A contrast-enhancing aerosol based on magnetic particle nondestructive defect detection
By using a contrast-enhancing aerosol composed of titanium dioxide, barium sulfate, glass microspheres, and acrylic emulsion in magnetic particle non-destructive testing, the problem of coating thickness and uniformity is solved, and the sensitivity and clarity of magnetic particle detection are improved. Efficient detection of tiny defects is achieved.
Patent Information
- Application Number
- CN202410497315.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-04-24
AI Technical Summary
In the existing magnetic particle non-destructive testing method, the thickness of the coating formed by the contrast enhancer is difficult to control, resulting in a decrease in the sensitivity of magnetic particle testing, and the unevenness of the coating affects the detection results, making it difficult to detect small defects.
Using a contrast-enhancing aerosol based on magnetic particle non-destructive defect detection, by selecting a combination of titanium dioxide, barium sulfate, and glass microspheres as a whitening agent, combined with a composite film-forming agent and defoaming agent of acrylic emulsion and polyvinyl alcohol, a super Thin, high covering power and uniform coating improve the sensitivity and clarity of magnetic particle detection.
It significantly improves the sensitivity and clarity of magnetic particle non-destructive detection, ensuring that the coating is thin and uniform, the magnetic powder accumulation is obvious, the magnetic marks are clear, and the coating is easy to remove by washing, avoiding detection distortion and missed detection.
Smart Images

Figure BDA0004807571480000061 
Figure BDA0004807571480000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing of metal parts, in particular to magnetic powder nondestructive testing of metal precision parts, and in particular to a contrast enhancement aerosol based on magnetic powder nondestructive defect detection. Background Art
[0002] Various metal precision products, parts, structural welds, blade welds, etc. need to be tested for defects in a timely manner. Nondestructive testing uses the characteristics of sound, light, magnetism, electricity, etc., and can quickly detect defects such as pores, cracks, and slag in metal products without damaging or affecting the performance of the inspected object.
[0003] Currently commonly used non-destructive testing methods include: ultrasonic testing (UT), magnetic particle testing (MT), liquid penetrant testing (PT), X-ray testing (RT), etc.
[0004] Nondestructive testing based on magnetic powder is a nondestructive testing method with simple operation, efficient inspection, intuitive and reliable, and high sensitivity. At present, magnetic particle nondestructive testing is widely used in precision metal parts, welded structures, etc. The principle of magnetic particle nondestructive testing is to use the property that metal parts can be magnetized. It is mainly used for metal products such as iron, nickel, cobalt and its alloys, carbon steel, etc. Through magnetization, if there are defects such as pores, cold welding, cracks, etc. on the surface or near the surface of the product, the distribution of magnetic lines of force here will be distorted, also known as "leakage magnetic field". Sprinkle fine magnetic powder evenly on the surface of the metal product. Under the action of the magnetic field, the magnetic powder will gather in the direction of the defect, forming traces of magnetic powder accumulation, so that the location, distribution and size of the pore defects can be clearly, quickly and intuitively observed and judged.
[0005] When using magnetic particles to detect defects in metal products, since most metal products are brown, the magnetic particles and metal products are similar in color, and the accumulation and distribution of magnetic particles on the metal surface is not easy to be clearly observed, making it easy for magnetic particle detection to miss detection. In order to clearly, efficiently and accurately detect the accumulation of magnetic particles during magnetic particle detection, the existing technology mainly sprays a layer of white coating on the surface of the metal product to form a contrast with the color of the magnetic particles, so that the accumulation and distribution of the magnetic particles can be clearly observed.
[0006] For example, China Invention Patent Publication No. CN1210566C discloses a contrast enhancer for magnetic particle flaw detection, and the raw material composition is 2-6 weight percent titanium dioxide, 3-8 weight percent zinc oxide powder, 2-6 weight percent fluorescent brightener, 1-4 weight percent polyvinyl alcohol acetal, 22-40 weight percent butanol, and 36-70 weight percent methyl ethyl ketone. Its main characteristics are white color, whiteness of more than 85, which greatly improves the contrast effect of magnetic particle flaw detection, and is easy to clean after use; China Invention Patent Publication No. CN113686952A discloses a contrast enhancer, which includes the following components by weight percentage: 15-20 parts of a mixture of titanium dioxide, magnesium oxide, and zinc oxide powder; 3-5 parts of fluorescent brightener; 75-80 parts of volatile solvent; 0.5-2 parts of a mixture of ethyl cellulose ether and rosin resin; 30-50 parts of T-306 environmentally friendly solvent. The contrast enhancer is not only white in color, but also thin and uniform when sprayed, and dries immediately after spraying, which improves the detection efficiency.
[0007] However, although the existing contrast enhancers improve the clarity of observing the distribution of magnetic powder by forming a whitening film, the film formed by the contrast enhancer has a great impact on the detection sensitivity. Since the particle size of the currently used whitening agents such as titanium dioxide, magnesium oxide, and zinc oxide powder is generally around 10 microns, it is difficult to obtain a coating with a thickness of less than 1 micron. The thickness of the body layer formed by the existing contrast enhancers is generally 20-40um. The thicker the contrast enhancer coating, the weaker the force of the leakage magnetic field on the magnetic powder, which leads to a decrease in the sensitivity of magnetic powder detection, or even failure to detect defects. In addition, the uniformity of the coating thickness and the bubbles in the coating can also cause detection distortion. The thick coating film not only affects the adsorption of the "leakage magnetic field" on the magnetic powder at the defect, but also makes it difficult to produce sufficient adsorption for tiny defects, thereby reducing the sensitivity of flaw detection.
[0008] The current industrialized production of metal parts requires continuous, efficient and non-destructive detection, which places higher demands on contrast enhancers. There is an urgent need for contrast enhancers that can form ultra-thin, high-hiding, and uniformly thick coatings. Summary of the invention
[0009] When using magnetic particle nondestructive detection of metal parts, an ultra-thin, high-hiding, uniformly thick, and bubble-free contrast enhancement coating is of great significance for improving detection sensitivity and preventing missed detection. Based on this technical purpose, the present invention proposes a contrast enhancement aerosol based on magnetic particle nondestructive defect detection.
[0010] A contrast enhancement aerosol based on magnetic powder nondestructive defect detection is characterized by comprising a film-forming system and a propellant; wherein the components of the film-forming system include, by weight, 8-10 parts of an aqueous film-forming agent, 5-8 parts of a brightener, 0.5-1 parts of a leveling agent, 0.5-1 parts of a dispersant, 0.5-1 parts of a surfactant, 0.1-0.2 parts of a defoaming agent, and 100-150 parts of deionized water; wherein the film-forming agent is a composite of an acrylic emulsion and polyvinyl alcohol; the brightener is a composition of titanium dioxide, barium sulfate, and glass microspheres, wherein the titanium dioxide is selected from a particle size range of 0.15-0.45 μm; the barium sulfate is selected from spherical precipitated barium sulfate with a particle size less than 100 nm; and the glass microspheres are selected from high-sphericity microparticles with a particle size less than 1 μm.
[0011] Preferably, the aqueous film-forming agent is prepared by compounding polyvinyl alcohol and acrylic emulsion in a mass ratio of 1:2-3.
[0012] Preferably, the titanium dioxide, barium sulfate and glass microspheres in the whitening agent are used in a mass ratio of 10:1-2:1-2.
[0013] Preferably, the leveling agent is at least one of BYK-323 and BYK-326.
[0014] Preferably, the dispersant is phenyltrimethoxysilane.
[0015] Preferably, the surfactant is selected from at least one of polyoxyethylene fatty alcohol ethers, polyoxyethylene fatty acid esters, and ethylene oxide adducts of polypropylene glycol.
[0016] Preferably, the defoaming agent is a modified polyalkoxy ether.
[0017] Preferably, the propellant is dimethyl ether and / or butane; the amount is filled according to the tank pressure of the spray pressure tank, and the pressure is 1.7MPa, 1.8MPa, or 1.9MPa.
[0018] The contrast enhancement aerosol based on magnetic powder non-destructive defect detection is prepared by the following method:
[0019] (1) adding 5-8 parts of a brightener, 0.5-1 parts of a dispersant, 0.5-1 parts of a surfactant, and 40-50 parts of deionized water into a ball mill, and grinding at a low speed of 20-50 rpm for 0.5-1 h to obtain slurry I;
[0020] (2) adding 8-10 parts of an aqueous film-forming agent, 0.5-1 parts of a leveling agent, 0.1-0.2 parts of a defoaming agent, and 60-100 parts of deionized water into a mixer, and stirring and dispersing at a speed of 100-200 rpm to obtain slurry II;
[0021] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0022] In contrast enhancement aerosols, good flow and dispersion of whitening agents directly determine the thickness and uniformity of the coating. Conventional titanium dioxide with a particle size greater than 10μm is easy to disperse, but the coating is thicker; using nano-scale titanium dioxide can produce a thinner coating, but it is difficult to disperse or even agglomerate, which will cause the coating thickness uniformity to deteriorate and the coating is prone to agglomerated particles, affecting the distribution of magnetic particle detection.
[0023] The contrast enhancement aerosol spray coating has a significant effect on the sensitivity of magnetic particle detection due to its coating hiding power, coating thickness, coating uniformity, and coating bubbles. The whitening agent of the present invention is a combination of titanium dioxide, barium sulfate, and glass microspheres. The titanium dioxide has a particle size in the range of 0.15-0.45 μm, which has a high scattering ability and increases whiteness. At the same time, spherical precipitated barium sulfate with a particle size of less than 100 nm is used in combination to promote the dispersion of titanium dioxide, thereby ensuring the hiding power of the thin coating. In particular, spherical glass microspheres with a particle size of less than 1 μm are used in combination to increase the fluidity of the coating, thereby promoting the uniformity of the coating.
[0024] Furthermore, the film-forming agent is a composite of acrylic emulsion and polyvinyl alcohol. Acrylic acid forms a uniform film, but has strong water resistance after film formation and is difficult to clean. By using it in combination with polyvinyl alcohol, the film has good initial water resistance after film formation, which is conducive to the detection of magnetic powder and magnetic powder suspension without film removal. After the detection, the film-formed material is easy to be washed and removed, which increases the convenience of use.
[0025] Preferably, the defoamer is a modified polyalkoxy ether of BASF Foamaster MO 2114, which specifically reduces the surface tension of the aqueous film-forming agent and the brightener of the present invention, thereby reducing the stability of the foam included in the film-forming system, allowing the gas to quickly escape the film-forming system during spraying, effectively eliminating microbubbles during aerosol spraying, and increasing the uniformity of the coating.
[0026] Beneficial effects of the present invention:
[0027] (1) The contrast enhancement aerosol of the present invention selects appropriate titanium dioxide, barium sulfate, and glass microspheres to cooperate, so that the coating has good dispersibility, uniformity, and hiding power when it is thin, which can significantly improve the sensitivity and clarity of magnetic particle nondestructive detection.
[0028] (2) The present invention selects acrylic emulsion and polyvinyl alcohol to compound, so that the initial water resistance after film formation is good, which is conducive to the detection of magnetic powder and magnetic powder suspension without film removal. After the detection, the film is easy to be washed and removed, which increases the convenience of use.
[0029] (3) The present invention can effectively eliminate microbubbles in aerosol spraying and increase the uniformity of the coating by specifically selecting a defoaming agent that matches the film-forming agent and the whitening agent.
[0030] (4) The contrast enhancement aerosol of the present invention is simple and efficient in formulation, low in VOC, pollution-free, dries quickly after being sprayed on the surface of metal parts, has high efficiency in magnetic particle detection, and the coating is easy to be removed by water washing without causing corrosion to metal parts. DETAILED DESCRIPTION
[0031] This section generally describes the materials used in the experiments of the present invention. Although many materials and operating methods used to achieve the purpose of the present invention are well known in the art, the present invention is still described as detailed as possible. Based on the technical ideas of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present invention.
[0032] It is clear to those skilled in the art that, in the context, if not otherwise specified, the materials and operating methods used in the present invention are well known in the art. The raw materials involved in the embodiments are selected from conventional raw materials understood by those skilled in the art unless otherwise specified. The defoamer used is BASF's Foamaster MO 2114. The polyvinyl alcohol used is PVA 2488 and PVA1788. The acrylic emulsion is selected to have a solid content of 50% and a viscosity of 500-800 cP at room temperature.
[0033] Example 1
[0034] (1) Titanium dioxide with a particle size range of 0.15-0.45 μm, spherical precipitated barium sulfate with a particle size of less than 100 nm, and high-sphericity glass microspheres with a particle size of less than 1 μm are compounded in a mass ratio of 10:0.5:1, and 5 parts by weight are taken; 0.5 parts of phenyltrimethoxysilane dispersant is taken; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant is taken; 40 parts of deionized water are added to a ball mill, and ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0035] (2) Compounding polyvinyl alcohol (PVA2488) and acrylic emulsion in a mass ratio of 1:3, taking 10 parts, taking 0.5 parts of leveling agent BYK-323, taking 0.1 parts of defoaming agent (Foamaster MO 2114), and adding 80 parts of deionized water into a mixer, stirring and dispersing at a speed of 100 rpm to obtain slurry II;
[0036] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0037] Example 2
[0038] (1) Titanium dioxide with a particle size range of 0.15-0.45 μm, spherical precipitated barium sulfate with a particle size of less than 100 nm, and high-sphericity glass microspheres with a particle size of less than 1 μm are compounded in a mass ratio of 10:1:1, and 5 parts by weight are taken; 0.5 parts of phenyltrimethoxysilane dispersant is taken; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant is taken; 40 parts of deionized water are added to a ball mill, and ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0039] (2) Compound polyvinyl alcohol (PVA2488) and acrylic emulsion in a mass ratio of 1:2, take 10 parts, take 0.5 parts of leveling agent BYK-323, take 0.1 parts of defoaming agent (Foamaster MO 2114), and add 80 parts of deionized water into a mixer, stir and disperse at a speed of 100 rpm to obtain slurry II;
[0040] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0041] Example 3
[0042] (1) Titanium dioxide with a particle size range of 0.15-0.45 μm, spherical precipitated barium sulfate with a particle size of less than 100 nm, and high-sphericity glass microspheres with a particle size of less than 1 μm are compounded in a mass ratio of 10:1:0.5, and 5 parts by weight are taken; 0.5 parts of phenyltrimethoxysilane dispersant is taken; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant is taken; 40 parts of deionized water are added to a ball mill, and ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0043] (2) Compound polyvinyl alcohol (PVA 1788) and acrylic emulsion in a mass ratio of 1:3, take 10 parts, take 0.5 parts of leveling agent BYK-323, take 0.1 parts of defoaming agent (Foamaster MO 2114), and add 80 parts of deionized water into a mixer, stir and disperse at a speed of 100 rpm to obtain slurry II;
[0044] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0045] Comparative Example 1
[0046] A commercially available contrast-enhancing aerosol was used as a reference sample.
[0047] Comparative Example 2
[0048] (1) 5 parts by weight of titanium dioxide with a particle size range of 0.15-0.45 μm; 0.5 parts of phenyltrimethoxysilane dispersant; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant; 40 parts of deionized water were added to a ball mill and ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0049] (2) Compound polyvinyl alcohol (PVA2488) and acrylic emulsion in a mass ratio of 1:2, take 10 parts, take 0.5 parts of leveling agent BYK-323, take 0.1 parts of defoaming agent (Foamaster MO 2114), and add 80 parts of deionized water into a mixer, stir and disperse at a speed of 100 rpm to obtain slurry II;
[0050] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0051] Comparative Example 3
[0052] (1) Titanium dioxide with a particle size range of 0.15-0.45 μm and spherical precipitated barium sulfate with a particle size less than 100 nm are compounded in a mass ratio of 10:1, and 5 parts by weight are taken; 0.5 parts of phenyltrimethoxysilane dispersant is taken; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant is taken; 40 parts of deionized water are added to a ball mill, and ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0053] (2) Compound polyvinyl alcohol (PVA2488) and acrylic emulsion in a mass ratio of 1:2, take 10 parts, take 0.5 parts of leveling agent BYK-323, take 0.1 parts of defoaming agent (Foamaster MO 2114), and add 80 parts of deionized water into a mixer, stir and disperse at a speed of 100 rpm to obtain slurry II;
[0054] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0055] Comparative Example 4
[0056] (1) Titanium dioxide with a particle size range of 0.15-0.45 μm and high-sphericity glass microspheres with a particle size of less than 1 μm are compounded in a mass ratio of 10:1, and 5 parts by weight are taken; 0.5 parts of phenyltrimethoxysilane dispersant is taken; 0.5 parts of polyoxyethylene fatty alcohol ether surfactant is taken; 40 parts of deionized water are added to a ball mill, and the mixture is ground at a low speed of 50 rpm for 1 hour to obtain slurry I;
[0057] (2) Compound polyvinyl alcohol (PVA2488) and acrylic emulsion in a mass ratio of 1:2-3, take 10 parts, take 0.5 parts of leveling agent BYK-323, take 0.1 parts of defoaming agent (Foamaster MO 2114), and add 80 parts of deionized water into a mixer, stir and disperse at a speed of 100 rpm to obtain slurry II;
[0058] (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
[0059] Test data characterization:
[0060] In order to clearly characterize the coating hiding power, coating thickness and uniformity of the contrast-enhanced aerosol and the accuracy of magnetic particle detection of defects, the detection object is the same welded flat metal part, and the contrast-enhanced aerosol prepared by Implementation 1-3 and Comparative Example 1-4 is used to detect the welded flat metal part. The operation process is: clean the metal part, dry it, spray the contrast-enhanced aerosol at a distance of 15-20 cm from the surface of the metal part until the brown metal part color is completely covered; after the coating is dried, use a paint film meter to detect the thickness of 5 different points of the coating (as shown in Table 1); magnetize the metal part, and spray 10μm black magnetic powder at the same time, observe the location and shape of the magnetic powder accumulation on the surface of the metal part, and judge the location of the internal defects of the metal part and the relative size of the defect pores, as shown in Table 2.
[0061] Table 1:
[0062]
[0063]
[0064] Table 2:
[0065] Contrast enhancing aerosol Magnetic particle inspection accumulation Example 1 The coating is thin and uniform, the magnetic powder is obviously accumulated, and the magnetic traces are clear Example 2 The coating is thin and uniform, the magnetic powder is obviously accumulated, and the magnetic traces are clear Example 3 The coating is thin and uniform, the magnetic powder is obviously accumulated, and the magnetic traces are clear Comparative Example 1 The coating is thicker, the magnetic powder accumulation is not obvious, and the magnetic trace is weaker Comparative Example 2 The coating is slightly thicker, the magnetic powder accumulation lines are weakened, and the magnetic traces are weaker Comparative Example 3 The coating is slightly thicker, the magnetic powder accumulation lines are weakened, and the magnetic traces are weaker Comparative Example 4 The coating is slightly thicker, the magnetic powder accumulation lines are weakened, and the magnetic traces are weaker
[0066] Through testing, it is obvious that the contrast enhancement aerosol of the technical solution of the present invention in Examples 1-3 can form a thin and uniform white coating on the surface of the metal parts. When using magnetic particle detection, the magnetic powder accumulation is obvious at the defect and the magnetic trace is clear; Comparative Example 1 is a commercially available contrast enhancement aerosol that requires a thicker coating to cover the metal base color, and the film leveling is poor, the thickness uniformity is low, and the magnetic powder accumulation is significantly weakened during magnetic particle detection, which can easily cause missed detection. Comparative Example 2 does not use barium sulfate and glass beads in whitening, which affects the dispersion of titanium dioxide, requires a thicker coating to cover the metal base color, and the thickness uniformity of the coating is poor.
[0067] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A contrast enhancement aerosol based on magnetic powder non-destructive defect detection, characterized in that Including film forming systems and propellants; The components of the film-forming system include, by weight: 8-10 parts of aqueous film-forming agent, 5-8 parts of brightener, 0.5-1 parts of leveling agent, 0.5-1 parts of dispersant, 0.5-1 parts of surfactant, 0.1-0.2 parts of defoamer, and 100-150 parts of deionized water; wherein the film-forming agent is a composite of acrylic emulsion and polyvinyl alcohol; the brightener is a composition of titanium dioxide, barium sulfate, and glass microspheres, wherein the titanium dioxide has a particle size range of 0.15-0.45 μm; the barium sulfate is spherical precipitated barium sulfate with a particle size of less than 100 nm; and the glass microspheres are high-sphericity particles with a particle size of less than 1 μm. The contrast enhancement aerosol based on magnetic powder non-destructive defect detection is prepared by the following method: (1) adding 5-8 parts of a brightener, 0.5-1 parts of a dispersant, 0.5-1 parts of a surfactant, and 40-50 parts of deionized water into a ball mill, and grinding at a low speed of 20-50 rpm for 0.5-1 h to obtain slurry I; (2) adding 8-10 parts of an aqueous film-forming agent, 0.5-1 parts of a leveling agent, 0.1-0.2 parts of a defoaming agent, and 60-100 parts of deionized water into a mixer, and stirring and dispersing at a speed of 100-200 rpm to obtain slurry II; (3) Slurry I and slurry II are mixed at a stirring speed lower than 50 rpm, and quantitatively poured into an aerosol can. Then, the valve of the aerosol can is sealed, and the propellant is injected into the can to a specified pressure to obtain a contrast-enhanced aerosol for magnetic particle nondestructive defect detection.
2. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The aqueous film-forming agent is prepared by compounding polyvinyl alcohol and acrylic emulsion in a mass ratio of 1:2-3.
3. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The titanium dioxide, barium sulfate and glass microspheres in the whitening agent are used in a mass ratio of 10:1-2:1-2.
4. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The leveling agent is selected from at least one of BYK-323 and BYK-326.
5. The contrast enhancement aerosol based on magnetic powder non-destructive defect detection according to claim 1, characterized in that: The dispersant is phenyltrimethoxysilane.
6. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The surfactant is selected from at least one of polyoxyethylene fatty alcohol ethers, polyoxyethylene fatty acid esters, and ethylene oxide adducts of polypropylene glycol.
7. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The defoaming agent is a modified polyalkoxy ether.
8. The contrast enhancement aerosol based on magnetic powder nondestructive defect detection according to claim 1, characterized in that: The propellant is selected from dimethyl ether and / or butane.