong adsorption and diffusion capabilities for sodium ions.

[0054] In Comparative Example 1, since nano-silica is directly generated in the polyacrylonitrile dispersion, the generated nano-silica particles have different sizes and agglomeration phenomenon, and the generated carbon-based composite negative electrode material has uneven pores and different sizes, so the electrochemical performance is poor; in Comparative Example 2, since hydroxy Zn-MOF is not covalently bonded to nano-silica, the generated carbon-based composite negative electrode material directly coats the nano-silica, and the porosity of the nano-silica surface and the carbon-based composite negative electrode material is reduced, resulting in low battery capacity; in Comparative Example 3, since the polymer template is not quaternized, the obtained nano-silica polymer has low stability, and the generated carbon-based composite negative electrode material has a low nitrogen doping content, resulting in a battery capacity lower than that of Examples 1 to 3.

[0055] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a carbon-based composite negative electrode material for a sodium ion battery, It is characterized in that The steps include: Step 1: dissolving the nano-silica polymer in N,N-dimethylformamide in a reaction kettle, dispersing the hydroxy Zn-MOF in N,N-dimethylformamide and adding the mixture into the reaction kettle, heating to 40-50° C., stirring and reacting for 1-1.5 hours, removing the solvent by rotary evaporation, and vacuum drying to obtain the nano-silica / Zn-MOF polymer; Step 2: heating the nano-silica / Zn-MOF polymer to 1000-1200° C. in a tube furnace under nitrogen protection for 2-3 hours at a heating rate of 5° C. / min to obtain a carbon-based composite negative electrode material; The nano silicon dioxide polymer is prepared by the following steps: In a reaction kettle, polyacrylonitrile and polymethyl methacrylate are dissolved in N-methylpyrrolidone, stirred and reacted at 70-80°C for 4-6 hours, polymethacrylate N,N-dimethylaminoethyl ester is added to the reaction kettle, stirred and reacted for 40-60 minutes, 1,2-bis(2-iodoethoxy)ethane is added, and the polymer template is obtained after standing for 48-72 hours, tetramethoxysilane and anhydrous ethanol are stirred and mixed, and then added to the reaction kettle, ammonia water is added to the reaction kettle, and stirred and reacted for 4-6 hours, the solvent is removed by rotary evaporation, and the insoluble matter is collected, and the insoluble matter is dried in a vacuum to obtain a nano-silica polymer.

2. A method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 1, It is characterized in that The hydroxy Zn-MOF is prepared by the following steps: In a reaction kettle, pamoic acid and 2,5-dihydroxyterephthalic acid were dissolved in N,N-dimethylformamide, and Zn(ClO 4 ) 2 6H 2 O is dissolved in methanol solution and added into the reaction kettle for mixing, and the mixture is sealed and heated to 75-85°C for reaction for 24-36h. After cooling, the mixture is washed with methanol and dried in vacuum to obtain hydroxy Zn-MOF.

3. A method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 2, It is characterized in that The dosage ratio of pamoic acid, 2,5-dihydroxyterephthalic acid and N,N-dimethylformamide is 4-5g:2-3g:200-250mL; the Zn(ClO 4 ) 2 6H 2 The dosage ratio of O and methanol is: 4-5g:100-125mL.

4. The method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 1, It is characterized in that In step 1, the usage ratio of the nano-silica polymer to N,N-dimethylformamide is 10-15 g: 20-30 mL; the usage ratio of the hydroxy Zn-MOF to N,N-dimethylformamide is 2-3 g: 10-15 mL.

5. The method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 1, It is characterized in that The usage ratio of polyacrylonitrile, polymethyl methacrylate, N-methylpyrrolidone, poly(N,N-dimethylaminoethyl methacrylate) and 1,2-bis(2-iodoethoxy)ethane is 10-15g:3-5g:80-85g:10-15g:3-4g.

6. A method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 1, It is characterized in that The dosage ratio of the tetramethoxysilane, anhydrous ethanol and aqueous ammonia is 3-5 mL: 45-50 mL: 15-20 mL.

7. A method for preparing a carbon-based composite negative electrode material for a sodium ion battery according to claim 6, It is characterized in that The mass fraction of the ammonia water is 1.5-2%.

Citation Information

Patent Citations

  • Sodium-ion battery carbon-based composite negative electrode material and preparation method thereof

    CN106935856A

  • Sodium-ion battery bamboo charcoal composite negative electrode and preparation method thereof

    CN118039884A

Cited By

  • Modified pole piece for energy storage and polymer solid-state battery

    CN121076068A