Bipolar integrated circuit, manufacturing method thereof and driver

By adjusting the process parameters of bipolar integrated circuits, especially the re-diffusion conditions of the base and emitter regions, the problems of low VOH and large IOZ are solved, the electrical parameters are improved, and the normal operation of the driver is ensured.

CN118398558BActive Publication Date: 2024-10-15TIANSHUI TIANGUANG SEMICON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410851544.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

In drivers produced using ordinary bipolar integrated circuit manufacturing processes, the high-level output voltage VOH is relatively low and the static high-resistance current IOZ is relatively large, which cannot meet the design requirements, resulting in insufficient and high output voltage of the device in the high-level state. The leakage current is too high in the resistive state.

Method used

By cyclically adjusting process parameters during the manufacturing process of bipolar integrated circuits, including the re-diffusion temperature and time of the base and emitter areas, combined with the VOH and IOZ test results, the process parameters are adjusted to increase the VOH value and reduce the IOZ value to ensure electrical parameters. Meet the preset requirements.

Benefits of technology

By increasing the base junction depth and emitter area amplification, the high-level output voltage VOH is significantly increased and the static high-resistance current IOZ is reduced, ensuring the normal use of the driver and meeting the design requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398558B_ABST
    Figure CN118398558B_ABST
Patent Text Reader

Abstract

The present invention provides a bipolar integrated circuit and a manufacturing method and driver thereof, and specifically relates to the technical field of integrated circuit manufacturing. The manufacturing method comprises: cyclically executing the following steps in the manufacturing process of the bipolar integrated circuit: manufacturing the bipolar integrated circuit based on the current process parameters, the process parameters comprising a first temperature and a first time, the first temperature being used to control the temperature of the silicon wafer after the base region pre-diffusion when the base region is re-diffused, and the first time being used to control the time of phosphorus pre-diffusion when the silicon wafer is pre-diffused in the emitter region; performing a VOH test and / or an IOZ test on the bipolar integrated circuit; when the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, modifying the first temperature and / or the first time in the process parameters according to the preset rules to obtain new process parameters, and using the new process parameters as the current process parameters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of integrated circuit manufacturing, and in particular to a bipolar integrated circuit and a manufacturing method and a driver thereof. Background Art

[0002] The driver is composed of two identical digital logic circuits arranged in a symmetrical form, so that the purpose of balanced driving can be achieved. The driver manufactured using low-power Schottky technology has the characteristics of 5V single power supply, TTL level compatibility, complementary output, and high impedance when the power is disconnected. Its three-state output has the ability to drive balanced transmission such as twisted pair or parallel line transmission lines to output large current, and can be in high impedance when the power is disconnected. Low-power Schottky can reduce power consumption without sacrificing speed, and is widely used in electronic devices such as portable computers, battery-powered systems, power generators, terminals, modems, etc.

[0003] When the driver is produced by ordinary bipolar integrated circuit manufacturing process, after cleaning, epitaxy, oxidation, base diffusion, emitter diffusion, photolithography, metallization, passivation and other processes, the high-level output voltage VOH will be low and the static high-impedance current (High Impedance Currents, IOZ, including high-level current IOZH and low-level current IOZL) will be large during the driver test. If VOH is low, when the driver is used, when the device is in a high-level state, the minimum voltage on the output pin cannot meet the application requirements; if IOZ is large, when the driver is working, when the pin is in a high-impedance state, the device impedance cannot meet the design requirements and the pin leakage current is too high.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for manufacturing a bipolar integrated circuit to alleviate the technical problems of low electrical parameter high-level output voltage VOH and large electrical parameter static high-resistance current in the prior art.

[0006] In order to solve the above technical problems, the present invention particularly adopts the following technical solutions:

[0007] The present invention provides a method for manufacturing a bipolar integrated circuit, comprising:

[0008] The following steps are repeated in the manufacturing process of bipolar integrated circuits:

[0009] Manufacturing a bipolar integrated circuit based on current process parameters, the process parameters including a first temperature and a first time, wherein the process of manufacturing the bipolar integrated circuit includes performing base region pre-diffusion on a silicon wafer, performing base region re-diffusion on the silicon wafer after the base region pre-diffusion, performing emitter region pre-diffusion on the silicon wafer, and performing emitter region re-diffusion on the silicon wafer after the emitter region pre-diffusion;

[0010] The first temperature is used to control the temperature of the base region re-diffusion of the silicon wafer after the base region pre-diffusion, and the process of the emitter region pre-diffusion of the silicon wafer includes phosphorus pre-diffusion through a small amount of nitrogen;

[0011] The first time is used to characterize the duration of phosphorus pre-diffusion when the emitter region pre-diffusion is performed on the silicon wafer;

[0012] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0013] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first temperature and / or the first time in the process parameters are modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0014] In an optional implementation of the first aspect, it also includes:

[0015] When the VOH test result or the IOZ test result of the bipolar integrated circuit meets the preset requirement, the current process parameter is maintained.

[0016] In an optional implementation manner of the first aspect, when a VOH test result or an IOZ test result of the bipolar integrated circuit does not meet a preset requirement, the method includes:

[0017] A VOH test result of the bipolar integrated circuit is less than a first threshold value of the VOH test high level output voltage;

[0018] Or, the IOZ test result of the bipolar integrated circuit is greater than a second threshold value of the IOZ test high-resistance current.

[0019] In an optional implementation manner of the first aspect, the preset rule includes:

[0020] A first positive correlation functional relationship between the first parameter and the second parameter;

[0021] A second positive correlation function relationship between the third parameter and the fourth parameter;

[0022] The first parameter is used to indicate the absolute value of the difference between the VOH test result and the first threshold;

[0023] The third parameter is used to indicate the absolute value of the difference between the IOZ test result and the second threshold value;

[0024] The second parameter and the fourth parameter are respectively used to indicate the adjustment step size;

[0025] The modifying the first temperature and the first time in the process parameters according to the preset rule includes:

[0026] Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit;

[0027] Determine a first adjustment step size based on the first difference and the first positive correlation function relationship;

[0028] Determine a second adjustment step size based on the second difference and the second positive correlation function relationship;

[0029] Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size;

[0030] Based on the current process parameters and the target adjustment step, new process parameters are determined.

[0031] In an optional implementation manner of the first aspect, when the VOH test result or the IOZ test result of the bipolar integrated circuit meets the preset requirements, the method includes:

[0032] The VOH test result of the bipolar integrated circuit is not less than the first threshold;

[0033] Furthermore, an IOZ test result of the bipolar integrated circuit is not greater than the second threshold.

[0034] In an optional implementation of the first aspect, before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes:

[0035] Determine initial process parameters; the initial process parameters include: when the base region is re-diffused, heat-treating the silicon wafer after the base region pre-diffusion treatment in dry oxygen, wet oxygen, and dry oxygen atmospheres at a first temperature in sequence;

[0036] The first temperature is 1040°C to 1060°C;

[0037] Manufacturing a bipolar integrated circuit based on the initial process parameters;

[0038] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0039] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first temperature in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0040] In an optional implementation of the first aspect, before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes:

[0041] Determine initial process parameters; the initial process parameters include: when the emitter region is pre-diffused, the silicon wafer after the base region is re-diffused is pre-diffused with phosphorus at the first time;

[0042] The first time is 3 minutes to 6 minutes;

[0043] Manufacturing a bipolar integrated circuit based on the initial process parameters;

[0044] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0045] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first time in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0046] In an optional implementation manner of the first aspect, when a VOH test result or an IOZ test result of the bipolar integrated circuit does not meet a preset requirement, a first parameter is determined by using the VOH test result and the first threshold value;

[0047] Determine the second parameter according to the IOZ test result and the second threshold value;

[0048] Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit;

[0049] Determine a first adjustment step size based on the first difference and the first positive correlation function relationship;

[0050] Determine a second adjustment step size based on the second difference and the second positive correlation function relationship;

[0051] Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size;

[0052] The first temperature of the base region re-diffusion heat treatment or the first time of phosphorus diffusion during the emitter region pre-diffusion is reset until the VOH test result and / or the IOZ test result of the bipolar integrated circuit meet the preset requirements.

[0053] In an optional implementation manner of the first aspect, the preset requirement of the VOH test is VOH ≥ 2.75V, and the first threshold is 2.75V;

[0054] The preset requirement of the IOZ test is ≤10 μA, and the second threshold is 10 μA.

[0055] A second aspect of the present invention provides a driver, comprising a bipolar integrated circuit manufactured by the manufacturing method described in the first aspect.

[0056] Compared with the prior art, the present invention has at least the following beneficial effects:

[0057] The manufacturing method of the bipolar integrated circuit provided by the present invention corrects the first temperature and / or the first time through the VOH test result or the IOZ test result, increases the base junction depth, and thus increases the VOH value. At the same time, because the base junction depth changes, the change in base diffusion directly affects the emission region diffusion, and it is necessary to increase the phosphorus diffusion source time, so that the manufactured bipolar integrated circuit increases the electrical parameter high-level output voltage VOH and reduces the electrical parameter static high-resistance current. When the bipolar integrated circuit is applied to a driver, the normal use of the driver is ensured. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0059] Figure 1 Output high level test condition for gate circuit;

[0060] Figure 2 The figure is a flow chart of the manufacturing method of the bipolar integrated circuit of the present invention. DETAILED DESCRIPTION

[0061] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, but not all of the embodiments. The components of the embodiment of the present invention can be arranged and designed in various different configurations.

[0062] High Impedance Currents (IOZH / IOZL), IOZL refers to the leakage current (I) generated on an output pin (O) in a high impedance state (Z) when a low level (L) is applied to the output pin (O); IOZH refers to the leakage current (I) generated on the output pin (O) in a high impedance state (Z) when a high level (H) is applied to the output pin (O). The purpose of the IOZ test is to ensure that when the device output pin is preset to a high impedance state, its output impedance is high enough, or that the pin can be in the "off" state. In essence, it is to ensure that the impedance of the output pin when it is turned off meets the design requirements to ensure that the pin will not generate leakage current higher than that defined in the specification.

[0063] According to the characteristics of the gate circuit output terminal, the gate circuit output high level test conditions are as follows Figure 1 shown.

[0064] The high level VOH formula is as follows:

[0065]

[0066] Among them, VOH is high level; Vcc min is the minimum power supply voltage; R is the base resistance; ICER3 is the CE leakage current of T3 tube in the off state; IR2 is the reverse leakage current of diode; IR4 is the collector current of T4 tube; ICER6 is the CE leakage current of T6 tube; IL is the load current; VBE4 is the EB junction voltage of T4 tube; VBE5 is the EB junction voltage of T5 tube; β4 is the gain of the diffusion process control of the emitter region of T4 tube; β5 is the gain of the diffusion process control of the emitter region of T5 tube.

[0067] According to the high-level VOH formula, the base resistance R of the device and the amplification factor β controlled by the emitter diffusion process have a great influence on the high level. If the base resistance is too large or the emitter amplification factor is too small, the VOH will be too low.

[0068] As mentioned above, the high-resistance current IOZ test is essentially to determine whether the impedance of the output pin when it is turned off meets the design requirements, so as to ensure that the pin will not generate leakage current higher than that defined in the specification. In the manufacturing process, the device resistance is reduced by increasing the base junction depth during the base diffusion process, and the emitter region amplification factor is increased by controlling the emitter diffusion process and increasing the phosphorus diffusion time, which can improve the device's double junction characteristics, harden the breakdown, and reduce the device leakage current during the test, thereby solving the problem of low output voltage in the VOH test and large high-resistance current in the IOZ test.

[0069] The present invention provides a method for manufacturing a bipolar integrated circuit, such as Figure 2 As shown, including:

[0070] The following steps are repeated in the manufacturing process of bipolar integrated circuits:

[0071] Manufacturing a bipolar integrated circuit based on current process parameters, the process parameters including a first temperature and a first time, wherein the process of manufacturing the bipolar integrated circuit includes performing base region pre-diffusion on a silicon wafer, performing base region re-diffusion on the silicon wafer after the base region pre-diffusion, performing emitter region pre-diffusion on the silicon wafer, and performing emitter region re-diffusion on the silicon wafer after the emitter region pre-diffusion;

[0072] The first temperature is used to control the temperature of the base region re-diffusion of the silicon wafer after the base region pre-diffusion, and the process of the emitter region pre-diffusion of the silicon wafer includes phosphorus pre-diffusion through a small amount of nitrogen;

[0073] The first time is used to control the phosphorus pre-diffusion time when the emitter region pre-diffusion is performed on the silicon wafer;

[0074] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0075] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first temperature and / or the first time in the process parameters are modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0076] The current method for preparing a bipolar integrated circuit includes the following steps:

[0077] A P-type silicon wafer substrate is provided, and the substrate is initially oxidized, photolithographically processed, and arsenic diffused and implanted to form an N+ buried layer on the silicon wafer to obtain a first silicon wafer.

[0078] Forming an N-type epitaxial layer with a thickness of 3 to 5 μm on the first silicon wafer to obtain a second silicon wafer;

[0079] Performing isolation oxidation and isolation diffusion on the second silicon wafer to form a P-type isolation region to obtain a third silicon wafer;

[0080] The third silicon wafer is subjected to phosphorus bridge oxidation, photolithography, phosphorus bridge pre-diffusion, and phosphorus bridge re-diffusion to obtain a fourth silicon wafer;

[0081] Performing base region pre-diffusion and base region re-diffusion on the fourth silicon wafer to form a base region with a junction depth of 2 to 3 μm, thereby obtaining a fifth silicon wafer;

[0082] Testing the sheet resistance of the fifth silicon wafer, and performing oxidation, photolithography, emitter region pre-diffusion, and emitter region re-diffusion on the fifth silicon wafer having a sheet resistance of 200 Ω / □ to 220 Ω / □ to form an emitter region and a collector region with a junction depth of 1.5 to 2.5 μm to obtain a sixth silicon wafer;

[0083] The sixth silicon wafer is subjected to photolithography, metal electrode deposition and passivation to obtain the bipolar integrated circuit.

[0084] It should be noted that, in the present application, the terms "first", "second", "third", "fourth", "fifth", "sixth", "seventh" and "eighth" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0085] The purpose of pre-diffusion is to form high-concentration doping, and re-diffusion is the process of diffusing the high-concentration doping area to form a base region to achieve the required base junction depth.

[0086] The emission region diffusion includes the following steps:

[0087] The method multiple β of the fifth silicon wafer after the emitter region diffusion pre-diffusion treatment is tested, and the silicon wafer with β satisfying 70-90 is subjected to emitter region re-diffusion to obtain a sixth silicon wafer.

[0088] As the temperature of the base region increases, the base region junction depth changes accordingly. The change in base region diffusion directly affects the emitter region diffusion. The β value is increased by increasing the phosphorus diffusion source time.

[0089] Optionally, the emitter region pre-diffusion includes diffusing the silicon wafer in a phosphorus-containing gas atmosphere at 1075°C~1085°C for 3~10 min, and heat treating it in a nitrogen atmosphere at 390°C~410°C for 30~40 min, and the nitrogen flow rate of the nitrogen atmosphere is 5L / min.

[0090] The silicon wafer is diffused with phosphorus in a phosphorus-containing atmosphere to form an N-type on the surface of the silicon wafer, so that the phosphorus source and the oxygen in the diffusion furnace tube react to generate phosphorus pentoxide vapor, which is converted into phosphorus atoms and surface silicon glass (PSG) during phosphorus diffusion. Phosphorus enters the silicon as an n-type substitutional impurity; after diffusion, it is heat treated in a nitrogen atmosphere.

[0091] The high-level output voltage of the bipolar integrated circuit obtained by the present invention is not less than 2.75V, and the static high-resistance current is not more than 10μA. The bipolar integrated circuit device comprises a P-type silicon wafer substrate, and an N+ buried layer, an N-type epitaxial layer and an insulating layer sequentially grown on the silicon wafer substrate, wherein the epitaxial layer is provided with a base region, an emitter region, a collector region, a P-type isolation region and a phosphorus bridge region, the P-type isolation region runs through the N-type epitaxial layer and extends to the P-type silicon wafer substrate, the silicon wafer substrate is 400-500μm thick, the epitaxial layer is 3-5μm thick, the base region junction depth is 2-3μm, and the emitter region junction depth is 1.5-2.5μm.

[0092] In an optional implementation of the first aspect, it also includes:

[0093] When the VOH test result or the IOZ test result of the bipolar integrated circuit meets the preset requirement, the current process parameter is maintained.

[0094] In an optional implementation manner of the first aspect, when a VOH test result or an IOZ test result of the bipolar integrated circuit does not meet a preset requirement, the method includes:

[0095] A VOH test result of the bipolar integrated circuit is less than a first threshold value of the VOH test high level output voltage;

[0096] Or, the IOZ test result of the bipolar integrated circuit is greater than a second threshold value of the IOZ test high-resistance current.

[0097] In an optional implementation manner of the first aspect, the preset rule includes:

[0098] A first positive correlation functional relationship between the first parameter and the second parameter;

[0099] A second positive correlation function relationship between the third parameter and the fourth parameter;

[0100] The first parameter is used to indicate the absolute value of the difference between the VOH test result and the first threshold;

[0101] The third parameter is used to refer to the absolute value of the difference between the IOZ test result and the second threshold value;

[0102] The second parameter and the fourth parameter are used to indicate the adjustment step size;

[0103] The modifying the first temperature and the first time in the process parameters according to the preset rule includes:

[0104] Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit;

[0105] Determine a first adjustment step size based on the first difference and the first positive correlation function relationship;

[0106] Determine a second adjustment step size based on the second difference and the second positive correlation function relationship;

[0107] Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size;

[0108] Based on the current process parameters and the target adjustment step, new process parameters are determined.

[0109] In an optional implementation manner of the first aspect, when the VOH test result or the IOZ test result of the bipolar integrated circuit meets the preset requirements, the method includes:

[0110] The VOH test result of the bipolar integrated circuit is not less than the first threshold;

[0111] Furthermore, an IOZ test result of the bipolar integrated circuit is not greater than the second threshold.

[0112] In an optional implementation of the first aspect, before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes:

[0113] Determine initial process parameters; the initial process parameters include: when the base region is re-diffused, heat-treating the silicon wafer after the base region pre-diffusion treatment in dry oxygen, wet oxygen, and dry oxygen atmospheres at a first temperature in sequence;

[0114] The first temperature is 1040°C to 1060°C;

[0115] Manufacturing a bipolar integrated circuit based on the initial process parameters;

[0116] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0117] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first temperature in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0118] Optionally, the heat treatment time ratio of the dry oxygen, wet oxygen and dry oxygen atmosphere is 2:30~40:2, the dry oxygen atmosphere has an oxygen flow rate of 2~4L / min, and the wet oxygen atmosphere has an oxygen flow rate of 2~4L / min and a water flow rate of 5~7mL / min.

[0119] In the present invention, dry oxygen and wet oxygen are used to adjust the oxygen concentration, thereby adjusting the quality of the oxide layer and controlling the sheet resistance of the semiconductor product. If the sheet resistance value is too low, oxygen can continue to be introduced to form an oxide layer to reduce the resistance; if the sheet resistance value is higher than the required value, the semiconductor semi-finished product cannot be used. Therefore, during the regulation process, when the sheet resistance value is close to the target value, wet oxygen is used for oxidation, so that the oxygen concentration is relatively low and the sheet resistance value can be accurately reduced.

[0120] In an optional implementation manner of the first aspect, the VOH test result or the IOZ test result of the bipolar integrated circuit not meeting the preset requirement further comprises:

[0121] The VOH test result of the bipolar integrated circuit is greater than a third threshold value of the VOH test high level output voltage;

[0122] Or, the IOZ test result of the bipolar integrated circuit is less than a fourth threshold value of the IOZ test high-resistance current.

[0123] If these two values ​​are too large, it may mean that the base resistance R of the device and the amplification factor β of the emitter diffusion process control are redundant and can be adjusted appropriately to shorten the overall production cycle.

[0124] In an optional implementation manner of the first aspect, the VOH test result needs to be greater than a first threshold, and the upper limit is not specifically limited.

[0125] In an optional implementation of the first aspect, the first threshold is 2.75V.

[0126] In an optional implementation manner of the first aspect, the preset requirement of the IOZ test needs to be less than the second threshold, and the lower limit is not specifically limited.

[0127] In an optional implementation of the first aspect, the second threshold is 10 μA.

[0128] In an optional implementation of the first aspect, before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes:

[0129] Determine initial process parameters; the initial process parameters include: when the emitter region is pre-expanded, the silicon wafer after the base region is re-diffused is pre-diffused with phosphorus at the first time;

[0130] The first time is 3 minutes to 6 minutes;

[0131] Manufacturing a bipolar integrated circuit based on the initial process parameters;

[0132] Performing a VOH test and / or an IOZ test on the bipolar integrated circuit;

[0133] When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first time in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

[0134] In an optional implementation manner of the first aspect, when a VOH test result or an IOZ test result of the bipolar integrated circuit does not meet a preset requirement, a first parameter is determined by using the VOH test result and the first threshold value;

[0135] Determine the second parameter according to the IOZ test result and the second threshold value;

[0136] Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit;

[0137] Determine a first adjustment step size based on the first difference and the first positive correlation function relationship;

[0138] Determine a second adjustment step size based on the second difference and the second positive correlation function relationship;

[0139] Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size;

[0140] The first temperature of the base region re-diffusion heat treatment or the first time of phosphorus diffusion during the emitter region pre-diffusion is reset until the VOH test result and / or the IOZ test result of the bipolar integrated circuit meet the preset requirements.

[0141] In an optional implementation manner of the first aspect, the preset requirement of the VOH test is VOH ≥ 2.75V, and the first threshold is 2.75V;

[0142] The preset requirement of the IOZ test is ≤10 μA, and the second threshold is 10 μA.

[0143] A second aspect of the present invention provides a driver, comprising a bipolar integrated circuit manufactured by the manufacturing method described in the first aspect.

[0144] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0145] Example 1

[0146] This embodiment provides a method for manufacturing a bipolar integrated circuit, and the specific steps are as follows:

[0147] 1. The first bipolar integrated circuit was prepared

[0148] a. Choose P type <111> The silicon wafer is used as the substrate silicon wafer, wherein the diameter of the silicon wafer is 76.2 mm, the thickness is 450 μm, and the resistivity is 10.5 (Ω.cm); the P-type <111> The silicon wafers have passed the inspection and the surface has been polished;

[0149] b. Cleaning of substrate silicon wafers: The substrate silicon wafers are cleaned with a cleaning solution of H2SO4: H2O2 = 3:1 at a temperature of 130°C and a cleaning solution of HCL:H2O2:H2O = 1:1:5 at a temperature of 100°C for 10 minutes each. The cleaned substrate silicon wafers are rinsed with water for 10 minutes, dried and sent for inspection;

[0150] c. Perform initial oxidation process on substrate silicon wafers: put qualified silicon wafers into quartz boat, then move the boat into the quartz tube furnace mouth, cover the ground mouth, and start the program; program operation: the quartz boat moves into the constant temperature zone of the quartz tube at a boat speed of 14cm / min, oxygen is introduced at a base temperature of 800℃, and the temperature is raised to the process temperature of 1120℃ at a rate of 10℃ per minute. At a constant temperature of 1120℃, the process is operated with the process conditions of "10 minutes of dry oxygen + 85 minutes of wet oxygen + 10 minutes of dry oxygen", and then the temperature is lowered to 800℃ at a rate of 10℃ per minute. The oxygen flow rate during the entire operation is 5L / min, and the water flow rate is 6ml / min, and the program operation ends. Remove the ground mouth, withdraw the boat, and use a boat speed of 14cm / min to test the oxide layer thickness of the sample. If it meets the process requirements and passes the inspection, the silicon wafer on the quartz boat is placed in a silicon wafer box;

[0151] d. Photolithography is performed on the substrate silicon wafer with the oxide layer after completing step c, wherein the steps are as follows:

[0152] ① Glue coating: The viscosity of the photoresist is 60SC, and the photoresist and solvent are diluted according to a ratio of 3:1, and the coating thickness is 7000Å;

[0153] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 115°C for 10 minutes;

[0154] ③ Alignment: Place a special mask on the photolithography machine, expose the substrate silicon wafer under the mercury lamp of the photolithography machine for 10±1 seconds, so that the mask pattern is imaged on the surface of the substrate silicon wafer;

[0155] ④ Development and fixing: first develop with xylene for 10 seconds, then fix with butyl acetate for 10 seconds;

[0156] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140℃ for 30 minutes;

[0157] ⑥ Oxide layer corrosion: The hardened substrate silicon wafer is corroded with a 6:1 H2O:NH4F etching solution for 3 minutes;

[0158] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in a 3:1 H2SO4:H2O2 soaking solution for 10 minutes to remove the photoresist;

[0159] f. Arsenic diffusion process: After arsenic is injected into the silicon wafer that has completed photolithography and passed the inspection, it is placed in a diffusion furnace at a temperature of 1200℃ and N2 is passed through to carry out an annealing and diffusion process for 360 minutes.

[0160] g. N-type epitaxy: A 3.8μm epitaxial layer was grown in an epitaxial furnace at a temperature of 1180°C. The square resistance test showed that the data met the process requirements and passed the inspection.

[0161] h. Isolation oxidation process:

[0162] Put the qualified silicon wafers into the quartz boat, and then move the boat to the quartz tube furnace mouth, cover the ground mouth, and move the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. At the base temperature of 800℃, oxygen is introduced, and the temperature is raised to the process temperature of 1090℃ at 10℃ per minute. At the constant temperature of 1090℃, the process is operated with the process conditions of "10 minutes of dry oxygen + 85 minutes of wet oxygen + 10 minutes of dry oxygen", and then the temperature is reduced to 800℃ at 10℃ per minute. The oxygen flow rate during the entire operation is 3L / min, and the water flow rate is 6ml / min. The program operation is completed. Remove the ground mouth, withdraw the boat, and measure the oxide layer thickness of the sample. If it meets the process requirements and passes the inspection, take the silicon wafer on the quartz boat into the silicon wafer box and send it to photolithography. The steps are the same as d.

[0163] i. Isolation pre-expansion

[0164] Put the qualified silicon wafers into the quartz boat, then move the boat to the quartz tube furnace mouth, cover the ground mouth, and move the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. After the boat is finished, the temperature is kept at 1020℃, and nitrogen is introduced for 15 minutes at a nitrogen introduction rate of 5 liters per minute. Then, the ground mouth is removed, the boat is withdrawn, and the boat speed is 14cm / min. The square resistance of the sample is measured, which meets the process requirements and is qualified;

[0165] j. Isolation and expansion

[0166] Put the pre-diffused silicon wafer into the quartz boat, then move the boat to the quartz tube furnace mouth, cover the ground mouth, and start the program; the quartz boat moves into the constant temperature zone of the quartz tube at a boat speed of 14cm / min, nitrogen is introduced at a base temperature of 800℃, and the temperature is raised to the process temperature of 1110℃ at 10℃ per minute. At a constant temperature of 1110℃, the process is run with the process conditions of "40 minutes of dry nitrogen + 10 minutes of wet oxygen", and then the temperature is lowered to 800℃ at 10℃ per minute. The oxygen flow rate during the entire operation is 5L / min, and the water flow rate is 6ml / min, and the program is finished. Remove the ground mouth, withdraw the boat, and the boat speed is 14cm / min. After the quartz boat withdraws, send the silicon wafer on the quartz boat for inspection. After passing the inspection, perform phosphorus bridge oxidation and test the oxide layer thickness. If it meets the process requirements, it will be sent to the photolithography step in the same way as d after passing the inspection;

[0167] k. Phosphorus bridge pre-expansion

[0168] Put the qualified silicon wafers into the quartz boat, then put the boat into the quartz tube furnace mouth, cover the ground mouth, and put the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. After the boat is put into the boat, the temperature is kept at 1050℃. After nitrogen and oxygen are introduced for 3 minutes, the nitrogen is turned on for phosphorus pre-diffusion. The phosphorus pre-diffusion time is 20 minutes. Among them, the oxygen introduction rate is 1.5 liters per minute; the nitrogen introduction rate is 2 liters per minute; the nitrogen introduction rate is 100 milliliters per minute. After the source is completed, nitrogen and oxygen are introduced for 5 minutes, the ground mouth is removed, the boat is withdrawn, the boat speed is 14cm / min, and the square resistance of the sample is measured. It meets the process requirements and the inspection is qualified; the silicon wafers on the quartz boat are loaded into the wafer box.

[0169] l. Phosphorus bridge expansion

[0170] Put the qualified silicon wafers into the quartz boat, and then move the boat to the quartz tube furnace mouth, cover the ground mouth, and move the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. After entering the boat, oxygen is introduced at a base temperature of 800℃, and the temperature is raised to the process temperature of 1050℃ at 10℃ per minute. At 1050℃ constant temperature, the process is run with the process conditions of "5 minutes of dry oxygen + 30 minutes of wet oxygen + 10 minutes of dry oxygen", and then the temperature is lowered to 800℃ at 10℃ per minute. The oxygen flow rate during the entire operation is 5L / min, and the water flow rate is 6ml / min. The program is finished. Remove the ground mouth, withdraw the boat, and measure the oxide layer thickness of the sample. If it meets the process requirements and passes the inspection, take the silicon wafer on the quartz boat into the silicon wafer box and send it to photolithography. The steps are the same as d.

[0171] m. Base area pre-expansion

[0172] Put the same silicon wafer that has passed the inspection into the quartz boat, then move the boat into the quartz tube furnace mouth, cover the ground mouth, and move the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. After the boat is finished, the temperature is maintained at 940℃, and nitrogen is introduced for 25-30 minutes at a nitrogen introduction rate of 3 liters per minute. Then, the ground mouth is removed, the boat is withdrawn, and the boat speed is 14cm / min. The square resistance of the sample is measured, and it meets the process requirements and passes the inspection; the silicon wafer on the quartz boat is taken into the silicon wafer box;

[0173] n. Base area expansion:

[0174] Put the qualified silicon wafers into the quartz boat, and then move the boat to the quartz tube furnace mouth, cover the ground mouth, and move the quartz boat into the constant temperature zone of the quartz tube at a boat speed of 14cm / min. After the boat is entered, the temperature is maintained at 1050℃, and the process is operated under the process conditions of "2 minutes of dry oxygen + 30~40 minutes of wet oxygen + 2 minutes of dry oxygen". The oxygen flow rate during the entire operation is 3L / min, and the water flow rate is 6ml / min. After the process is completed, remove the ground mouth, withdraw the boat, and measure the square resistance of the sample. If it meets the process requirements and passes the inspection, take the silicon wafer on the quartz boat into the silicon wafer box and send it to the photolithography, and the step is the same as d;

[0175] o. Pre-expansion of the launch area

[0176] Put the qualified silicon wafers into the quartz boat, push the boat into the constant temperature zone of the quartz furnace tube, cover the ground mouth, keep the temperature at 1080°C, introduce nitrogen and oxygen for 3 minutes, the oxygen flow rate is 80mL / min, and the nitrogen flow rate is 2L / min; turn on the nitrogen source for phosphorus pre-diffusion, the phosphorus pre-diffusion time is 3 minutes, and the nitrogen flow rate is 100mL / min. After the source is completed, introduce nitrogen and oxygen for 1 minute, the oxygen flow rate is 80mL / min, and the nitrogen flow rate is 2L / min. Then, pull the quartz boat out of the quartz tube, measure the β value of 74-87, which meets the process requirements and passes the inspection; take the silicon wafers on the quartz boat into the silicon wafer box;

[0177] p. Expanding the launch area

[0178] Put the qualified silicon wafers into the quartz boat, push the quartz boat into the constant temperature zone of the quartz furnace tube, cover the ground mouth, maintain the temperature at 410℃, pass nitrogen for 40 minutes with a nitrogen flow rate of 5L / min, remove the ground mouth, pull the quartz boat out of the quartz tube, take out the silicon wafers on the quartz boat and send them for photolithography, the steps are the same as d.

[0179] q. Front metal deposition

[0180] The silicon wafer undergoes front-side metal deposition process to complete front-end production.

[0181] 2. Mid-term test

[0182] The test was conducted using the JC3166 test bench of the integrated circuit test system. The test program was written according to the product process specification requirements. The die whose parameters met the process standard specifications after the front-end was completed were screened, the die with abnormal parameters were eliminated, and the electrical characteristics of the test die were recorded. The VOH test data was 2.70V, and IOZH and IOZL were 11-15μA, which did not meet the preset conditions.

[0183] Calculate the absolute value of the difference between VOH and the first threshold as the first parameter, the first parameter is 0.05V;

[0184] Calculate the absolute value of the IOZ test result and the second threshold as the second parameter, and the second parameter is 1-5μA;

[0185] According to the first positive correlation function, the first adjustment step is determined to be 20°C; according to the second positive correlation function, the second adjustment step is determined to be 2 minutes;

[0186] Reset the first temperature to 1070° C. and the first time to 5 minutes, and repeat steps 1 and 2 in a cycle.

[0187] According to the first positive correlation function, the first adjustment step is determined to be 10°C; according to the second positive correlation function, the second adjustment step is determined to be 1min;

[0188] Reset the first temperature to 1080° C. and the first time to 6 minutes, and repeat steps 1 and 2 in a cycle.

[0189] According to the first positive correlation function, the first adjustment step is determined to be 5°C; according to the second positive correlation function, the second adjustment step is determined to be 1min;

[0190] Reset the first temperature to 1085° C. and the first time to 7 minutes, and repeat steps 1 and 2 in a cycle.

[0191] Until the VOH test data is 2.76-2.84V, IOZH and IOZL are 1-8μA, meeting the parameter standard VOH≥2.75V, IOZH, IOZL≤10μA requirements, all are qualified after the test flow.

[0192] Example 2

[0193] This embodiment provides a bipolar integrated circuit. The manufacturing process is different from that of Embodiment 1 in that the first temperature of the base region re-expansion in step n is 1070° C., and the first time of phosphorus pre-diffusion in step o is 10 minutes.

[0194] The VOH test data of Example 2 is 2.76-2.82V, and IOZH and IOZL are 0.6-8.4μA, which meets the parameter standard requirements of VOH≥2.75V, IOZH, IOZL≤10μA, and all are qualified after the test flow.

[0195] Example 3

[0196] This embodiment provides a bipolar integrated circuit. The preparation process is different from that of embodiment 1 in that the first temperature of the base region re-expansion in step n is 1080° C., the first phosphorus pre-diffusion time in step o is 5 minutes, and the remaining steps are the same as those in embodiment 1 and will not be repeated here.

[0197] The VOH test data of Example 3 is 2.76-2.85V, and IOZH and IOZL are 1.4-9.5μA, which meets the parameter standard requirements of VOH≥2.75V, IOZH, IOZL≤10μA, and all are qualified after the test flow.

[0198] Example 4

[0199] This embodiment provides a bipolar integrated circuit. The manufacturing process is different from that of embodiment 1 in that the β value measured after the emitter region pre-expansion in step o is 70, and the remaining steps are the same as those in embodiment 1, which will not be described again.

[0200] Example 4 The VOH test data is 2.76-2.81V, IOZH and IOZL are 0.2-7.6μA, which meets the parameter standard VOH≥2.75V, IOZH, IOZL≤10μA requirements, and all are qualified after the test flow.

[0201] Example 5

[0202] This embodiment provides a bipolar integrated circuit. The manufacturing process is different from that of the embodiment 1 in that the β value measured after the emitter region pre-expansion in step o is 90, and the remaining steps are the same as those of the embodiment 1, which will not be described again.

[0203] Example 5 The VOH test data is 2.76-2.83V, IOZH and IOZL are 2.3-8.9μA, which meets the parameter standard VOH≥2.75V, IOZH, IOZL≤10μA requirements, and all are qualified after the current test.

[0204] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for manufacturing a bipolar integrated circuit, characterized in that: include: The following steps are repeated in the manufacturing process of bipolar integrated circuits: Manufacturing a bipolar integrated circuit based on current process parameters, the process parameters including a first temperature and a first time, wherein the process of manufacturing the bipolar integrated circuit includes performing base region pre-diffusion on a silicon wafer, performing base region re-diffusion on the silicon wafer after the base region pre-diffusion, performing emitter region pre-diffusion on the silicon wafer, and performing emitter region re-diffusion on the silicon wafer after the emitter region pre-diffusion; The first temperature is used to control the temperature of the base region re-diffusion of the silicon wafer after the base region pre-diffusion, and the process of the emitter region pre-diffusion of the silicon wafer includes phosphorus pre-diffusion through a small amount of nitrogen; The first time is used to characterize the duration of phosphorus pre-diffusion when the emitter region pre-diffusion is performed on the silicon wafer; Performing a VOH test and / or an IOZ test on the bipolar integrated circuit; The VOH test is a high-level output voltage test, and the IOZ test is a high-resistance current test; When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, modify the first temperature and / or the first time in the process parameters according to the preset rules to obtain new process parameters, and use the new process parameters as the current process parameters; When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, it includes: A VOH test result of the bipolar integrated circuit is less than a first threshold value of the VOH test high level output voltage; Or, the IOZ test result of the bipolar integrated circuit is greater than the second threshold value of the IOZ test high-resistance current; The preset rules include: A first positive correlation functional relationship between the first parameter and the second parameter; A second positive correlation function relationship between the third parameter and the fourth parameter; The first parameter is used to indicate the absolute value of the difference between the VOH test result and the first threshold; The third parameter is used to indicate the absolute value of the difference between the IOZ test result and the second threshold value; The second parameter and the fourth parameter are respectively used to indicate the adjustment step size; The modifying the first temperature and the first time in the process parameters according to the preset rule includes: Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit; Determine a first adjustment step size based on the first difference and the first positive correlation function relationship; Determine a second adjustment step size based on the second difference and the second positive correlation function relationship; Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size; Based on the current process parameters and the target adjustment step, new process parameters are determined.

2. The manufacturing method according to claim 1, characterized in that: Also includes: When the VOH test result or the IOZ test result of the bipolar integrated circuit meets the preset requirement, the current process parameter is maintained.

3. The manufacturing method according to claim 1, characterized in that: When the VOH test result or IOZ test result of the bipolar integrated circuit meets the preset requirements, it includes: The VOH test result of the bipolar integrated circuit is not less than the first threshold; Furthermore, an IOZ test result of the bipolar integrated circuit is not greater than the second threshold.

4. The manufacturing method according to claim 1, characterized in that: Before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes: Determine initial process parameters; the initial process parameters include: when the base region is re-diffused, heat-treating the silicon wafer after the base region pre-diffusion treatment in dry oxygen, wet oxygen, and dry oxygen atmospheres at a first temperature in sequence; The first temperature is 1040°C to 1060°C; Manufacturing a bipolar integrated circuit based on the initial process parameters; Performing a VOH test and / or an IOZ test on the bipolar integrated circuit; When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first temperature in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

5. The manufacturing method according to claim 1, characterized in that: Before manufacturing the bipolar integrated circuit based on the current process parameters, the method further includes: Determine initial process parameters; the initial process parameters include: when the emitter region is pre-diffused, the silicon wafer after the base region is re-diffused is pre-diffused with phosphorus at the first time; The first time is 3 minutes to 6 minutes; Manufacturing a bipolar integrated circuit based on the initial process parameters; Performing a VOH test and / or an IOZ test on the bipolar integrated circuit; When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirements, the first time in the initial process parameters is modified according to the preset rules to obtain new process parameters, and the new process parameters are used as the current process parameters.

6. The manufacturing method according to claim 2, characterized in that: When the VOH test result or the IOZ test result of the bipolar integrated circuit does not meet the preset requirement, determining a first parameter by using the VOH test result and the first threshold value; Determine the second parameter according to the IOZ test result and the second threshold value; Determine a first difference value based on a VOH test result of the bipolar integrated circuit, and determine a second difference value based on an IOZ test result of the bipolar integrated circuit; Determine a first adjustment step size based on the first difference and the first positive correlation function relationship; Determine a second adjustment step size based on the second difference and the second positive correlation function relationship; Determine a target adjustment step size based on the first adjustment step size and the second adjustment step size; The first temperature of the base region re-diffusion heat treatment or the first time of phosphorus diffusion during the emitter region pre-diffusion is reset until the VOH test result and / or the IOZ test result of the bipolar integrated circuit meet the preset requirements.

7. The manufacturing method according to claim 1, characterized in that: The preset requirement of the VOH test is VOH ≥ 2.75V, and the first threshold is 2.75V; The preset requirement of the IOZ test is ≤10 μA, and the second threshold is 10 μA.

8. A driver, characterized in that: A bipolar integrated circuit manufactured by the manufacturing method according to any one of claims 1 to 7.