A method for improving permanent magnet loss performance by ion implantation and permanent magnet
The Sm2Co17 permanent magnet material is processed through Bi and N common ion implantation process, which solves the problem of high permanent magnet loss in high-speed motors, reduces temperature rise and improves service life, achieves higher performance indicators, and avoids expensive Use of materials.
Patent Information
- Application Number
- CN202410595872.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The permanent magnets in high-speed motors are prone to heat up under harsh working conditions, resulting in irreversible demagnetization of the magnets, high losses, and affecting service life and performance.
Bi and N common ion implantation process is adopted, and the surface of Sm2Co17 rare earth permanent magnet material is polished, polished and ultrasonic cleaning, and Bi and N ions are implanted in the vacuum cavity, and then annealed to reduce magnet losses.
It significantly reduces the loss of permanent magnets, reduces temperature rise, improves its performance and service life under harsh operating conditions, while avoiding the need for expensive rare earth materials.
Smart Images

Figure BDA0004838929470000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ion implantation technology, and in particular to a method for improving the loss performance of a permanent magnet by ion implantation and a permanent magnet. Background Art
[0002] The loss distribution of conventional motors is as follows: (1) The copper loss of the stator winding accounts for 34% of the total loss. (2) The iron loss of the stator core accounts for 18% of the total loss. If the motor is running in an overload state, the stator core will also have magnetic saturation loss, so the stator iron loss will increase a lot. (3) The rotor loss accounts for 24% of the total loss. If the motor is running in an overload state, the iron loss of the rotor core will also increase a lot. (4) Traditional motors are all radial flux, the magnetic path is long and the magnetic loss is large. (5) The fan blades at both ends of the rotor of this motor and the large heat dissipation fan blades installed at the tail of the motor will also generate wind friction loss when the motor is running, accounting for 10% of the total loss. (6) Stray losses account for 14% of the losses of this motor.
[0003] Among high-speed motors, permanent magnet motors are widely used due to their simple structure, high power density, no excitation loss, high efficiency, etc. However, harsh working conditions such as high speed and heavy load can easily cause the motor to heat up and cause irreversible demagnetization of the magnet, which ultimately leads to the serious consequence that the motor cannot operate.
[0004] Eddy current loss refers to the energy loss caused by the induced current in the conductor when the conductor moves in a non-uniform magnetic field or is in a magnetic field that changes with time. The closed current lines formed inside the conductor are called eddy currents (also known as Foucault currents). The size of eddy current loss is related to factors such as the way the magnetic field changes, the movement of the conductor, the geometric shape of the conductor, the magnetic permeability and electrical conductivity of the conductor.
[0005] The present invention performs Bi and N co-ion implantation on SmCo permanent magnets, thereby reducing magnet loss, reducing the temperature rise under working conditions, and improving the service life and performance index of the magnets. Summary of the invention
[0006] The present invention provides a method for improving the loss performance of a permanent magnet by ion implantation and a permanent magnet, so as to solve the technical problem of high motor loss in the prior art. Specifically:
[0007] A method for improving the loss performance of a permanent magnet by ion implantation comprises the following steps:
[0008] After grinding the surface of the permanent magnet sample with sandpaper, polishing until the surface roughness is less than 0.2 μm, then placing the permanent magnet with the polished surface facing upward in a beaker filled with alcohol for ultrasonic cleaning, taking out the sample and drying it, fixing the sample on a target plate and placing it in a vacuum chamber equipped with an ion implantation system, the ion implantation system including a Bi ion implantation source and a N ion implantation source;
[0009] The vacuum degree was adjusted and Bi ion implantation was performed at room temperature with an implantation dose of 5×10 14 -5×10 15 / cm 2 , energy is 100-200keV; N ion implantation is carried out at room temperature, the implantation dose is 1×1014-1×1015 / cm2, and the energy is 50-100keV;
[0010] After the ion implantation, an annealing treatment is performed at a temperature of 450° C. to 490° C. for 4 to 6 hours.
[0011] Furthermore, the permanent magnet sample is Sm2Co17 rare earth permanent magnet material.
[0012] Furthermore, the permanent magnet sample is prepared by powder metallurgy process.
[0013] Furthermore, the surface of the permanent magnet sample is polished using sandpaper with 200 to 1000 meshes.
[0014] Furthermore, the surface is polished using a polishing agent in a mechanical polishing machine.
[0015] Furthermore, ultrasonic cleaning was performed for 20 minutes.
[0016] Furthermore, the vacuum degree of the vacuum chamber is adjusted to 0.1-0.4 Pa before ion implantation.
[0017] Furthermore, the vacuum degree during the annealing process is less than 10 -2 Pa.
[0018] A permanent magnet modified by the method.
[0019] Furthermore, the permanent magnet sample is a Sm2Co17 rare earth permanent magnet material, which is prepared by a powder metallurgy process.
[0020] The method of ion implantation provided in this scheme to improve the loss performance of permanent magnets adopts a Bi and N ion co-implantation process to reduce the loss of permanent magnets.
[0021] After grinding the surface of the permanent magnet sample with sandpaper of 200 to 1000 mesh, the surface was polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2 μm. Thereafter, the polished surface of the permanent magnet was placed in a beaker containing alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, the sample was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0022] The vacuum degree of the vacuum chamber was adjusted to 0.1-0.4 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 5×10 14 -5×10 15 / cm 2 , the energy is 100-200keV; N ion implantation is performed at room temperature, and the implantation dose is 1×10 14 -1×10 15 / cm 2 , energy is 50-100keV,
[0023] After ion implantation, annealing treatment is performed at a temperature of 450°C-490°C for 4-6 hours; the vacuum degree is less than 10 -2 Pa.
[0024] The permanent magnet sample is Sm2Co17 rare earth permanent magnet material, which is prepared by powder metallurgy process.
[0025] Performance test: The treated permanent magnet sample is placed at 20°C, and the sample length and resistance per unit length are measured. The resistance performance is tested according to the GB / T6146-2010 precision resistance permanent magnet resistivity test method. The magnetic performance is tested according to the GB / T3217 permanent magnet (hard magnetic) material magnetic test method. The permanent magnet sample is placed at 500Vac, 50Hz, 20°C for 3 minutes, and then its surface temperature rise is measured.
[0026] By ion implantation of Bi and N ions, the surface conductivity of the permanent magnet is reduced and the eddy current phenomenon is significantly weakened. In addition, due to the precipitation of Bi and N compounds at the grain boundaries, the pinning effect is conducive to maintaining higher magnetic properties. In addition, since the present invention avoids the use of relatively expensive rare earth materials, its application prospects are broader. DETAILED DESCRIPTION
[0027] Embodiment 1:
[0028] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0029] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 1×10 15 / cm 2, the energy is 150keV; N ion implantation is performed at room temperature, and the implantation dose is 5×10 14 / cm 2 , energy is 75keV,
[0030] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0031] The prepared samples were tested.
[0032] Embodiment 2:
[0033] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0034] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 5×10 15 / cm 2 , the energy is 200keV; N ion implantation is performed at room temperature, and the implantation dose is 1×10 15 / cm 2 , energy is 100keV,
[0035] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0036] The prepared samples were tested.
[0037] Embodiment 3:
[0038] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0039] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 5×10 15 / cm 2 , the energy is 100keV; N ion implantation is performed at room temperature, and the implantation dose is 1×10 14 / cm 2 , energy is 50keV,
[0040] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0041] The prepared samples were tested.
[0042] Comparative Example 1:
[0043] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2 μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source.
[0044] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 1×10 15 / cm 2 , energy is 150keV,
[0045] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0046] The prepared samples were tested.
[0047] Comparative Example 2:
[0048] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2 μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a N ion implantation source.
[0049] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and N ion implantation was performed at room temperature with an implantation dose of 5×10 14 / cm 2 , energy is 75keV,
[0050] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0051] The prepared samples were tested.
[0052] Comparative Example 3:
[0053] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0054] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 1×10 15 / cm 2 , the energy is 150keV; N ion implantation is performed at room temperature, and the implantation dose is 5×10 15 / cm 2 , energy is 150keV,
[0055] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0056] The prepared samples were tested.
[0057] Comparative Example 4:
[0058] The Sm2Co17 rare earth permanent magnet material prepared by powder metallurgy was polished with sandpaper of 200 to 1000 meshes, and then polished with a polishing agent in a mechanical polisher until the surface roughness was less than 0.2μm. Thereafter, the permanent magnet was placed with the polished surface facing up in a beaker filled with alcohol for ultrasonic cleaning for 20 minutes. After the sample was taken out and dried, it was fixed on a target plate and placed in a vacuum chamber equipped with an ion implantation system, which included a Bi ion implantation source and a N ion implantation source.
[0059] The vacuum degree of the vacuum chamber was adjusted to 0.2 Pa, and Bi ion implantation was performed at room temperature with an implantation dose of 1×10 15 / cm 2 , the energy is 150keV; N ion implantation is performed at room temperature, and the implantation dose is 5×10 13 / cm 2 , energy is 50keV,
[0060] After ion implantation, annealing treatment is performed at 470°C for 5 hours; the vacuum degree is less than 10 -2 Pa.
[0061] The prepared samples were tested.
[0062] Table 1 Test results
[0063]
Claims
1. A method for improving the loss performance of permanent magnets by ion implantation. Features: The steps include: After grinding the surface of the permanent magnet sample with sandpaper, polishing until the surface roughness is less than 0.2 μm, then placing the permanent magnet with the polished surface facing upward in a beaker filled with alcohol for ultrasonic cleaning, taking out the sample and drying it, fixing the sample on a target plate and placing it in a vacuum chamber equipped with an ion implantation system, the ion implantation system including a Bi ion implantation source and a N ion implantation source; The vacuum degree was adjusted and Bi ion implantation was performed at room temperature with an implantation dose of 5×10 14 -5×10 15 / cm 2 , the energy is 100-200keV; N ion implantation is performed at room temperature, and the implantation dose is 1×10 14 -1×10 15 / cm 2 , energy is 50-100keV; After ion implantation, annealing is performed at a temperature of 450°C to 490°C for 4 to 6 hours; The permanent magnet sample is Sm2Co17 rare earth permanent magnet material; The permanent magnet samples were prepared by powder metallurgy process.
2. The method according to claim 1, Features: Use 200-1000 mesh sandpaper to grind the surface of the permanent magnet sample.
3. The method according to claim 1, Features: The surface is polished using a polishing agent in a mechanical polishing machine.
4. The method according to claim 1, Features: Ultrasonic cleaning for 20 minutes.
5. The method according to claim 1, Features: Before ion implantation, the vacuum degree of the vacuum chamber was adjusted to 0.1-0.4 Pa.
6. The method according to claim 1, Features: The vacuum degree during annealing is less than 10 -2 Pa.
7. The permanent magnet modified by the method according to claim 1.