A production method of environmentally friendly far-infrared negative ion fiber

Through multiple surface modifications of NdFeB powder and tourmaline powder, the problems of complex anion fiber production process and pollution were solved, and environmentally friendly far-infrared anion fiber with significant medical and health care effects was prepared, which improved the corrosion resistance and corrosion resistance of the fiber. mechanical properties.

CN118390189BActive Publication Date: 2024-10-22GUANGZHOU TAIDA FIBER PROD CO LTD

Patent Information

Application Number
CN202410627940.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-10-22
Estimated Expiration
2044-05-20

AI Technical Summary

Technical Problem

The existing negative ion fiber production process is complex and polluting, which cannot meet the needs of modern industrial production. Moreover, the corrosion resistance of NdFeB powder is poor, which affects the magnetic properties.

Method used

The NdFeB powder is multi-surface modified using acid chemical etching, nano-silica in-situ growth coating and silane coupling agent graft modification technology, and is passed through calcium stearate and titanate coupling agents. The tourmaline powder is surface-modified to form a coating layer to increase negative ion production and far-infrared emissivity, while enhancing the mechanical properties of the fiber.

Benefits of technology

The environmentally friendly far-infrared negative ion fiber is prepared, which has the functions of regulating the nervous system, promoting blood circulation, enhancing metabolism, sterilizing and deodorizing, and improving the corrosion resistance and mechanical properties of the fiber to meet the environmental protection and performance requirements of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118390189B_ABST
    Figure CN118390189B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of negative ion fibers, and provides a method for producing environmentally friendly far-infrared negative ion fibers, comprising: soaking NdFeB powder in an acidic aqueous solution to obtain acid-modified NdFeB powder; dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution, dripping an alcohol solution of ethyl orthosilicate to obtain a reaction solution, and dripping ammonia water to obtain silicon-coated NdFeB powder; dispersing the silicon-coated NdFeB powder in an organic solvent, adding a silane coupling agent to the dispersion to obtain modified NdFeB powder; mixing and heating a titanate coupling agent with an alcoholic aqueous solution, adding tourmaline powder and calcium stearate to obtain modified tourmaline powder; adding the modified NdFeB powder and the modified tourmaline powder to a polyester melt to obtain a spinning stock solution, and ejecting the solution through a spinning head into a coagulation bath to form a primary fiber. The far-infrared negative ion fiber prepared by the invention has the effects of regulating the nervous system, promoting blood circulation, enhancing metabolism, sterilization and deodorization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative ion fibers and relates to a production method of environmentally friendly far-infrared negative ion fibers. Background Art

[0002] Negative ion fiber is a fiber with the function of releasing negative ions. The negative ions released by this fiber have a significant effect on improving air quality and the environment. In particular, the health benefits of negative ions on the human body have been increasingly accepted by people.

[0003] At present, the production process of negative ion fiber is mainly to add a nano-level tourmaline powder with negative ion releasing function in the fiber production process, so that these tourmaline powders are embedded in the surface of the fiber. The electrons emitted by these tourmalines hit the oxygen molecules around the fiber and turn them into charged negative oxygen ions.

[0004] However, the existing negative ion fiber production process is often complicated and will produce certain pollution, which cannot meet the needs of modern industrial production. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for producing environmentally friendly far-infrared negative ion fibers. The far-infrared negative ion fibers prepared by the present invention can produce negative ions that are safe and have no side effects on the human body. The negative ions have the effects of regulating the nervous system, promoting blood circulation, enhancing metabolism, sterilizing and deodorizing.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for producing environmentally friendly far-infrared negative ion fibers, the method comprising:

[0008] (I) soaking NdFeB powder in an acidic aqueous solution, filtering after soaking, washing the solid with water until neutral, and drying the solid to obtain acid-modified NdFeB powder; subsequently, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution, dropping an alcohol solution of ethyl orthosilicate into the NdFeB solution, mixing evenly after the dropping is completed to obtain a reaction solution, dropping ammonia water into the reaction solution and stirring until the ethyl orthosilicate is hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and drying to obtain silicon-coated NdFeB powder; finally, dispersing the silicon-coated NdFeB powder in an organic solvent to form a dispersion, adding a silane coupling agent to the dispersion, mixing and stirring, filtering, washing and drying to obtain modified NdFeB powder;

[0009] (II) mixing a titanate coupling agent with an alcohol aqueous solution and heating the mixture to obtain a coupling agent solution, adding tourmaline powder and calcium stearate to the coupling agent solution, mixing the mixture to obtain a mixed solution, heating the mixed solution under sealed conditions to react so that the calcium stearate is coated on the surface of the tourmaline powder, and after the reaction is completed, filtering, washing and drying the mixture to obtain a modified tourmaline powder;

[0010] (III) adding the modified NdFeB powder obtained in step (I) and the modified tourmaline powder obtained in step (II) into a polyester melt, mixing and stirring to obtain a spinning solution; sending the spinning solution into a spinning head, spraying it out from the spinning head into a coagulation bath, and forming primary fibers after coagulation; the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers.

[0011] The far-infrared negative ion fiber provided by the present invention has the functions of generating negative ions and emitting far-infrared rays, and can achieve the effects of regulating the nervous system, promoting blood circulation, enhancing metabolism, sterilizing and deodorizing, etc. It can stimulate the activity of human cells better than single-function fiber materials, and therefore has better medical care effects. Functional textiles are made from the far-infrared negative ion fiber provided by the present invention as raw materials. When human skin contacts this functional textile, under the action of the modified tourmaline powder in the fabric, weak current and far-infrared rays are generated, and the electrical stimulation is transmitted to the central nervous system through the skin by the peripheral nerves. The far-infrared rays have strong penetration and radiation power, and have significant temperature control effect and resonance effect. After being absorbed by the human body, the water molecules in the body can resonate, activate the water molecules, enhance the binding force between the molecules, and increase the oxygen content in the body, so that the cells can be revitalized. The modified NdFeB powder can generate magnetic lines of force sufficient to penetrate the acupuncture points of the human body, which helps to promote blood circulation, dilate capillaries, and enhance metabolism.

[0012] The corrosion resistance of NdFeB powder is poor. In severe cases, it will corrode and rust under dry conditions, which has a great impact on the magnetic properties of NdFeB powder. To this end, the present invention performs multiple surface modifications on NdFeB powder, specifically including: acid chemical etching, in-situ growth coating of silicon dioxide and grafting modification of silane coupling agent. The three surface modification processes are organically combined and synergistic. Acid chemical etching can improve the surface roughness of NdFeB powder and bring active functional groups such as carboxyl and hydroxyl to NdFeB powder, providing active sites for the subsequent in-situ growth of nano-silicon dioxide, so as to improve the bonding strength of nano-silicon dioxide particles on the surface of NdFeB powder; then, nano-silicon dioxide is in-situ generated on the surface of NdFeB powder by the sol-gel method. Nano-silicon dioxide particles have good heat resistance and mechanical strength, which can effectively improve the heat resistance and mechanical properties of NdFeB powder, and can be used as mechanical reinforcing fillers while ensuring the magnetic properties of NdFeB powder; in addition, since nano-silicon dioxide particles are non-metallic, non-conductive insulators, they can reduce the conductivity between NdFeB powders and inhibit the formation of micro-electricity on the surface of NdFeB powder, thereby effectively improving the resistivity of NdFeB powder, and can also reduce magnetic loss when used under high-frequency conditions. However, NdFeB powder still has defects such as strong hygroscopicity, easy corrosion and poor interface compatibility with polyester matrix. Therefore, the present invention further performs silane coupling agent grafting modification on its outer surface, which can reduce its hygroscopicity on the one hand. At the same time, the silane coupling agent coating layer formed on the surface of NdFeB powder can isolate oxygen and water vapor in the environment, thereby greatly improving the antioxidant properties of NdFeB powder, thereby improving the corrosion resistance of NdFeB powder. On the other hand, it is also beneficial to improve the interface compatibility between NdFeB powder and polyester matrix, improve the thermal stability of NdFeB powder in subsequent processing, ensure the good magnetic properties of NdFeB powder, and improve the overall mechanical properties of far-infrared negative ion fiber.

[0013] The present invention uses calcium stearate and titanate coupling agent as compound modifiers to perform surface modification on tourmaline powder. In addition to maintaining its high negative ion generation amount and far-infrared emissivity, it can also be used as reinforcing fillers to improve the comprehensive mechanical properties of far-infrared negative ion fiber. On the one hand, calcium stearate and titanate coupling agent deposited on the surface of tourmaline powder form a coating layer, which can play a steric hindrance role. When subjected to uniaxial stress, the coating layer is well entangled with the polyester matrix, thereby increasing the interaction between the polyester matrix and the tourmaline powder; on the other hand, by performing surface modification on the tourmaline powder, the far-infrared negative ion fiber undergoes a brittle-tough transition, which is because the coating layer deposited on the surface of the tourmaline powder has a certain plastic deformation ability. Under the action of stress, the coating layer can be deformed to relieve the stress concentration phenomenon, so that the stress can be smoothly transferred from the polyester matrix to the tourmaline powder, and most of the energy and load are absorbed by the tourmaline powder, thereby improving the toughness and impact resistance of the far-infrared negative ion fiber.

[0014] As a preferred technical solution of the present invention, the environmentally friendly far-infrared negative ion fiber comprises the following components in parts by weight:

[0015] 5-15 parts of modified NdFeB powder;

[0016] 1-10 parts of modified tourmaline powder;

[0017] Polyester 70-80 parts.

[0018] Among them, the weight proportion of modified NdFeB powder can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15 parts, the weight proportion of modified tourmaline powder can be 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 parts, and the weight proportion of polyester can be 70, 71, 72, 73, 74, 75, 76, 77, 78, 79 or 80 parts, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0019] The present invention specifically limits the addition amount of modified NdFeB powder to 5-15 parts, and the solidification time of the polyester melt is extended with the increase of the addition amount of modified NdFeB powder. This is because the solidification process is the process of opening and closing of the polyester melt molecular chains in the coagulation bath. After the added modified NdFeB powder enters the coagulation bath, due to its large particle size and low surface activity, it can hinder the opening and closing process of the polyester melt molecular chains in the coagulation bath, so that the chemical reaction activity between the polyester melt and the coagulation bath is weakened, thereby hindering the solidification reaction of the polyester melt.

[0020] As a preferred technical solution of the present invention, in step (I), the mass fraction of the acidic aqueous solution is 20-30wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt% or 30wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In some optional examples, the acidic aqueous solution includes any one of an aqueous sulfuric acid solution, an aqueous nitric acid solution, or an aqueous hydrochloric acid solution, or a combination of at least two thereof.

[0022] In some optional examples, the immersion time of the NdFeB powder in the acidic aqueous solution is 40-50 min, for example, it can be 40 min, 41 min, 42 min, 43 min, 44 min, 45 min, 46 min, 47 min, 48 min, 49 min or 50 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] In some optional instances, the immersion temperature of the NdFeB powder in the acidic aqueous solution is 60-70°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] The surface of the NdFeB powder that has not been treated with acid is relatively smooth, which makes the interface bonding performance between it and the polyester matrix poor. When the far-infrared negative ion fiber is subjected to longitudinal load, the interface between the NdFeB powder and the polyester matrix cannot effectively transfer the load, making the NdFeB powder in the far-infrared negative ion fiber easily extracted from the polyester matrix.

[0025] The present invention performs acid immersion treatment on NdFeB powder, so that a large number of rough structures such as grooves and fine lines are generated on the surface of NdFeB powder. On the one hand, the reaction activity of the surface of NdFeB powder can be improved, and reaction active sites are provided for the subsequent in-situ growth of nano-silicon dioxide particles, and it is also beneficial for the nano-silicon dioxide particles to adhere to the surface of NdFeB powder; on the other hand, the specific surface area of ​​NdFeB powder is increased through chemical etching, and mechanical meshing between NdFeB powder and polyester matrix is ​​promoted; in addition, after acid immersion, a certain amount of oxygen-containing active groups such as hydroxyl and carboxyl are introduced into the surface of NdFeB powder, thereby improving the surface polarity of NdFeB powder, making the surface of NdFeB powder easier to be infiltrated by polyester melt, thereby improving the interface bonding strength between the two phases.

[0026] As a preferred technical solution of the present invention, in step (I), the mass fraction of ethyl orthosilicate in the alcohol solution of ethyl orthosilicate is 20-30wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt% or 30wt%, not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In some optional examples, the mass ratio of the acid-modified NdFeB powder to tetraethyl orthosilicate is 1:(1-2), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In some optional examples, the dripping speed of the alcohol solution of tetraethyl orthosilicate is 0.5-1 mL / min, for example, it can be 0.5 mL / min, 0.55 mL / min, 0.6 mL / min, 0.65 mL / min, 0.7 mL / min, 0.75 mL / min, 0.8 mL / min, 0.85 mL / min, 0.9 mL / min, 0.95 mL / min or 1 mL / min, not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0029] In some optional examples, after the addition of the alcohol solution of tetraethyl orthosilicate is completed, mixing and stirring is continued for 30-40 minutes, for example, it can be 30 minutes, 31 minutes, 32 minutes, 33 minutes, 34 minutes, 35 minutes, 36 minutes, 37 minutes, 38 minutes, 39 minutes or 40 minutes, not limited to the listed values, other values ​​not listed within the numerical range are also applicable.

[0030] In some optional examples, aqueous ammonia is added dropwise to the reaction solution to adjust the pH value of the reaction solution to 9-10, for example, it can be 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9 or 10.0, not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0031] In some optional examples, the drying temperature is 60-70°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] In some optional examples, the drying time is 12-24 hours, for example, it can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours or 24 hours, not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] The present invention generates nano-silicon dioxide in situ on the surface of NdFeB powder by a sol-gel method, so that a stable chemical bond is formed between the polyester matrix and the NdFeB powder, thereby effectively improving the thermal stability of the NdFeB powder and improving the magnetic properties and mechanical reinforcement performance of the NdFeB powder.

[0034] As a preferred technical solution of the present invention, in step (I), the concentration of the silicon-coated NdFeB powder in the dispersion is 0.1-0.5 g / mL, for example, it can be 0.1 g / mL, 0.15 g / mL, 0.2 g / mL, 0.25 g / mL, 0.3 g / mL, 0.35 g / mL, 0.4 g / mL, 0.45 g / mL or 0.5 g / mL, not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] In some optional examples, the organic solvent includes any one of methanol, ethanol, toluene or acetone, or a combination of at least two of them.

[0036] In some optional examples, the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent is 1:(0.01-0.05), for example, it can be 1:0.01, 1:0.015, 1:0.02, 1:0.025, 1:0.03, 1:0.035, 1:0.04, 1:0.045, 1:0.05, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] The particle size of NdFeB powder varies greatly, with the smaller particle size being about a few microns and the larger particle size far exceeding 50μm, which easily causes stress concentration in the polyester matrix, ultimately affecting the mechanical properties of the far-infrared negative ion fiber. In addition, the shape of NdFeB powder is irregular, with sharp edges and a very smooth surface. Without any surface treatment, it is directly doped into the polyester matrix, which is more likely to form excessive stress concentration at the sharp edges of the NdFeB powder. If it exceeds a certain limit, it will cause fiber cracks, which is not conducive to the filling and coating of the NdFeB powder by the polyester melt, and reduces the interface bonding strength between the NdFeB powder and the polyester matrix, resulting in a decrease in the overall mechanical properties of the far-infrared negative ion fiber. The present invention treats the NdFeB powder with a silane coupling agent, which can simultaneously exert physical and chemical effects.

[0038] On the one hand, the physical effect of the silane coupling agent is that while the NdFeB powder is subjected to the silane coupling agent grafting modification treatment, the silane coupling agent molecular layer can also be coated on the surface of the NdFeB powder. The surface roughness of the modified NdFeB powder is improved, which can passivate the sharpness of the edge of the powder particles. At the same time, the rough structure of the silane coupling agent molecular layer can also enhance the mechanical meshing between the NdFeB powder and the polyester matrix. In addition, NdFeB powder is a hydrophilic substance and has poor interfacial compatibility with the polyester matrix. After the surface treatment with the silane coupling agent, the hydrophilic functional groups in the silane coupling agent molecular chain are connected to the NdFeB powder, and the hydrophobic functional groups in the molecular chain face outward, which changes the surface polarity of the NdFeB powder, making the NdFeB powder change from hydrophilic to hydrophobic, thereby improving the interfacial bonding between the NdFeB powder and the polyester matrix, and ultimately improving the overall mechanical properties of the far-infrared negative ion fiber.

[0039] On the other hand, the chemical action of the silane coupling agent is reflected in that after the NdFeB powder is immersed in acid solution, a certain amount of oxygen-containing active groups such as hydroxyl and carboxyl are introduced on the surface of the NdFeB powder; when the NdFeB powder is surface treated with the silane coupling agent, some functional groups in the silane coupling agent molecular chain react with the hydroxyl and carboxyl groups on the surface of the NdFeB powder to form chemical bonds, and the other functional groups are physically entangled with the polyester molecular chain in three-dimensional space, thereby forming a "molecular bridge" between the NdFeB powder and the polyester matrix; in addition, the silane coupling agent molecule has a long-chain structure, and after being physically entangled with the polyester molecular chain, it can form a three-dimensional network structure that penetrates each other in space, and its effect of improving interface bonding is even greater than that of chemical bonding.

[0040] Therefore, the present invention can simultaneously exert physical and chemical modification effects by subjecting the NdFeB powder to silane coupling agent modification treatment, thereby enabling a stronger interface bond to be formed between the polyester matrix and the NdFeB powder.

[0041] The present invention particularly limits the mass ratio of silicon-coated NdFeB powder to silane coupling agent to 1:(0.01-0.05), and the appropriate addition of silane coupling agent can increase the interface bonding performance between NdFeB powder and polyester matrix, and the addition amount is too small to achieve the corresponding effect; at the same time, the silane coupling agent is also not easy to disperse, and the NdFeB powder cannot be completely and evenly wrapped, resulting in poor interface compatibility between NdFeB powder and polyester matrix, and pore defects are prone to occur in the far-infrared negative ion fiber finally prepared. And too high an addition amount will also make it impossible for the silane coupling agent to be coated on the surface of the NdFeB powder with a monomolecular layer, and the silane coupling agent molecular layer wrapped on the surface of the NdFeB powder is too thick, which affects the dispersion effect of the NdFeB powder in the polyester melt, and then causes the interface bonding strength between the NdFeB powder and the polyester matrix to decrease, and in addition, since the silane coupling agent is a non-magnetic substance, its excessive addition amount will cause the magnetic properties of the far-infrared negative ion fiber finally prepared to decrease.

[0042] In some optional examples, the mixing time of the dispersion and the silane coupling agent is 1-2h, for example, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] As a preferred technical solution of the present invention, in step (II), the mass ratio of the titanate coupling agent to the alcohol aqueous solution is (0.8-1):(1.5-2.5), for example, it can be 0.8:1.5, 0.82:1.6, 0.84:1.7, 0.86:1.8, 0.88:1.9, 0.9:2.0, 0.92:2.1, 0.94:2.2, 0.96:2.3, 0.98:2.4 or 1:2.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] In some optional examples, the titanate coupling agent is mixed with the alcohol aqueous solution and heated to 40-50°C, for example, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] As a preferred technical solution of the present invention, in step (II), the mass ratio of the tourmaline powder to the titanate coupling agent is (5-15):1, for example, it can be 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1 or 15:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] The present invention particularly limits the mass ratio of tourmaline powder to titanate coupling agent to (5-15): 1. With the increase of the addition amount of titanate coupling agent, the activation index and water contact angle of modified tourmaline powder gradually increase. The alkoxy group in the titanate coupling agent forms a chemical bond with the hydroxyl group on the surface of the tourmaline powder, and finally forms an organic active molecular layer between the interface of the tourmaline powder and the polyester matrix. Since the modified tourmaline powder and the polyester matrix have better compatibility, the interface strength between the two is higher, so that the far-infrared negative ion fiber can effectively transfer the stress to the modified tourmaline powder through the interface when subjected to stress. The rigid modified tourmaline powder acts as a stress concentration point and can improve the tensile strength of the far-infrared negative ion fiber. With the increase of the addition amount of the titanate coupling agent, the utilization efficiency of the titanate coupling agent gradually decreases, because the number of hydroxyl groups on the surface of the tourmaline powder is fixed, which limits the number of coupling reactions.

[0047] When the mass ratio of tourmaline powder to titanate coupling agent reaches 15:1, the grafting reaction of titanate coupling agent has reached saturation. At this time, the activation index and water contact angle of modified tourmaline powder tend to be stable. Continuing to increase the amount of titanate coupling agent added will increase additional costs. In addition, when the amount of titanate coupling agent added is too high, the tensile strength of far-infrared negative ion fiber shows a downward trend. This is because the amount of titanate coupling agent grafted on the surface of modified tourmaline powder is large, which increases the thickness of the organic active molecular layer deposited on the surface of tourmaline powder, but its strength is low, which will affect the interface strength between tourmaline powder and polyester matrix, resulting in a decrease in the ability to transmit impact energy.

[0048] In some optional examples, the mass ratio of the tourmaline powder to the calcium stearate is (5-15):(0.5-1.8), for example, it can be 5:0.5, 6:0.7, 7:0.8, 8:1.0, 9:1.2, 10:1.3, 11:1.4, 12:1.5, 13:1.6, 14:1.7 or 15:1.8, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] The addition of calcium stearate will reduce the surface tension of polyester melt to a certain extent, which is conducive to the dispersion of tourmaline powder in the composite polyester matrix. Calcium stearate is an anionic surfactant with long-chain alkyl groups in its molecular structure, which has a certain affinity with polyester; at the same time, the hydroxyl groups in the calcium stearate molecules can react physically and chemically with the surface of tourmaline powder, thereby greatly improving the interfacial compatibility between tourmaline powder and polyester matrix and improving the dispersion effect of tourmaline powder in polyester melt.

[0050] The present invention particularly limits the mass ratio of tourmaline powder to calcium stearate to (5-15): (0.5-1.8), and along with the increase of calcium stearate addition, the activation index and water contact angle of modified tourmaline powder are gradually improved. When the addition of calcium stearate exceeds the upper limit of the range defined by the present invention, the addition of calcium stearate is continuously increased, the activation index of modified tourmaline powder does not change much and the water contact angle also tends to be stable. This is because the specific surface area of ​​modified tourmaline powder is a fixed value, along with the increase of calcium stearate addition, the surface of modified tourmaline powder is completely coated, so that its surface gradually turns from hydrophilicity to hydrophobicity, which not only increases additional processing cost, but also causes the modified tourmaline powder to agglomerate due to the increase of hydrophobicity.

[0051] As a preferred technical solution of the present invention, in step (II), the heating temperature of the mixed solution is 60-70°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In some optional examples, the stirring speed of the mixed liquid is 100-200r / min, for example, it can be 100r / min, 110r / min, 120r / min, 130r / min, 140r / min, 150r / min, 160r / min, 170r / min, 180r / min, 190r / min or 200r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] In some optional examples, the reaction time of the mixed solution is 40-50 min, for example, it can be 40 min, 41 min, 42 min, 43 min, 44 min, 45 min, 46 min, 47 min, 48 min, 49 min or 50 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] As a preferred technical solution of the present invention, in step (III), the temperature of the coagulation bath is 40-50°C, for example, it can be 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] In some optional examples, the coagulation bath includes sulfuric acid, zinc sulfate, sodium sulfate and deionized water.

[0056] In some optional examples, the concentration of sulfuric acid in the coagulation bath is 50-60 g / L, for example, it can be 50 g / L, 51 g / L, 52 g / L, 53 g / L, 54 g / L, 55 g / L, 56 g / L, 57 g / L, 58 g / L, 59 g / L or 60 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] In some optional examples, the concentration of zinc sulfate in the coagulation bath is 15-20 g / L, for example, 15 g / L, 15.5 g / L, 16 g / L, 16.5 g / L, 17 g / L, 17.5 g / L, 18 g / L, 18.5 g / L, 19 g / L, 19.5 g / L or 20 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] In some optional examples, the concentration of sodium sulfate in the coagulation bath is 100-200 g / L, for example, it can be 100 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L, 180 g / L, 190 g / L or 200 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] As a preferred technical solution of the present invention, in step (III), the drawing speed of the spun fiber is 20-160 m / min, for example, it can be 20 m / min, 30 m / min, 40 m / min, 50 m / min, 60 m / min, 70 m / min, 80 m / min, 90 m / min, 100 m / min, 110 m / min, 120 m / min, 130 m / min, 140 m / min, 501 m / min or 60 m / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] In some optional examples, the diameter of the spinneret hole is 0.08-0.15 mm, for example, 0.08 mm, 0.085 mm, 0.09 mm, 0.095 mm, 0.1 mm or 0.015 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Exemplarily, the present invention provides a method for producing environmentally friendly far-infrared negative ion fibers, the production method specifically comprising the following steps:

[0062] (1) Soaking NdFeB powder in a 20-30wt% acidic aqueous solution, soaking for 40-50min at 60-70°C, filtering, washing the solid with water until neutral, and drying the solid to obtain acid-modified NdFeB powder; then, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution, adding a 20-30wt% alcohol solution of ethyl orthosilicate to the NdFeB solution at a dropping speed of 0.5-1mL / min, wherein the mass ratio of the acid-modified NdFeB powder to the ethyl orthosilicate is 1:(1-2), and continuing to mix and stir for 30-40min after the addition is completed to obtain The reaction liquid is added with ammonia water to adjust the pH value of the reaction liquid to 9-10, and the reaction liquid is stirred until the tetraethyl orthosilicate is hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and the mixture is dried at 60-70°C for 12-24h to obtain silicon-coated NdFeB powder; finally, the silicon-coated NdFeB powder is dispersed in a solvent to form a dispersion liquid of 0.1-0.5g / mL, and a silane coupling agent is added to the dispersion liquid and mixed and stirred for 1-2h, wherein the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent is 1:(0.01-0.05), and the modified NdFeB powder is obtained after suction filtration, washing and drying;

[0063] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of (0.8-1):(1.5-2.5) and heating to 40-50° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of tourmaline powder to titanate coupling agent is (5-15):1, and the mass ratio of tourmaline powder to calcium stearate is (5-15):(0.5-1.8), mixing to obtain a mixed solution, heating the mixed solution to 60-70° C. under sealed conditions and stirring at a speed of 100-200 r / min to react, the reaction time is 40-50 min, so that the calcium stearate is coated on the surface of the tourmaline powder, and after the reaction is completed, filtering, washing and drying to obtain modified tourmaline powder;

[0064] (3) adding 5-15 parts of the modified NdFeB powder obtained in step (1) and 1-10 parts of the modified tourmaline powder obtained in step (2) into 70-80 parts of a polyester melt, mixing and stirring to obtain a spinning solution; feeding the spinning solution into a spinning head, ejecting the spinning solution through the spinning head into a coagulation bath at 40-50° C., wherein the diameter of the spinneret hole of the spinning head is 0.08-0.15 mm, the concentration of sulfuric acid in the coagulation bath is 50-60 g / L, the concentration of zinc sulfate is 15-20 g / L, and the concentration of sodium sulfate is 100-200 g / L, and primary fibers are formed after coagulation, and the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the primary fibers is 20-160 m / min.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] The far-infrared negative ion fiber provided by the present invention has the functions of generating negative ions and emitting far-infrared rays, and can achieve the effects of regulating the nervous system, promoting blood circulation, enhancing metabolism, sterilizing and deodorizing, etc. It can stimulate the activity of human cells better than single-function fiber materials, and therefore has better medical care effects. Functional textiles are made from the far-infrared negative ion fiber provided by the present invention as raw materials. When human skin contacts this functional textile, under the action of the modified tourmaline powder in the fabric, weak current and far-infrared rays are generated, and the electrical stimulation is transmitted to the central nervous system through the skin by the peripheral nerves. The far-infrared rays have strong penetration and radiation power, and have significant temperature control effect and resonance effect. After being absorbed by the human body, the water molecules in the body can resonate, activate the water molecules, enhance the binding force between the molecules, and increase the oxygen content in the body, so that the cells can be revitalized. The modified NdFeB powder can generate magnetic lines of force sufficient to penetrate the acupuncture points of the human body, which helps to promote blood circulation, dilate capillaries, and enhance metabolism.

[0067] The corrosion resistance of NdFeB powder is poor. In severe cases, it will corrode and rust under dry conditions, which has a great impact on the magnetic properties of NdFeB powder. To this end, the present invention performs multiple surface modifications on NdFeB powder, specifically including: acid chemical etching, in-situ growth coating of silicon dioxide and grafting modification of silane coupling agent. The three surface modification processes are organically combined and synergistic. Acid chemical etching can improve the surface roughness of NdFeB powder and bring active functional groups such as carboxyl and hydroxyl to NdFeB powder, providing active sites for the subsequent in-situ growth of nano-silicon dioxide, so as to improve the bonding strength of nano-silicon dioxide particles on the surface of NdFeB powder; then, nano-silicon dioxide is in-situ generated on the surface of NdFeB powder by the sol-gel method. Nano-silicon dioxide particles have good heat resistance and mechanical strength, which can effectively improve the heat resistance and mechanical properties of NdFeB powder, and can be used as mechanical reinforcing fillers while ensuring the magnetic properties of NdFeB powder; in addition, since nano-silicon dioxide particles are non-metallic, non-conductive insulators, they can reduce the conductivity between NdFeB powders and inhibit the formation of micro-electricity on the surface of NdFeB powder, thereby effectively improving the resistivity of NdFeB powder, and can also reduce magnetic loss when used under high-frequency conditions. However, NdFeB powder still has defects such as strong hygroscopicity, easy corrosion and poor interface compatibility with polyester matrix. Therefore, the present invention further performs silane coupling agent grafting modification on its outer surface, which can reduce its hygroscopicity on the one hand. At the same time, the silane coupling agent coating layer formed on the surface of NdFeB powder can isolate oxygen and water vapor in the environment, thereby greatly improving the antioxidant properties of NdFeB powder, thereby improving the corrosion resistance of NdFeB powder. On the other hand, it is also beneficial to improve the interface compatibility between NdFeB powder and polyester matrix, improve the thermal stability of NdFeB powder in subsequent processing, ensure the good magnetic properties of NdFeB powder, and improve the overall mechanical properties of far-infrared negative ion fiber.

[0068] The present invention uses calcium stearate and titanate coupling agent as compound modifiers to perform surface modification on tourmaline powder. In addition to maintaining its high negative ion generation amount and far-infrared emissivity, it can also be used as reinforcing fillers to improve the comprehensive mechanical properties of far-infrared negative ion fiber. On the one hand, calcium stearate and titanate coupling agent deposited on the surface of tourmaline powder form a coating layer, which can play a steric hindrance role. When subjected to uniaxial stress, the coating layer is well entangled with the polyester matrix, thereby increasing the interaction between the polyester matrix and the tourmaline powder; on the other hand, by performing surface modification on the tourmaline powder, the far-infrared negative ion fiber undergoes a brittle-tough transition, which is because the coating layer deposited on the surface of the tourmaline powder has a certain plastic deformation ability. Under the action of stress, the coating layer can be deformed to relieve the stress concentration phenomenon, so that the stress can be smoothly transferred from the polyester matrix to the tourmaline powder, and most of the energy and load are absorbed by the tourmaline powder, thereby improving the toughness and impact resistance of the far-infrared negative ion fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 A production process flow chart of the environmentally friendly far-infrared negative ion fiber provided in Examples 1-9 of the present invention;

[0070] Figure 2 This is a scanning electron microscope image of unmodified NdFeB powder;

[0071] Figure 3 This is a scanning electron microscope image of the modified NdFeB powder prepared in Example 1;

[0072] Figure 4 is a scanning electron microscope image of unmodified tourmaline powder;

[0073] Figure 5 This is a scanning electron microscope image of the modified tourmaline powder prepared in Example 1. DETAILED DESCRIPTION

[0074] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.

[0075] Example 1

[0076] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. Figure 1 As shown, the production method specifically comprises the following steps:

[0077] (1) Soaking NdFeB powder in a 20wt% aqueous sulfuric acid solution, the ratio of NdFeB powder to the aqueous sulfuric acid solution is 10g:1L, soaking at 70°C for 40min and filtering, washing the solid with water until neutral, and drying the solid to obtain acid-modified NdFeB powder; then, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution with a concentration of 0.1g / mL, adding a 20wt% ethyl orthosilicate ethanol solution to the NdFeB solution at a dropping speed of 0.5mL / min, the mass ratio of the acid-modified NdFeB powder to the ethyl orthosilicate is 1:1, and after the addition is completed, Continue mixing and stirring for 30 minutes to obtain a reaction solution, add ammonia water to the reaction solution to adjust the pH value of the reaction solution to 9, stir until the tetraethyl orthosilicate is hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and dry at 60°C for 24 hours to obtain silicon-coated NdFeB powder; finally, disperse the silicon-coated NdFeB powder in methanol to form a 0.1 g / mL dispersion, add silane coupling agent KH550 to the dispersion, mix and stir for 1 hour, the mass ratio of silicon-coated NdFeB powder to silane coupling agent KH550 is 1:0.01, and obtain modified NdFeB powder after suction filtration, washing and drying;

[0078] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of 0.8:1.5 and heating the mixture to 40° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of the tourmaline powder to the titanate coupling agent is 5:1, and the mass ratio of the tourmaline powder to the calcium stearate is 5:0.5, and mixing to obtain a mixed solution; heating the mixed solution to 60° C. under sealed conditions and stirring the mixed solution at a speed of 100 r / min to react for 50 minutes, so that the calcium stearate is coated on the surface of the tourmaline powder; and after the reaction is completed, filtering, washing and drying the mixed solution to obtain a modified tourmaline powder;

[0079] (3) 5 parts by weight of the modified NdFeB powder obtained in step (1) and 1 part by weight of the modified tourmaline powder obtained in step (2) are added to 70 parts by weight of a polyester melt, mixed and stirred to obtain a spinning solution; the spinning solution is fed into a spinning head, and ejected from the spinning head into a coagulation bath at 40° C., the spinneret diameter of the spinning head is 0.08 mm, the concentration of sulfuric acid in the coagulation bath is 50 g / L, the concentration of zinc sulfate is 15 g / L, and the concentration of sodium sulfate is 200 g / L, and primary fibers are formed after coagulation, and the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the primary fibers is 20 m / min.

[0080] Figure 2 and Figure 3 The scanning electron microscope images of NdFeB powder before and after modification are shown in Figure 2. Figure 2 and Figure 3By comparison, it can be seen that nano-silicon dioxide particles are formed on the surface of NdFeB powder and are coated and wrapped by silane coupling agent.

[0081] Figure 4 and Figure 5 The scanning electron microscope images of tourmaline powder before and after modification are respectively Figure 4 and Figure 5 By comparison, it can be seen that the unmodified tourmaline powder has serious agglomeration phenomenon, which is mainly due to the strong surface polarity of the tourmaline powder, which is easy to cause agglomeration. The agglomeration phenomenon of the modified tourmaline powder is significantly alleviated, and the tourmaline powder is evenly dispersed, showing excellent dispersibility. This is because the surface of the tourmaline powder is modified with organic groups after the modification, and its surface polarity is reduced to a certain extent, thus showing better dispersion characteristics.

[0082] Example 2

[0083] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. Figure 1 As shown, the production method specifically comprises the following steps:

[0084] (1) Soaking NdFeB powder in a 22 wt% aqueous sulfuric acid solution, the ratio of NdFeB powder to the aqueous sulfuric acid solution is 10 g:1 L, soaking at 68°C for 42 min and filtering, washing the solid with water until neutral, and drying the solid to obtain an acid-modified NdFeB powder; then, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution with a concentration of 0.2 g / mL, adding a 22 wt% ethyl orthosilicate ethanol solution to the NdFeB solution at a dropping speed of 0.6 mL / min, the mass ratio of the acid-modified NdFeB powder to the ethyl orthosilicate being 1:1.2, and then The mixture was mixed and stirred for 32 minutes to obtain a reaction solution, and ammonia water was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 9.2, and the mixture was stirred until the tetraethyl orthosilicate was hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and the mixture was dried at 62°C for 22 hours to obtain silicon-coated NdFeB powder; finally, the silicon-coated NdFeB powder was dispersed in ethanol to form a dispersion solution of 0.2 g / mL, and a silane coupling agent KH560 was added to the dispersion solution and mixed and stirred for 1.2 hours, wherein the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent KH560 was 1:0.02, and the modified NdFeB powder was obtained after suction filtration, washing and drying;

[0085] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of 0.86:1.8 and heating the mixture to 42° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of the tourmaline powder to the titanate coupling agent is 8:1, and the mass ratio of the tourmaline powder to the calcium stearate is 8:1.0, and mixing to obtain a mixed solution; heating the mixed solution to 62° C. under sealed conditions and stirring the mixed solution at a speed of 120 r / min to react for 48 minutes, so that the calcium stearate is coated on the surface of the tourmaline powder; after the reaction is completed, filtering, washing and drying the mixed solution to obtain a modified tourmaline powder;

[0086] (3) 8 parts by weight of the modified NdFeB powder obtained in step (1) and 3 parts by weight of the modified tourmaline powder obtained in step (2) are added to 72 parts by weight of a polyester melt, mixed and stirred to obtain a spinning solution; the spinning solution is fed into a spinning head, and ejected from the spinning head into a coagulation bath at 42° C., the spinneret diameter of the spinning head is 0.1 mm, the concentration of sulfuric acid in the coagulation bath is 52 g / L, the concentration of zinc sulfate is 16 g / L, and the concentration of sodium sulfate is 180 g / L, and primary fibers are formed after coagulation. The primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the primary fibers is 60 m / min.

[0087] Example 3

[0088] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. Figure 1 As shown, the production method specifically comprises the following steps:

[0089] (1) Soaking NdFeB powder in a 25wt% nitric acid aqueous solution, with the ratio of NdFeB powder to sulfuric acid aqueous solution being 10g:1L, soaking at 65°C for 45min and filtering, washing the solid with water until neutral, and drying the solid to obtain an acid-modified NdFeB powder; subsequently, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution with a concentration of 0.3g / mL, and dripping 25wt% ethyl orthosilicate ethanol solution into the NdFeB solution at a dripping speed of 0.7mL / min, with the mass ratio of the acid-modified NdFeB powder to ethyl orthosilicate being 1:1.5, and then The mixture was mixed and stirred for 35 minutes to obtain a reaction solution, and ammonia water was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 9.5, and the mixture was stirred until ethyl orthosilicate was hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and the mixture was dried at 65°C for 20 hours to obtain silicon-coated NdFeB powder; finally, the silicon-coated NdFeB powder was dispersed in toluene to form a dispersion solution of 0.3 g / mL, and silane coupling agent KH560 was added to the dispersion solution and mixed and stirred for 1.5 hours, wherein the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent KH560 was 1:0.03, and the modified NdFeB powder was obtained after suction filtration, washing and drying;

[0090] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of 0.9:2.0 and heating to 45° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of tourmaline powder to titanate coupling agent is 10:1, and the mass ratio of tourmaline powder to calcium stearate is 10:1.3, and mixing to obtain a mixed solution, heating the mixed solution to 65° C. under sealed conditions and stirring at a speed of 150 r / min to react for 45 minutes, so that the calcium stearate is coated on the surface of the tourmaline powder, and after the reaction is completed, filtering, washing and drying to obtain modified tourmaline powder;

[0091] (3) 10 parts by weight of the modified NdFeB powder obtained in step (1) and 5 parts by weight of the modified tourmaline powder obtained in step (2) are added to 75 parts by weight of a polyester melt and mixed to obtain a spinning solution; the spinning solution is fed into a spinning head, and ejected from the spinning head into a coagulation bath at 45° C., the spinneret hole diameter of the spinning head is 0.12 mm, the concentration of sulfuric acid in the coagulation bath is 55 g / L, the concentration of zinc sulfate is 17 g / L, and the concentration of sodium sulfate is 150 g / L. After coagulation, nascent fibers are formed, and the nascent fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the nascent fibers is 100 m / min.

[0092] Example 4

[0093] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. Figure 1As shown, the production method specifically comprises the following steps:

[0094] (1) Soaking NdFeB powder in a 28 wt % nitric acid aqueous solution, with the ratio of NdFeB powder to sulfuric acid aqueous solution being 10 g:1 L, soaking at 62° C. for 48 min and filtering, washing the solid with water until neutral, and drying the solid to obtain an acid-modified NdFeB powder; subsequently, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution with a concentration of 0.4 g / mL, and dripping 28 wt % ethyl orthosilicate ethanol solution into the NdFeB solution at a dripping speed of 0.8 mL / min, with the mass ratio of the acid-modified NdFeB powder to ethyl orthosilicate being 1:1.8, and then The mixture was mixed and stirred for 38 minutes to obtain a reaction solution, and ammonia water was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 9.8, and the mixture was stirred until ethyl orthosilicate was hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and the mixture was dried at 68°C for 15 hours to obtain silicon-coated NdFeB powder; finally, the silicon-coated NdFeB powder was dispersed in acetone to form a dispersion solution of 0.4 g / mL, and silane coupling agent KH570 was added to the dispersion solution and mixed and stirred for 1.8 hours, wherein the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent KH570 was 1:0.04, and the modified NdFeB powder was obtained after suction filtration, washing and drying;

[0095] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of 0.96:2.3 and heating the mixture to 48° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of the tourmaline powder to the titanate coupling agent is 12:1, and the mass ratio of the tourmaline powder to the calcium stearate is 13:1.6, and mixing to obtain a mixed solution; heating the mixed solution to 68° C. under sealed conditions and stirring the mixed solution at a speed of 180 r / min to react for 42 minutes, so that the calcium stearate is coated on the surface of the tourmaline powder; and after the reaction is completed, filtering, washing and drying the mixed solution to obtain a modified tourmaline powder;

[0096] (3) 12 parts by weight of the modified NdFeB powder obtained in step (1) and 7 parts by weight of the modified tourmaline powder obtained in step (2) are added to 78 parts by weight of a polyester melt, mixed and stirred to obtain a spinning solution; the spinning solution is fed into a spinning head, and ejected from the spinning head into a coagulation bath at 48° C., the spinneret hole diameter of the spinning head is 0.14 mm, the concentration of sulfuric acid in the coagulation bath is 58 g / L, the concentration of zinc sulfate is 18 g / L, and the concentration of sodium sulfate is 120 g / L, and primary fibers are formed after coagulation, and the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the primary fibers is 140 m / min.

[0097] Example 5

[0098] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. Figure 1 As shown, the production method specifically comprises the following steps:

[0099] (1) Soaking NdFeB powder in a 30 wt % hydrochloric acid aqueous solution, the ratio of NdFeB powder to sulfuric acid aqueous solution is 10 g:1 L, soaking at 60 ° C for 50 min and filtering, washing the solid with water until neutral, and drying the solid to obtain acid-modified NdFeB powder; then, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution with a concentration of 0.5 g / mL, adding a 30 wt % ethyl orthosilicate ethanol solution to the NdFeB solution at a drop rate of 1 mL / min, the mass ratio of the acid-modified NdFeB powder to the ethyl orthosilicate is 1:2, and continuing after the addition is completed The mixture was mixed and stirred for 40 minutes to obtain a reaction solution, and ammonia water was added dropwise to the reaction solution to adjust the pH value of the reaction solution to 10, and the mixture was stirred until ethyl orthosilicate was hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and the mixture was dried at 70°C for 12 hours to obtain silicon-coated NdFeB powder; finally, the silicon-coated NdFeB powder was dispersed in acetone to form a dispersion solution of 0.5 g / mL, and a silane coupling agent KH570 was added to the dispersion solution and mixed and stirred for 2 hours, wherein the mass ratio of the silicon-coated NdFeB powder to the silane coupling agent KH570 was 1:0.05, and the modified NdFeB powder was obtained after suction filtration, washing and drying;

[0100] (2) mixing a titanate coupling agent and an alcohol aqueous solution in a mass ratio of 1:2.5 and heating the mixture to 50° C. to obtain a coupling agent solution; adding tourmaline powder and calcium stearate to the coupling agent solution, wherein the mass ratio of the tourmaline powder to the titanate coupling agent is 15:1, and the mass ratio of the tourmaline powder to the calcium stearate is 15:1.8, and mixing to obtain a mixed solution; heating the mixed solution to 70° C. under sealed conditions and stirring the mixture at a speed of 200 r / min to react for 40 minutes, so that the calcium stearate is coated on the surface of the tourmaline powder; after the reaction is completed, filtering, washing and drying the mixture to obtain a modified tourmaline powder;

[0101] (3) 15 parts by weight of the modified NdFeB powder obtained in step (1) and 10 parts by weight of the modified tourmaline powder obtained in step (2) are added to 80 parts by weight of a polyester melt, mixed and stirred to obtain a spinning solution; the spinning solution is fed into a spinning head, and ejected from the spinning head into a coagulation bath at 50° C., the spinneret hole diameter of the spinning head is 0.15 mm, the concentration of sulfuric acid in the coagulation bath is 60 g / L, the concentration of zinc sulfate is 20 g / L, and the concentration of sodium sulfate is 100 g / L, and primary fibers are formed after coagulation, and the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers, wherein the stretching speed of the primary fibers is 160 m / min.

[0102] Example 6

[0103] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. The difference from Embodiment 1 is that in step (3), the amount of modified NdFeB powder added is adjusted to 2 parts by weight, and the other process parameters and operating steps are exactly the same as those in Embodiment 1.

[0104] Example 7

[0105] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. The difference from Embodiment 1 is that in step (3), the amount of modified NdFeB powder added is adjusted to 18 parts by weight, and the other process parameters and operating steps are exactly the same as those in Embodiment 1.

[0106] Example 8

[0107] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. The difference from Embodiment 1 is that in step (3), the amount of modified tourmaline powder added is adjusted to 0.5 parts by weight, and the other process parameters and operating steps are exactly the same as those in Embodiment 1.

[0108] Example 9

[0109] This embodiment provides a method for producing environmentally friendly far-infrared negative ion fibers. The difference from Embodiment 1 is that in step (3), the amount of NdFeB powder-modified tourmaline powder added is adjusted to 15 parts by weight, and the other process parameters and operating steps are exactly the same as those in Embodiment 1.

[0110] Comparative Example 1

[0111] This comparative example provides a method for producing environmentally friendly far-infrared negative ion fibers, which differs from Example 1 in that step (1) is omitted, the NdFeB powder is not modified, and the unmodified NdFeB powder is subjected to step (3), and other process parameters and operating steps are exactly the same as those in Example 1.

[0112] Comparative Example 2

[0113] This comparative example provides a method for producing environmentally friendly far-infrared negative ion fibers, which differs from Example 1 in that step (2) is omitted, the tourmaline powder is not modified, and the unmodified tourmaline powder is subjected to step (3), and the other process parameters and operating steps are exactly the same as those of Example 1.

[0114] The negative ion generation concentration, far infrared emissivity and tensile strength of the environmentally friendly far infrared negative ion fibers prepared in Examples 1-9 and Comparative Examples 1-2 were tested, and the test results are shown in Table 1.

[0115] Table 1 Test results of environmentally friendly far-infrared negative ion fibers

[0116]

[0117]

[0118] It can be seen from the test data provided in Table 1 that the environmentally friendly far-infrared negative ion fibers prepared in Examples 1-5 have the effects of generating negative ions and emitting far-infrared rays. The clothes woven with such fibers can continuously stimulate negative ions to the human body when worn, so that the human body remains energetic. At the same time, since the environmentally friendly far-infrared negative ion fibers have excellent mechanical properties, they can still maintain a good wearing feeling after repeated washing, greatly extending the service life of the clothes.

[0119] It can be seen from the test data of Example 1, Example 6 and Example 7 that too high or too low addition amount of modified NdFeB powder will affect the negative ion generation concentration, far-infrared emissivity and tensile strength of the environmentally friendly far-infrared negative ion fiber.

[0120] It can be seen from the test data of Example 1, Example 8 and Example 9 that too high or too low addition amount of modified tourmaline powder will affect the negative ion generation concentration, far-infrared emissivity and tensile strength of the environmentally friendly far-infrared negative ion fiber.

[0121] It can be seen from the test data of Example 1 and Comparative Example 1 that the environmentally friendly far-infrared negative ion fiber prepared in Comparative Example 1 is because the NdFeB powder is not modified in Comparative Example 1, resulting in agglomeration of the NdFeB powder in the polyester matrix, thereby affecting the negative ion concentration, far-infrared emissivity and tensile strength of the environmentally friendly far-infrared negative ion fiber.

[0122] It can be seen from the test data of Example 1 and Comparative Example 2 that the environmentally friendly far-infrared negative ion fiber prepared in Comparative Example 2 is because the tourmaline powder is not modified in Comparative Example 2, resulting in agglomeration of the tourmaline powder in the polyester matrix, thereby affecting the negative ion generation concentration, far-infrared emissivity and tensile strength of the environmentally friendly far-infrared negative ion fiber.

[0123] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for producing environmentally friendly far-infrared negative ion fiber, characterized in that: The production method comprises: (I) soaking NdFeB powder in an acidic aqueous solution, filtering after soaking, washing the solid with water until neutral, and drying the solid to obtain acid-modified NdFeB powder; subsequently, dispersing the acid-modified NdFeB powder in deionized water to obtain a NdFeB solution, dropping an alcohol solution of ethyl orthosilicate into the NdFeB solution, mixing evenly after the dropping is completed to obtain a reaction solution, dropping ammonia water into the reaction solution and stirring until the ethyl orthosilicate is hydrolyzed to in-situ grow nano-silicon dioxide on the surface of the acid-modified NdFeB powder, and drying to obtain silicon-coated NdFeB powder; finally, dispersing the silicon-coated NdFeB powder in an organic solvent to form a dispersion, adding a silane coupling agent to the dispersion, mixing and stirring, filtering, washing and drying to obtain modified NdFeB powder; (II) mixing a titanate coupling agent with an alcohol aqueous solution and heating the mixture to obtain a coupling agent solution, adding tourmaline powder and calcium stearate to the coupling agent solution, mixing the mixture to obtain a mixed solution, heating the mixed solution under sealed conditions to react so that the calcium stearate is coated on the surface of the tourmaline powder, and after the reaction is completed, filtering, washing and drying the mixture to obtain a modified tourmaline powder; (III) adding the modified NdFeB powder obtained in step (I) and the modified tourmaline powder obtained in step (II) into a polyester melt, mixing and stirring to obtain a spinning solution; sending the spinning solution into a spinning head, spraying it out from the spinning head into a coagulation bath, and forming primary fibers after coagulation; the primary fibers are stretched, washed, oiled and dried to obtain the environmentally friendly far-infrared negative ion fibers.

2. The production method according to claim 1, characterized in that The environmentally friendly far-infrared negative ion fiber comprises the following components in parts by weight: 5-15 parts of modified NdFeB powder; 1-10 parts of modified tourmaline powder; Polyester 70-80 parts.

3. The production method according to claim 1, characterized in that In step (I), the mass fraction of the acidic aqueous solution is 20-30wt%; The acidic aqueous solution includes any one of a sulfuric acid aqueous solution, a nitric acid aqueous solution or a hydrochloric acid aqueous solution or a combination of at least two thereof; The immersion time of the NdFeB powder in the acidic aqueous solution is 40-50 minutes; The immersion temperature of the NdFeB powder in the acidic aqueous solution is 60-70°C.

4. The production method according to claim 1, characterized in that In step (I), the mass fraction of ethyl orthosilicate in the alcohol solution of ethyl orthosilicate is 20-30wt%; The mass ratio of the acid-modified NdFeB powder to tetraethyl orthosilicate is 1:(1-2); The dripping speed of the alcohol solution of tetraethyl orthosilicate is 0.5-1 mL / min; After the alcohol solution of ethyl orthosilicate is added dropwise, continue mixing and stirring for 30-40 minutes; Adding aqueous ammonia to the reaction solution dropwise to adjust the pH value of the reaction solution to 9-10; The drying temperature is 60-70°C; The drying time is 12-24 hours.

5. The production method according to claim 1, characterized in that: In step (I), the concentration of the silicon-coated NdFeB powder in the dispersion is 0.1-0.5 g / mL; The organic solvent includes any one of methanol, ethanol, toluene or acetone, or a combination of at least two thereof; The mass ratio of the silicon-coated NdFeB powder to the silane coupling agent is 1:(0.01-0.05); The mixing time of the dispersion and the silane coupling agent is 1-2 hours.

6. The production method according to claim 1, characterized in that: In step (II), the mass ratio of the titanate coupling agent to the alcohol aqueous solution is (0.8-1):(1.5-2.5); The titanate coupling agent is mixed with the alcohol aqueous solution and then heated to 40-50°C.

7. The production method according to claim 1, characterized in that: In step (II), the mass ratio of the tourmaline powder to the titanate coupling agent is (5-15):1; The mass ratio of the tourmaline powder to the calcium stearate is (5-15):(0.5-1.8).

8. The production method according to claim 1, characterized in that: In step (II), the heating temperature of the mixed solution is 60-70°C; The stirring speed of the mixed liquid is 100-200r / min; The reaction time of the mixed solution is 40-50 min.

9. The production method according to claim 1, characterized in that: In step (III), the temperature of the coagulation bath is 40-50°C; The coagulation bath comprises sulfuric acid, zinc sulfate, sodium sulfate and deionized water; The concentration of sulfuric acid in the coagulation bath is 50-60 g / L; The concentration of zinc sulfate in the coagulation bath is 15-20 g / L; The concentration of sodium sulfate in the coagulation bath is 100-200 g / L.

10. The production method according to claim 1, characterized in that: In step (III), the drafting speed of the spun fiber is 20-160 m / min; The diameter of the spinneret hole of the spinning head is 0.08-0.15 mm.

Citation Information

Patent Citations

  • Far infrared anionic magnetic fiber and manufacturing method thereof

    CN101871139A

  • Multifunctional tourmaline health-care material and preparation method thereof

    CN102060471A

  • Production process of novel health fiber containing various functional elements

    CN103849955A

  • Yarn made by blending fiber having anions and far-infrared function and hemp-cotton fiber

    CN106049070A

  • Neodymium iron boron magnetic composite material and preparation method thereof

    CN114806157A

Cited By

  • Dual confinement ionic conductive fiber and preparation method and application thereof

    CN122406397A