A composite flame retardant thermal insulation decorative board

By using organic flame retardant of various flame retardant elements in flame retardant insulation decorative panels combined with polyurethane gel, and using composite structures of inorganic silicon crystal panels and color steel panels, the flame retardant and thermal insulation properties of existing decorative panels are solved. The problem of insufficient results has achieved higher flame retardant effects and lower energy consumption.

CN118386616BActive Publication Date: 2024-11-12QINGDAO WANXING BUILDING MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410111220.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2024-11-12
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

The flame retardant and thermal insulation decorative panels have insufficient flame retardant and thermal insulation performance, resulting in poor fire resistance and high energy consumption under fire conditions, making it difficult to meet building safety and energy-saving needs.

Method used

Using organic flame retardant containing a variety of flame retardant elements (N, P, S, Si) combined with polyurethane gel, a flame retardant insulation layer is formed through cross-linking reaction, which improves the flame retardant and insulation properties of the material, and passes inorganic The composite structure of silicon crystal panels and color steel panels enhances the mechanical properties of the decorative panels.

Benefits of technology

It significantly improves the flame retardant and thermal insulation properties of decorative panels, reduces the thermal conductivity, enhances the mechanical properties of the materials, meets the needs of building safety and energy saving, and expands its application range.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a composite flame retardant heat-insulating decorative board, belonging to the technical field of decorative boards. It comprises a substrate, a heat-insulating layer arranged on one side of the substrate, and a decorative layer arranged on the other side of the heat-insulating layer, wherein the heat-insulating layer material is a flame retardant heat-insulating polyurethane gel, and a layer of flame retardant heat-insulating polyurethane gel material having flame retardant heat-insulating effect is arranged between the substrate and the decorative board, thereby obtaining a decorative board having multiple functions such as flame retardant, heat-insulating and mechanical properties, effectively overcoming the limitation of a single decorative board on the market, and the polyurethane gel heat-insulating decorative board can promote the popularization and application of new gel materials in flame retardant heat-insulating materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of decorative panels, and in particular to a composite flame-retardant heat-insulating decorative panel. Background Art

[0002] Flame retardant thermal insulation decorative panels are a new type of building material that has attracted much attention in the construction field in recent years. With the society's continuous pursuit of building safety and energy saving, flame retardant thermal insulation decorative panels have been widely studied and applied due to their excellent flame retardant properties and superior thermal insulation decorative characteristics.

[0003] The occurrence of building fires poses a great threat to people's lives and property safety, so the development of building materials with good flame retardant properties has become an urgent problem to be solved. Flame retardant thermal insulation decorative panels introduce flame retardants into the material composition, and through the reasonable design of the material structure, they have fire resistance under fire conditions. This not only provides higher safety for buildings, but also meets the construction industry's requirements for the continuous improvement of the fire resistance of building materials.

[0004] In addition, as the concept of energy conservation and environmental protection has become more popular, building energy conservation has also become a research hotspot in the global construction field. Flame-retardant thermal insulation decorative panels not only have excellent flame retardant properties, but also have excellent thermal insulation properties, which effectively reduces the energy consumption of buildings during winter heating and summer cooling, and provides a feasible solution for building energy conservation. Its thermal insulation performance can not only improve the thermal environment inside the building, but also reduce the adverse impact on the environment, which is in line with the concept of sustainable building development.

[0005] Therefore, the research results of flame retardant thermal insulation decorative panels not only have positive significance for improving the fire safety and energy conservation and environmental protection level of buildings, but also promote technological innovation and industrial upgrading in the field of building materials. With the continuous deepening of research, flame retardant thermal insulation decorative panels are expected to become an important, safe and reliable material choice in the construction field.

[0006] Chinese patent CN115162641A discloses a fireproof and heat-insulating decorative board and its preparation method and application. The composition of the fireproof and heat-insulating decorative board of the invention includes an aluminum silicate fiber reinforced silica aerogel layer, an adhesive layer and a stone-like decorative layer arranged in sequence. The preparation method of the fireproof and heat-insulating decorative board of the invention includes the following steps: first, separately prepare the aluminum silicate fiber reinforced silica aerogel layer and the stone-like decorative layer, and then glue the two with an adhesive to obtain a fireproof and heat-insulating decorative board. The fireproof and heat-insulating decorative board of the present invention has the advantages of excellent fireproof effect, excellent thermal insulation performance, good decorative effect, etc. However, the flame retardant and thermal insulation properties in the invention are not very good, and the thermal conductivity coefficient is 0.020W / (m·K). It is necessary to further improve the flame retardant and thermal insulation properties of the decorative board to further expand its application. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides a composite flame-retardant thermal insulation decorative board.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0009] A composite flame retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, wherein the heat-insulating layer material is flame retardant heat-insulating polyurethane gel.

[0010] The substrate is any one of an inorganic silicon crystal plate, a ceramic plate, an aluminum plate, and a stainless steel plate.

[0011] The decorative layer material is a color steel plate, and the thickness is 0.4-0.8 mm.

[0012] The thickness of the thermal insulation layer is 5-10 mm.

[0013] The flame retardant heat-insulating polyurethane gel is formed by mixing and cross-linking a flame retardant A component and a heat-insulating B component.

[0014] Organic flame retardants containing single flame retardant elements such as nitrogen, phosphorus, sulfur or silicon cannot achieve efficient flame retardancy. Therefore, it is necessary to synthesize multiple flame retardant elements by optimizing the process, and improve the flame retardant properties of the material by combining the synergistic flame retardant effect between the elements. Although containing multiple flame retardant elements can effectively improve the flame retardancy of the material, if the individual components containing flame retardant elements are mixed with the substrate, the compatibility and synergy between the components will be poor, which will not only lead to unstable effect of the flame retardant, but also poor flame retardant effect and even affect other properties of the substrate. The present invention can effectively overcome the above-mentioned defects by synthesizing an organic flame retardant containing multiple flame retardant elements such as N, P, S, and Si elements at the same time. The flame retardant is rich in N, P, S, and Si elements, which release phosphoric acid, nitride, sulfide, and silicon compound when heated, and has the advantages of high flame retardant efficiency, good carbonization, and good compatibility with the substrate.

[0015] During the combustion process, as the temperature rises, the flame retardant can form inert nitrogen compounds, phosphorus compound films, silicon compounds SiO2 and other flame retardant substances on the surface of the material. Specifically, nitrogen is inert at high temperatures and can inhibit the formation of flames and the combustion process; phosphorus elements may form phosphorus compounds at high temperatures, generating a layer of phosphorus compound film to isolate oxygen and slow down combustion. Some phosphorus compounds can prevent the combustion chain reaction in the gas phase, thereby inhibiting the spread of flames; sulfur is inert at high temperatures and can inhibit the formation and spread of flames. Some sulfur compounds can participate in gas phase reactions during combustion and reduce the combustion temperature; some silicon-containing compounds may generate silicon compounds during combustion, and these compounds can inhibit the combustion process.

[0016] In short, the substances generated above have the function of inhibiting the transfer of heat, oxygen and other thermal degradation products, inhibiting the release of smoke and combustible gases, and playing a barrier role. In addition, phosphorus and nitrogen elements can form metaphosphates and release inert gases to greatly assist in the flame retardant effect. The participation of sulfur in the reaction can reduce the propagation rate of combustion and the heat release of the flame, generate non-volatile sulfide products, inhibit free radical chain reactions, and prevent the combustion process. The three elements work synergistically to improve the flame retardant properties of the material, while also improving the mechanical properties of the substrate.

[0017] The method for preparing the flame retardant A component comprises the following steps:

[0018] S1: Dissolve 11-mercaptoundecylphosphoric acid and cyanuric chloride in pyridine, add sodium hydroxide aqueous solution to adjust the pH, and stir to react to obtain intermediate a;

[0019] S2: Under nitrogen protection, N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and ethanol aqueous solution are mixed, sodium hydroxide aqueous solution is added to adjust the pH to neutral, and the above intermediate a is added and stirred to obtain intermediate b;

[0020] S3, under nitrogen protection, the intermediate b and dimethyl sulfoxide are mixed evenly, 1,5-pentanediamine is added and stirred to obtain intermediate c;

[0021] S4 Under nitrogen protection, the intermediate c and dimethyl sulfoxide are mixed evenly, O-ethyl thiophosphoryl dichloride is added and stirred to obtain a flame retardant component A.

[0022] The specific reaction mechanism is that S1 uses 11-mercaptoundecyl phosphoric acid and cyanuric chloride as the main reactants and sodium hydroxide as the catalyst. A substitution reaction occurs under heating and stirring conditions. The mercapto group in 11-mercaptoundecyl phosphoric acid replaces a chlorine atom in cyanuric chloride to obtain intermediate a; S2 uses N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine as the flame retardant element Si source and sodium hydroxide as the catalyst. A substitution reaction occurs under heating and stirring conditions. The ammonia in N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine S3 uses 1,5-pentanediamine as the grafting intermediate, and replaces the third chlorine atom in intermediate b with an amino group in 1,5-pentanediamine under stirring to obtain intermediate c; S4 uses O-ethylthiophosphoryl dichloride as the flame retardant element S source, and a substitution reaction occurs under heating and stirring. The acyl chloride in O-ethylthiophosphoryl dichloride replaces another amino group in intermediate c, and the two acyl chlorides in O-ethylthiophosphoryl dichloride are replaced with the amino group in intermediate c to obtain the final product, flame retardant A component.

[0023] Preferably, the method for preparing the flame retardant component A comprises the following steps:

[0024] S1: Dissolve 2-4 parts by weight of 11-mercaptoundecylphosphoric acid and 1-3 parts by weight of cyanuric chloride in 40-80 parts by weight of pyridine at 0-6°C, add 0.1-0.5 parts by weight of 1-3 mol / L sodium hydroxide aqueous solution, adjust the pH to 6.5-7.5, stir at 300-500 rpm for 1-3 hours, remove the solvent by distillation under reduced pressure, recrystallize, wash, and dry to obtain intermediate a;

[0025] S2: Under nitrogen protection, 2-3 parts by weight of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and 60-160 parts by weight of 40-60wt% ethanol aqueous solution are mixed, 0.5-2mol / L sodium hydroxide aqueous solution is added to adjust the pH to neutral, 3-6 parts by weight of the above intermediate a are added, and the mixture is stirred at 70-90°C and 300-500rpm for 1-3h, and the solvent is distilled off under reduced pressure, recrystallized, washed, and dried to obtain intermediate b;

[0026] S3: Under nitrogen protection and at 20-30° C., 3-8 parts by weight of the intermediate b and 60-140 parts by weight of dimethyl sulfoxide are uniformly mixed, 0.5-2 parts by weight of 1,5-pentanediamine are added, the pH is adjusted to 6.5-7.5, and the mixture is stirred at 300-500 rpm for 0.5-2 h. The solvent is removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain the intermediate c.

[0027] S4: Under nitrogen protection and at 50-70°C, 3-6 parts by weight of the intermediate c and 60-140 parts by weight of dimethyl sulfoxide are uniformly mixed, 1-3 parts by weight of O-ethylthiophosphoryl dichloride are added, stirred at 300-500 rpm for 2-5 hours, cooled to room temperature, recrystallized, washed, and dried to obtain a flame retardant component A.

[0028] Polyurethane is a lightweight material with a low mass, which helps to reduce the weight of the material structure and improve the performance of the thermal insulation material. Polyurethane gel has good thermal insulation performance, which is mainly due to the special properties of its molecular structure and physical properties: (1) Polyurethane gel has a closed-cell structure in which gas cannot flow easily. This structure can reduce the convective heat transfer of gas and hinder the transfer of heat, thereby improving the thermal insulation performance. (2) The thermal conductivity of polyurethane gel is relatively low, which makes polyurethane gel perform well in avoiding heat transfer. (3) Polyurethane gel is a soft material that can fill and wrap surfaces of various shapes. This softness helps to reduce cracks and gaps in the thermal insulation structure and improve the thermal insulation effect. (4) Polyurethane has good chemical stability and strong resistance to water and some chemicals, which helps to maintain the long-term stability of its thermal insulation performance.

[0029] Specifically, the present invention uses poly(1,4-butylene adipate) and polymethylene polyphenyl polyisocyanate as main raw materials, uses dibutyltin dilaurate as a catalyst, and uses polyethyleneimine as a chain extender, which can not only increase the side branches of polyurethane, diffuse and extend the polyurethane molecular chains, and provide a network cross-linking structure, but also introduce linear polyethyleneimine into the polyurethane with a cross-linked network structure, and finally form an interpenetrating cross-linked network. This three-dimensional cross-linked network polymer can form a gel, and the flame retardant component A is cross-linked with the gel through a cross-linking agent, so as to give the polyurethane gel good flame retardant properties; the purpose of adding the surfactant epoxy soybean oil is to improve the dispersibility between the substances; the finally obtained thermal insulation layer has good thermal insulation and flame retardant effects, and also has good mechanical properties.

[0030] The heat-insulating B component is made of the following raw materials in parts by weight: 15-30 parts by weight of poly(1,4-butylene adipate), 20-30 parts by weight of polymethylene polyphenyl polyisocyanate, and 0.5-1.2 parts by weight of dibutyltin dilaurate.

[0031] The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps:

[0032] Y1: 15-30 parts by weight of poly(1,4-butylene adipate), 20-30 parts by weight of polymethylene polyphenyl polyisocyanate, and 0.5-1.2 parts by weight of dibutyltin dilaurate are mixed, and the mixture is stirred at 90-110° C. and 400-600 rpm for 1-3 hours under an argon atmosphere, and then cooled to obtain a heat-retaining component B;

[0033] Y2: 3-6 parts by weight of polyethyleneimine, 1-3 parts by weight of a cross-linking agent, 0.5-1.5 parts by weight of epoxy soybean oil, and 3-6 parts by weight of a flame retardant component A are mixed evenly, and then added together with 0.5-2 parts by weight of cyclopentane to the thermal insulation component B prepared in step S1, stirred evenly, and kept warm at 100-130°C for 50-70 minutes to obtain a flame retardant thermal insulation polyurethane gel.

[0034] The cross-linking agent is diethanolamine.

[0035] The method for preparing the composite flame retardant heat-insulating decorative board comprises the following steps:

[0036] (1) unwinding the color steel coil and pressing it into a color steel plate, pouring and coating the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying it so that the thickness of the final heat-insulating layer is 5-10 mm;

[0037] (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-track press for lamination at a lamination pressure of 0.04-0.1 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0038] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0039] Beneficial effects of the invention: The invention provides a composite flame retardant thermal insulation decorative board and a method for preparing the decorative board. By arranging a layer of flame retardant thermal insulation polyurethane gel material with flame retardant and thermal insulation effects between the substrate and the decorative board, a decorative board with multiple functions such as flame retardant, thermal insulation and mechanical properties is obtained, which effectively overcomes the limitation of the single decorative board on the market. The polyurethane gel thermal insulation decorative board can promote the promotion and application of new gel materials in flame retardant and thermal insulation materials, and provide new choices and new methods for the practical application of new thermal insulation decorative materials. DETAILED DESCRIPTION

[0040] The above content of the present invention is further described in detail below in conjunction with specific implementation modes, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments.

[0041] Introduction of some raw materials in this application:

[0042] Poly(1,4-butylene adipate) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., with the product number: P302959-100g.

[0043] Polyethyleneimine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., item number: E107080-100g Example 1

[0044] A composite flame-retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, which are arranged in sequence. The substrate is an inorganic silicon crystal board.

[0045] The insulation layer material is a commercially available flame-retardant insulation polyurethane gel blanket, and the thickness of the insulation layer is 6 mm; the decoration layer material is a color steel plate, and the thickness is 0.5 mm.

[0046] The preparation method of the composite flame retardant heat-insulating decorative board comprises the following steps:

[0047] (1) unwinding the color steel coil and pressing it into a color steel plate, bonding a commercially available flame-retardant heat-insulating polyurethane gel blanket to one side of the color steel plate, and drying it so that the thickness of the final insulation layer is 6 mm;

[0048] (2) The inorganic silicon crystal plate and the color steel plate of the commercially available flame-retardant and heat-insulating polyurethane gel blanket are simultaneously conveyed to a double-track press for lamination at a lamination pressure of 0.05 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0049] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0050] Example 2

[0051] A composite flame-retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, which are arranged in sequence. The substrate is an inorganic silicon crystal board.

[0052] The material of the thermal insulation layer is flame-retardant thermal insulation polyurethane gel, and the thickness of the thermal insulation layer is 6 mm; the material of the decorative layer is color steel plate, and the thickness is 0.5 mm.

[0053] The flame retardant heat-insulating polyurethane gel is prepared by mixing a flame retardant component A and a heat-insulating component B and cross-linking them through a cross-linking agent; the cross-linking agent is diethanolamine.

[0054] The preparation method of the flame retardant component A comprises the following steps: dissolving 2.5 parts by weight of 11-mercaptoundecyl phosphoric acid and 2 parts by weight of cyanuric chloride in 50 parts by weight of pyridine at 4° C., adding 0.4 parts by weight of a 2 mol / L sodium hydroxide aqueous solution, adjusting the pH to 7, stirring at 400 rpm for 2 hours, distilling off the solvent under reduced pressure, recrystallizing, washing, and drying to obtain the flame retardant component A.

[0055] The heat-retaining component B is made of the following raw materials in parts by weight: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate.

[0056] The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps:

[0057] Y1: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate were mixed, stirred at 100° C. and 500 rpm for 2 h under an argon atmosphere, and cooled to obtain a heat-retaining component B;

[0058] Y2 mixes 4 parts by weight of polyethyleneimine, 2 parts by weight of a cross-linking agent, 0.8 parts by weight of epoxy soybean oil, and 4 parts by weight of a flame retardant component A, and adds them together with 1 part by weight of cyclopentane to the thermal insulation component B prepared in step S1, stirs evenly, and keeps warm at 110°C for 60 minutes to obtain a flame retardant and thermal insulation polyurethane gel.

[0059] The preparation method of the composite flame retardant heat-insulating decorative board comprises the following steps:

[0060] (1) unwinding the color steel coil and pressing it into a color steel plate, pouring and coating the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying it so that the thickness of the final heat-insulating layer is 6 mm;

[0061] (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-belt press machine for lamination at a lamination pressure of 0.05 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0062] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0063] Example 3

[0064] A composite flame-retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, which are arranged in sequence. The substrate is an inorganic silicon crystal board.

[0065] The material of the thermal insulation layer is flame-retardant thermal insulation polyurethane gel, and the thickness of the thermal insulation layer is 6 mm; the material of the decorative layer is color steel plate, and the thickness is 0.5 mm.

[0066] The flame retardant heat-insulating polyurethane gel is prepared by mixing a flame retardant component A and a heat-insulating component B and cross-linking them through a cross-linking agent; the cross-linking agent is diethanolamine.

[0067] The method for preparing the flame retardant A component comprises the following steps:

[0068] S1: At 4°C, 2.5 parts by weight of 11-mercaptoundecylphosphoric acid and 2 parts by weight of cyanuric chloride are dissolved in 50 parts by weight of pyridine, 0.4 parts by weight of 2 mol / L sodium hydroxide aqueous solution are added, the pH is adjusted to 7, the mixture is stirred at 400 rpm for 2 hours, the solvent is removed by distillation under reduced pressure, the mixture is recrystallized, washed and dried to obtain intermediate a;

[0069] S2 Under nitrogen protection, 2.4 parts by weight of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and 80 parts by weight of 50wt% ethanol aqueous solution are mixed, 1 mol / L sodium hydroxide aqueous solution is added to adjust the pH to neutral, 4 parts by weight of the above intermediate a are added, and the mixture is stirred at 80°C and 400 rpm for 1.5 hours. The solvent is distilled off under reduced pressure, recrystallized, washed, and dried to obtain flame retardant component A.

[0070] The heat-retaining component B is made of the following raw materials in parts by weight: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate.

[0071] The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps:

[0072] Y1: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate were mixed, stirred at 100° C. and 500 rpm for 2 h under an argon atmosphere, and cooled to obtain a heat-retaining component B;

[0073] Y2 mixes 4 parts by weight of polyethyleneimine, 2 parts by weight of a cross-linking agent, 0.8 parts by weight of epoxy soybean oil, and 4 parts by weight of a flame retardant component A, and adds them together with 1 part by weight of cyclopentane to the thermal insulation component B prepared in step S1, stirs evenly, and keeps warm at 110°C for 60 minutes to obtain a flame retardant and thermal insulation polyurethane gel.

[0074] The preparation method of the composite flame retardant heat-insulating decorative board comprises the following steps:

[0075] (1) unwinding the color steel coil and pressing it into a color steel plate, pouring and coating the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying it so that the thickness of the final heat-insulating layer is 6 mm;

[0076] (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-belt press machine for lamination at a lamination pressure of 0.05 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0077] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0078] Example 4

[0079] A composite flame-retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, which are arranged in sequence. The substrate is an inorganic silicon crystal board.

[0080] The material of the thermal insulation layer is flame-retardant thermal insulation polyurethane gel, and the thickness of the thermal insulation layer is 6 mm; the material of the decorative layer is color steel plate, and the thickness is 0.5 mm.

[0081] The flame retardant heat-insulating polyurethane gel is prepared by mixing a flame retardant component A and a heat-insulating component B and cross-linking them through a cross-linking agent; the cross-linking agent is diethanolamine.

[0082] The method for preparing the flame retardant A component comprises the following steps:

[0083] S1: At 4°C, 2.5 parts by weight of 11-mercaptoundecylphosphoric acid and 2 parts by weight of cyanuric chloride are dissolved in 50 parts by weight of pyridine, 0.4 parts by weight of 2 mol / L sodium hydroxide aqueous solution are added, the pH is adjusted to 7, the mixture is stirred at 400 rpm for 2 hours, the solvent is removed by distillation under reduced pressure, the mixture is recrystallized, washed and dried to obtain intermediate a;

[0084] S2: Under nitrogen protection, 2.4 parts by weight of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and 80 parts by weight of 50 wt% ethanol aqueous solution were mixed, 1 mol / L sodium hydroxide aqueous solution was added to adjust the pH to neutral, 4 parts by weight of the above intermediate a were added, and the mixture was stirred at 80° C. and 400 rpm for 1.5 h. The solvent was removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain intermediate b;

[0085] S3: Under nitrogen protection and at 25°C, 5 parts by weight of the intermediate b and 80 parts by weight of dimethyl sulfoxide are uniformly mixed, 1 part by weight of 1,5-pentanediamine is added, the pH is adjusted to 7, and the mixture is stirred at 400 rpm for 1 hour. The solvent is removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain a flame retardant component A.

[0086] The heat-retaining component B is made of the following raw materials in parts by weight: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate.

[0087] The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps:

[0088] Y1: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate were mixed, stirred at 100° C. and 500 rpm for 2 h under an argon atmosphere, and cooled to obtain a heat-retaining component B;

[0089] Y2 mixes 4 parts by weight of polyethyleneimine, 2 parts by weight of a cross-linking agent, 0.8 parts by weight of epoxy soybean oil, and 4 parts by weight of a flame retardant component A, and then adds them together with 1 part by weight of cyclopentane to the thermal insulation component B prepared in step S1, stirs evenly, and keeps warm at 110°C for 60 minutes to obtain a flame retardant and thermal insulation polyurethane gel.

[0090] The preparation method of the composite flame retardant heat-insulating decorative board comprises the following steps:

[0091] (1) unwinding the color steel coil and pressing it into a color steel plate, pouring and coating the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying it so that the thickness of the final heat-insulating layer is 6 mm;

[0092] (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-belt press machine for lamination at a lamination pressure of 0.05 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0093] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0094] Example 5

[0095] A composite flame-retardant heat-insulating decorative board comprises a substrate, a heat-insulating layer arranged on one side of the substrate and a decorative layer arranged on the other side of the heat-insulating layer, which are arranged in sequence. The substrate is an inorganic silicon crystal board.

[0096] The material of the thermal insulation layer is flame-retardant thermal insulation polyurethane gel, and the thickness of the thermal insulation layer is 6 mm; the material of the decorative layer is color steel plate, and the thickness is 0.5 mm.

[0097] The flame retardant heat-insulating polyurethane gel is prepared by mixing a flame retardant component A and a heat-insulating component B and cross-linking them through a cross-linking agent; the cross-linking agent is diethanolamine.

[0098] The method for preparing the flame retardant A component comprises the following steps:

[0099] S1: At 4°C, 2.5 parts by weight of 11-mercaptoundecylphosphoric acid and 2 parts by weight of cyanuric chloride are dissolved in 50 parts by weight of pyridine, 0.4 parts by weight of 2 mol / L sodium hydroxide aqueous solution are added, the pH is adjusted to 7, the mixture is stirred at 400 rpm for 2 hours, the solvent is removed by distillation under reduced pressure, the mixture is recrystallized, washed and dried to obtain intermediate a;

[0100] S2: Under nitrogen protection, 2.4 parts by weight of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and 80 parts by weight of 50 wt% ethanol aqueous solution were mixed, 1 mol / L sodium hydroxide aqueous solution was added to adjust the pH to neutral, 4 parts by weight of the above intermediate a were added, and the mixture was stirred at 80° C. and 400 rpm for 1.5 h. The solvent was removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain intermediate b;

[0101] S3: Under nitrogen protection and at 25° C., 5 parts by weight of the intermediate b and 80 parts by weight of dimethyl sulfoxide were uniformly mixed, 1 part by weight of 1,5-pentanediamine was added, the pH was adjusted to 7, the mixture was stirred at 400 rpm for 1 hour, the solvent was removed by distillation under reduced pressure, the mixture was recrystallized, washed, and dried to obtain the intermediate c;

[0102] S4: Under nitrogen protection and at 60°C, 4 parts by weight of the intermediate c and 80 parts by weight of dimethyl sulfoxide were uniformly mixed, 2 parts by weight of O-ethylthiophosphoryl dichloride were added, and the mixture was stirred at 400 rpm for 3 hours. The mixture was cooled to room temperature, recrystallized, washed, and dried to obtain a flame retardant component A.

[0103] The heat-retaining component B is made of the following raw materials in parts by weight: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate.

[0104] The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps:

[0105] Y1: 20 parts by weight of poly(1,4-butylene adipate), 25 parts by weight of polymethylene polyphenyl polyisocyanate, and 1 part by weight of dibutyltin dilaurate were mixed, stirred at 100° C. and 500 rpm for 2 h under an argon atmosphere, and cooled to obtain a heat-retaining component B;

[0106] Y2 mixes 4 parts by weight of polyethyleneimine, 2 parts by weight of a cross-linking agent, 0.8 parts by weight of epoxy soybean oil, and 4 parts by weight of a flame retardant component A, and then adds them together with 1 part by weight of cyclopentane to the thermal insulation component B prepared in step S1, stirs evenly, and keeps warm at 110°C for 60 minutes to obtain a flame retardant and thermal insulation polyurethane gel.

[0107] The preparation method of the composite flame retardant heat-insulating decorative board comprises the following steps:

[0108] (1) unwinding the color steel coil and pressing it into a color steel plate, pouring and coating the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying it so that the thickness of the final heat-insulating layer is 6 mm;

[0109] (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-belt press machine for lamination at a lamination pressure of 0.05 MPa to bond the color steel plate and the inorganic silicon crystal plate into a composite plate;

[0110] (3) Cutting the composite board obtained above and stacking it for curing, thus obtaining the composite flame-retardant heat-insulating decorative board of the present invention.

[0111] Test Example 1

[0112] Oxygen index test: the test was conducted using method A of national standard GB / T2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test"; sample shape: Type II, the flame retardant and thermal insulation polyurethane gel was conditioned at a temperature of 23°C and a humidity of 50% for 90 hours before the test, the test sample had a length of 100 mm, a width of 10 mm, and a thickness of 10 mm, and 6 parallel groups were used to take the average value. The test results are shown in Table 1.

[0113] Table 1 Flame retardancy test results of flame retardant thermal insulation polyurethane gel

[0114] Oxygen index (%) Example 1 21.4 Example 2 25.9 Example 3 28.7 Example 4 32.1 Example 5 34.6

[0115] Test Example 2

[0116] 1. Tensile property test: The flame retardant and thermal insulation polyurethane gel materials prepared in Example 1 and Example 5 were tested according to the national standard GB / T6344-2008 "Determination of tensile strength and elongation at break of soft foam polymer materials"; the test specimens were type 1A, with a specimen width of 10 mm. Before the test, the specimens were placed in an environment with a temperature of 23°C and a relative humidity of 50% for 20 hours. Six groups were tested in parallel and the average value was taken. The results are shown in Table 2.

[0117] 2. Elongation at break test: The flame retardant and thermal insulation polyurethane gel materials prepared in Example 1 and Example 5 were tested according to the national standard GB / T6344-2008 "Determination of tensile strength and elongation at break of soft foam polymer materials". The test specimens were type 1A, with a specimen width of 10 mm. Before the test, the specimens were placed in an environment with a temperature of 23°C and a relative humidity of 50% for 20 hours. Six groups were tested in parallel and the average value was taken. The results are shown in Table 2.

[0118] Table 2 Mechanical properties test

[0119] Tensile strength(MPa) Elongation at break (%) Example 1 27.56 253.1 Example 5 35.72 284.6

[0120] Test Example 3

[0121] Thermal insulation performance test: The flame retardant thermal insulation polyurethane gel material obtained in Example 5 was injection molded and measured with reference to 3.2.2.3.2 Method B in the national standard GB / T10295-2008 "Determination of Steady-State Thermal Resistance of Insulating Materials and Related Specific Heat Flow Meter Method". The test temperature was 40°C. Each sample was tested 5 times on average and the average value was taken. The results are shown in Table 3.

[0122] Table 3 Thermal insulation performance test

[0123] Thermal conductivity / W / (m·K) Example 5 0.016

[0124] From the above results, it can be seen that the flame retardant and thermal insulation polyurethane gel material prepared by the present invention has good mechanical properties, flame retardant properties and thermal insulation properties. The thermal conductivity of the flame retardant and thermal insulation polyurethane gel prepared by the present invention meets the national standard of ≤0.041W / (m·K). The flame retardant and thermal insulation polyurethane gel prepared by the present invention has better flame retardant and mechanical properties than the commercially available flame retardant and thermal insulation polyurethane gel blanket in Example 1, indicating that the flame retardant and thermal insulation polyurethane gel prepared by the present invention is suitable for use in composite flame retardant and thermal insulation decorative panels, expanding the application range of the flame retardant and thermal insulation polyurethane gel. Compared with Examples 2-4, Example 5 synthesized an organic flame retardant containing multiple flame retardant elements such as N, P, S, and Si elements, which can effectively overcome the above-mentioned defects. The flame retardant is rich in N, P, S, and Si elements, which release phosphoric acid, nitrides, sulfides, and silicon compounds when heated. It has high flame retardant performance, good carbon expansion, and good compatibility with the substrate. In addition, phosphorus and nitrogen elements can form metaphosphates and release inert gases to greatly assist the flame retardant effect. The participation of sulfur in the reaction can reduce the propagation rate of combustion and the heat release of the flame, generate non-volatile sulfide products, inhibit free radical chain reactions, and prevent the combustion process. The three elements synergistically enhance the flame retardant properties of the material, while also improving the mechanical properties of the substrate. The flame retardant heat-insulating polyurethane gel material prepared by the present invention is a long-chain macromolecular compound with a network cross-structure, and can also form a cross-linked network structure with the introduced linear polyethyleneimine, and finally form a mutually penetrating cross-linked network. This three-dimensional cross-linked network polymer can form a gel, and finally the flame retardant component A and the gel are cross-linked together by a cross-linking agent, so that the polyurethane gel has good flame retardant properties. The flame retardant component A in the flame retardant heat-insulating polyurethane gel has good compatibility with the substrate, and the finally obtained thermal insulation layer has good thermal insulation and flame retardant effects, and also has good mechanical properties.

Claims

1. A composite flame retardant heat-insulating decorative board, characterized in that: It comprises a substrate, a heat-insulating layer arranged on one side of the substrate, and a decorative layer arranged on the other side of the heat-insulating layer, wherein the heat-insulating layer material is a flame-retardant heat-insulating polyurethane gel, and the flame-retardant heat-insulating polyurethane gel is formed by mixing and cross-linking a flame-retardant component A and a heat-insulating component B; The method for preparing the flame retardant A component comprises the following steps: S1: Dissolve 2-4 parts by weight of 11-mercaptoundecylphosphoric acid and 1-3 parts by weight of cyanuric chloride in 40-80 parts by weight of pyridine at 0-6°C, add 0.1-0.5 parts by weight of 1-3 mol / L sodium hydroxide aqueous solution, adjust the pH to 6.5-7.5, stir at 300-500 rpm for 1-3 hours, remove the solvent by distillation under reduced pressure, recrystallize, wash, and dry to obtain intermediate a; S2: Under nitrogen protection, 2-3 parts by weight of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine and 60-160 parts by weight of 40-60wt% ethanol aqueous solution are mixed, 0.5-2mol / L sodium hydroxide aqueous solution is added to adjust the pH to neutral, 3-6 parts by weight of the above intermediate a are added, and the mixture is stirred at 70-90°C and 300-500rpm for 1-3h, and the solvent is removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain intermediate b; S3: Under nitrogen protection and at 20-30° C., 3-8 parts by weight of the intermediate b and 60-140 parts by weight of dimethyl sulfoxide are uniformly mixed, 0.5-2 parts by weight of 1,5-pentanediamine are added, the pH is adjusted to 6.5-7.5, and the mixture is stirred at 300-500 rpm for 0.5-2 h. The solvent is removed by distillation under reduced pressure, recrystallized, washed, and dried to obtain the intermediate c. S4: Under nitrogen protection at 50-70° C., 3-6 parts by weight of the intermediate c and 60-140 parts by weight of dimethyl sulfoxide are uniformly mixed, 1-3 parts by weight of O-ethylthiophosphoryl dichloride are added, and the mixture is stirred at 300-500 rpm for 2-5 hours, cooled to room temperature, recrystallized, washed, and dried to obtain a flame retardant component A; The method for preparing the flame retardant heat-insulating polyurethane gel comprises the following steps: Y1: 15-30 parts by weight of poly(1,4-butylene adipate), 20-30 parts by weight of polymethylene polyphenyl polyisocyanate, and 0.5-1.2 parts by weight of dibutyltin dilaurate are mixed, and the mixture is stirred at 90-110° C. and 400-600 rpm for 1-3 hours under an argon atmosphere, and then cooled to obtain a heat-retaining component B; Y2: 3-6 parts by weight of polyethyleneimine, 1-3 parts by weight of a cross-linking agent, 0.5-1.5 parts by weight of epoxy soybean oil, and 3-6 parts by weight of a flame retardant component A are mixed evenly, and then added together with 0.5-2 parts by weight of cyclopentane to the thermal insulation component B prepared in step Y1, stirred evenly, and kept warm at 100-130°C for 50-70 minutes to obtain a flame retardant thermal insulation polyurethane gel.

2. The composite flame retardant heat insulation decorative board according to claim 1, characterized in that: The substrate is any one of an inorganic silicon crystal plate, a ceramic plate, an aluminum plate, and a stainless steel plate.

3. The composite flame retardant heat-insulating decorative board according to claim 1, characterized in that: The decorative layer material is a color steel plate with a thickness of 0.4-0.8 mm.

4. The composite flame retardant heat insulation decorative board according to claim 1, characterized in that: The thickness of the thermal insulation layer is 5-10 mm.

5. The composite flame retardant heat-insulating decorative board according to claim 1, characterized in that: The cross-linking agent is diethanolamine.

6. The method for preparing the composite flame retardant thermal insulation decorative board according to any one of claims 1 to 5, characterized in that: The steps include: (1) unwinding the color steel coil and pressing it into a color steel plate, pouring the flame retardant heat-insulating polyurethane gel on one side of the color steel plate through a coater, and drying; (2) The inorganic silicon crystal plate and the color steel plate coated with the flame-retardant polyurethane adhesive are simultaneously conveyed to a double-belt pressing machine for compounding, and the color steel plate and the inorganic silicon crystal plate are bonded into a composite plate; (3) Cutting the composite board obtained above and stacking it for curing can obtain the composite flame retardant and heat-insulating decorative board of the present invention.

Citation Information

Patent Citations

  • Fireproof thermal-insulation decorative board and preparation method and application thereof

    CN115162641A

  • Reactive type intumescent flame retardant for water-based polyurethane and preparation method of reactive type intumescent flame retardant

    CN104497050A

  • Flame-retardant polyurethane rigid foam plastic and preparation method and application thereof

    CN105884992A

  • Gel polyurethane ceramic spar in-situ composite heat insulation integrated board and production method thereof

    CN109930766A

  • Gel polyurethane ceramic spar in-situ composite thermal insulation integrated board and manufacturing method thereof

    CN109944405A