A polishing pad and its preparation method and application
By cross-arrangement of filament layers with different compression recovery rates in the buffer middle layer of the chemical mechanical polishing pad and forming annular grooves, the problem of reducing polishing efficiency at the end of the service life of the polishing pad is solved, and a longer service life and better service life are achieved High polishing efficiency.
Patent Information
- Application Number
- CN202410873231.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-01
AI Technical Summary
At the end of the service life of the existing chemical mechanical polishing pads, the polishing efficiency is greatly reduced, resulting in an increase in wafer shipment rate and cost. The reduction in the compression rate of the buffer layer cannot meet the effective rebound performance, which affects the service life of the polishing pad.
The service life of the polishing pad is extended by cross-arranged annular filament layers with different compression recovery rates in the buffer mid-layer of the polishing pad and forming annular grooves between the filamenting layers to achieve segmentation.
It extends the service life of the polishing pad, ensures polishing efficiency and planarization, improves chip shipment stability and reduces production costs.
Smart Images

Figure CN118404492B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of chemical mechanical planarization, and in particular to a polishing pad and a preparation method and application thereof. Background Art
[0002] In the past decade, the semiconductor industry has developed rapidly, and the feature size of integrated circuits has continued to shrink. The wire width has increased from 0.18µm to 5 / 7nm, indicating that integrated circuits have entered the nanoscale era. Nanoscale chips require high performance, high integration, high speed, and stability, and the flatness requirements of the interconnected layers of integrated circuits have also entered the nanoscale.
[0003] The deposition technologies of various layers of materials in modern integrated circuit wafers include physical vapor deposition (PVD) (also known as sputtering), chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD) and electrochemical plating (ECP). Due to the technical limitations of the deposition technology itself, the surface of the deposited material must be flattened later. Flattening technology can effectively remove surface morphology and surface defects that do not meet the circuit requirements during the material deposition process, such as high unevenness, surface roughness, material agglomeration, lattice damage, scratches and contamination. Chemical mechanical planarization or chemical mechanical polishing (CMP) is a common technology used to polish or flatten workpieces (such as semiconductor wafers). In traditional chemical mechanical polishing (CMP), the wafer is fixed to a carrier or polishing head by a fixing ring and is mounted on a carrier assembly together. The polishing head with the wafer fixed is mounted on a support in the chemical mechanical polishing (CMP) equipment, and the polishing turntable in the equipment is attached to the chemical mechanical polishing pad. During polishing, the wafer is in direct contact with the polishing layer of the polishing pad. The carrier assembly provides controllable pressure between the wafer and the polishing pad. The polishing pad rotates at a certain speed, and the wafer rotates at a speed different from the polishing pad. When the polishing pad contacts the wafer, the area is usually a circular polishing track or polishing area. At the same time, the polishing medium (such as polishing liquid) is distributed from the center of the polishing pad to the polishing pad through the transmission channel, and enters the gap between the wafer and the polishing layer. Through the chemical and mechanical action of the polishing layer and the polishing medium on the surface of the wafer, the surface material of the wafer is polished and made into a flat surface. Flattening and cleanliness are the two most important indicators in chemical mechanical polishing (CMP). In the process of chemical mechanical polishing (CMP), the consumption and replacement of polishing consumables are severe challenges to the stability of wafer shipment. Each round of consumable replacement means that the wafer will face new risks. Therefore, as one of the important consumables in the polishing process, extending the life of the chemical mechanical polishing pad (CMP Pad) is an effective guarantee to ensure wafer shipment and reduce costs.
[0004] CN102601747A proposes to consolidate an abrasive block on a substrate, wherein the abrasive block has at least two heights. By using an abrasive block having at least two heights, the grinding pad will not significantly reduce the grinding rate due to long-term grinding during the process of grinding the wafer, thereby making it easy to accurately control the degree of grinding of the wafer, thereby improving the effect and yield of wafer grinding. Consolidating abrasives in a polyurethane elastomer can improve and stabilize the polishing rate, but it cannot solve the problem that the buffer layer, due to repeated gravity application during the polishing process, changes from elastic deformation to plastic deformation, resulting in a significant reduction in the overall compression rate, and cannot meet the effective rebound performance, resulting in the problem of Lifetime expiration.
[0005] CN 114425743 A proposes to set at least two polishing parts with different heights on the polishing layer, and the different polishing parts are alternately worn during the polishing process, so as to achieve the purpose of extending the service life of the polishing pad. This patent extends the service life by improving the structure of the polishing layer, but cannot solve the problem that the buffer layer, due to repeated gravity application during the polishing process, changes from elastic deformation to plastic deformation, resulting in a significant reduction in the overall compression rate, and cannot meet the effective rebound performance, resulting in the end of the life.
[0006] CN1978140A proposes to determine the cutting speed of different areas of the polishing pad by measuring the groove depth and thickness of the polishing pad at different use periods, thereby setting the residence time of the correction disk in different areas of the polishing pad, and detecting the grinding rate of the abrasive particles and chemical mechanical polishing (CMP) in different areas of the polishing pad and measuring the groove depth and thickness of the polishing pad that has been used to the end of its life. According to the detection results of the above steps, the pressure of the correction disk in different areas of the polishing pad is set, and the appropriate pressure parameters are found through multiple experimental data statistics to make the in-plane loss and groove depth of each area of the polishing pad tend to be consistent. In this patent, by setting the pressure of each area of the polishing pad, the cutting of the polishing pad is made more uniform, the service life of the polishing pad can be extended, and the production cost can be reduced. In fact, it is an adjustment of the dressing process parameters, not an optimization of the chemical mechanical polishing pad (CMP Pad) itself.
[0007] During the chemical mechanical polishing (CMP) process, when the service life of the polishing pad is near the end, the polishing efficiency of the polished wafer will be greatly reduced, and the flattening effect will be greatly reduced, which will seriously affect the product shipment rate and factory cost. Therefore, the use time of the polishing pad will be strictly controlled in the chemical mechanical polishing (CMP) process. Generally, the total number of polished wafers or the total use time of the polishing pad is used to calculate the service life of the chemical mechanical polishing pad. The service life of the polishing pad is related to two factors: on the one hand, the polishing surface in the polishing pad is repeatedly scraped by the dressing component during the polishing process, resulting in the consumption of its thickness and macro pattern depth, and eventually losing the function of carrying and transporting the polishing liquid; on the other hand, the middle layer auxiliary pad (also called the buffer middle layer) used to improve the compression rate in the polishing pad is changed from elastic deformation to plastic deformation due to repeated gravity application during the polishing process, resulting in a significant reduction in the overall compression rate, which cannot meet the performance of effective rebound. The consumption of the polishing top layer of the polishing pad is difficult to avoid during polishing, but the compression rate and rebound rate of the middle layer auxiliary pad can be achieved by optimizing the structure of the middle layer. Summary of the invention
[0008] In order to solve the above-mentioned defects in the prior art, the present invention provides a polishing pad and a preparation method and application thereof, which controls the zoning and segmenting effect of the spliced combined buffer middle layer contained in the polishing pad to adjust the polishing time and extend the life of the polishing pad.
[0009] To achieve the above-mentioned purpose of the invention, the first aspect of the present invention provides a polishing pad, comprising a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer which are bonded in sequence, wherein an annular filament layer block with a first compression recovery rate and an annular filament layer block with a second compression recovery rate are cross-arranged from the center of the circle to the outside in an increasing diameter manner to form the buffer middle layer, the first compression recovery rate and the second compression recovery rate are different, and there is a gap between at least one group of adjacent filament layer blocks to form an annular groove; the filament layer block is selected from one or more of the filament layer block C1 and the filament layer block C; the filament layer block C1 has a width of 5-15 mm and a compression recovery rate of 35-75%; the filament layer block C has a width of 20-40 mm and a compression recovery rate of 60-90%.
[0010] Further, there are gaps between the multiple groups of adjacent filament layer blocks to form a plurality of annular grooves, wherein the width of the annular grooves is 1-10 mm, preferably 3-8 mm, more preferably 4-6 mm; the depth of the annular grooves is 1.2-2 mm, preferably 1.28-1.56 mm, more preferably 1.34-1.48 mm; and / or,
[0011] Preferably, each group of adjacent filament layer blocks has an annular groove between them; and / or,
[0012] Preferably, the buffer middle layer has a plurality of evenly distributed annular grooves, and / or,
[0013] Preferably, the plurality of annular filament layer blocks have the same center.
[0014] Furthermore, the adjacent filament layer blocks have different widths.
[0015] Furthermore, the width of the filament layer block C1 is preferably 8-14 mm, more preferably 10-12 mm; the compression recovery rate is preferably 45-65%, more preferably 50-60%; the width of the filament layer block C is preferably 25-35 mm, more preferably 28-32 mm; the compression recovery rate is preferably 70-90%, more preferably 85-90%.
[0016] Furthermore, the filament layer block C1 and the filament layer block C are selected from any one of a felt obtained by impregnating a non-woven fabric material with polyurethane, a soft polyurethane foam obtained by physical and chemical foaming, and a polyvinyl chloride foam; preferably, the felt is obtained by impregnating a non-woven fabric material with polyurethane; more preferably, the polyurethane impregnated with the non-woven fabric material is mainly composed of components including isocyanate monomers, polymer polyols, and small molecule chain extenders.
[0017] Furthermore, the polishing top layer is a polyurethane elastomer with a cavity structure made of any one selected from polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene; preferably, the polyurethane elastomer with a cavity structure is mixed and cured by at least the following three components: a prepolymer with an unreacted isocyanate (NCO) mass concentration of not less than 5.4%, hollow microspheres and a curing agent; more preferably, the prepolymer is formed by the reaction of isocyanate and a polymer polyol; the curing agent is a polyol and / or a polyamine.
[0018] Furthermore, the upper adhesive layer is a heat-sensitive adhesive layer; preferably, it is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 µm, the thickness of the adhesive coating on both sides of the substrate is 10-150 µm, and the overall thickness of the heat-sensitive adhesive layer is 40-420 µm.
[0019] Furthermore, the lower adhesive layer is a pressure-sensitive adhesive layer; preferably, it is a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 µm, the adhesive coating thickness on the upper side of the substrate is 10-150 µm, the adhesive coating thickness on the lower side of the substrate is 5-50 µm, and the overall thickness of the pressure-sensitive adhesive layer is 35-320 µm.
[0020] Furthermore, the supporting bottom layer is a film with high tensile strength and smooth surface, preferably any one of polyethylene terephthalate film, polyethylene film, and polyvinyl chloride film with a release agent coated on the surface, and more preferably a polyethylene terephthalate film with a release agent coated on the surface.
[0021] Another object of the present invention is to provide a method for preparing the polishing pad, comprising the steps of sequentially bonding the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer.
[0022] Another object of the present invention is to provide application of the polishing pad or the polishing pad prepared by the above method in chemical mechanical polishing, preferably application in chemical mechanical polishing of copper wafers.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The polishing pad of the present invention comprises a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer which are sequentially bonded, wherein an annular filament layer block with a first compression recovery rate and an annular filament layer block with a second compression recovery rate are cross-arranged in a manner of increasing diameter from the center of a circle outward to form the buffer middle layer, the value of the first compression recovery rate is different from the value of the second compression recovery rate, and there is a gap between at least one group of adjacent filament layer blocks to form an annular groove. The present invention arranges filament layer blocks with two different compression recovery capabilities in the buffer middle layer, so that the filament layer blocks of different properties can achieve segmented effects during polishing, thereby extending the service life of the polishing pad.
[0025] Specifically, the polishing pad of the present invention controls the two filament layer blocks C1 and the filament layer block C to have different widths and compression recovery rates, etc., so that the annular filament layer blocks with different physical properties can realize the segmented effect of the buffer middle layer during polishing. For example, the width of the annular filament layer block C1 is smaller than that of the annular filament layer block C, so the overall compressed area is smaller than that of the filament layer block C, and the compression recovery rate of the filament layer block C is greater than that of the filament layer block C1, that is, the height that can be recovered after compression and decompression is higher. Therefore, during compressive polishing in the early stage of Pad Lifetime, the filament layer block C assumes the main buffering role, but when the compression rebound of the filament layer block C is close to the end of its life, the filament layer block C1 can still take over C to assume the main buffering role, thereby extending the service life of the polishing pad by >45h.
[0026] Other features and advantages of the present invention will be described in detail through the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic top view of the structure of a buffer middle layer composed of spliced filament layer blocks in an embodiment of the present invention.
[0028] Figure 2 A schematic cross-sectional view of an annular protrusion area formed by splicing and assembling filament layer blocks in an embodiment of the present invention.
[0029] Figure 3 Schematic cross-sectional view of a multi-structure chemical mechanical polishing pad according to an embodiment of the present invention.
[0030] Among them, 1 is a buffer middle layer, 11 is an annular protrusion area (filament layer block), 111 is a filament layer block C1, 112 is a filament layer block C, 113 is an annular groove, 2 is a polished top layer, 3 is a heat-sensitive upper adhesive layer, 4 is a pressure-sensitive lower adhesive layer, and 5 is a supporting bottom layer. DETAILED DESCRIPTION
[0031] The following will clearly and completely describe the concept of the present application and the technical effects produced in combination with the embodiments, so as to fully understand the purpose, features and effects of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of them. Based on the embodiments of the present application, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present application.
[0032] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.
[0033] like Figure 3 As shown, the CMP polishing pad with extended service life of the present invention comprises a polishing top layer 2 of wear-resistant polyurethane elastomer, a heat-sensitive upper bonding layer 3, a buffering middle layer 1, a pressure-sensitive lower bonding layer 4 and a supporting bottom layer 5 bonded in sequence from top to bottom, and the five layers are bonded to form a multi-structure chemical mechanical polishing pad.
[0034] In some embodiments, Figure 1~2 As shown, annular filament layer blocks with a first compression recovery rate and annular filament layer blocks with a second compression recovery rate are cross-arranged in an increasing diameter from the center of the circle to the outside to form the buffer middle layer, the value of the first compression recovery rate is different from the value of the second compression recovery rate, and there is a gap between at least one group of adjacent filament layer blocks to form an annular groove 113, the function of the annular groove is to provide sufficient space for the lateral deformation caused by the compression of the filament layer blocks.
[0035] Preferably, there are gaps between multiple groups of adjacent filament layer blocks to form multiple annular grooves, the width of the annular grooves is 1-10 mm, preferably 3-8 mm, more preferably 4-6 mm; the depth of the annular grooves is 1.2-2 mm, preferably 1.28-1.56 mm, more preferably 1.34-1.48 mm. The filament layer blocks will be deformed in the horizontal direction under pressure during the polishing process. Setting the width and depth of the annular grooves can effectively provide space for the compression deformation of the filament layer blocks on both sides of the grooves, avoiding abnormal problems such as degumming of the polishing pad due to deformation and extrusion.
[0036] Preferably, each group of adjacent filament layer blocks has an annular groove between them.
[0037] Preferably, the buffer middle layer has a plurality of evenly distributed annular grooves.
[0038] Preferably, the plurality of annular filament layer blocks have the same center.
[0039] In some embodiments, the annular filament layer block is selected from one or more of the filament layer block C1 and the filament layer block C; for example, Figure 2 As shown, the C1 filament layer block 111 with a first compression recovery rate and the C filament layer block 112 with a second compression recovery rate are cross-arranged. In other embodiments, a composite filament layer block formed by splicing the C1 filament layer block and the C filament layer block can also be used, and the composite filament layer block is cross-arranged with the filament layer block C1 or the filament layer block C to ensure that adjacent filament layer blocks have different compression recovery capabilities, and only filament layer blocks with two different compression recovery rate values (the first compression recovery rate and the second compression recovery rate) are cross-arranged in the entire buffer middle layer.
[0040] In some embodiments, the filament layer block C1 and the filament layer block C are both selected from any one of a felt obtained by impregnating a non-woven fabric material with polyurethane, a soft polyurethane foam obtained by physical and chemical foaming, and a polyvinyl chloride foam; preferably, a felt obtained by impregnating a non-woven fabric material with polyurethane. The impregnated polyurethane material is mainly composed of an isocyanate monomer, a polymer polyol, and a small molecule chain extender component. Specifically, the isocyanate monomer is, for example, p-phenylene diisocyanate, o-toluidine diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, allophanate-modified diphenylmethane diisocyanate, biuret-modified diphenylmethane diisocyanate, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, cyclohexane diisocyanate, and any one of these and a mixture thereof, but is not limited thereto. The polymer polyol is, for example, at least one of polytetramethylene ether glycol, polypropylene ether glycol, polycarbonate polyol, polycaprolactone polyol, ethylene adipate or butylene adipate ester polyols, or a copolymer or mixture thereof, but is not limited thereto. The small molecule chain extender is, for example, any one of 1,4-butanediol (BDO), 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol (DEG), triethylene glycol, neopentyl glycol (NPG), sorbitol, diethylaminoethanol (DEAE) or a mixture thereof, and the mass ratio of each isocyanate monomer, polymer polyol, and small molecule chain extender component is, for example, 7.3:2.4:0.3.
[0041] Although the two filament layer blocks C1 and C may be made of the same material, they have different compression recovery rates and, preferably, different widths. Specifically, the width of the filament layer block C1 is 5-15 mm, for example, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, preferably 8-14 mm, and more preferably 10-12 mm; the compression recovery rate is 35-75%, for example, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, preferably 45-65%, and more preferably 50-60%; the width of the filament layer block C is 20-40 mm, 20 mm, 22 mm, 25 mm, 28 mm, 30 mm, 32 mm, 35 mm, 38 mm, 40 mm, preferably 25-35 mm, and more preferably 28-32 mm; the compression recovery rate is 60-90%, for example, 60%, 65%, 70%, 75%, 80%, 85%, 90%, preferably 70-90%, and more preferably 85-90%.
[0042] Those skilled in the art will understand that, for example, Figure 2As shown, in the buffer middle layer formed by the cross-arrangement of multiple C1 filament layer blocks 111 and multiple filament layer blocks 112, the compression recovery rates of the filament layer blocks C1 and the filament layer blocks C are different, but in the entire buffer middle layer, the compression recovery rate values of the filament layer blocks C1 are the same, and the compression recovery rate values of the filament layer blocks C are the same, that is, only filament layer blocks with two different compression recovery rate values are used in the entire buffer middle layer to cross-arrange, thereby ensuring the uniformity and timeliness of the force applied to the buffer middle layer during the polishing process, and at the same time ensuring that the two filament layer blocks with different properties achieve segmented effects during polishing and extend the service life of the CMP polishing pad.
[0043] Generally, compared with the filament layer block C, the filament layer block C1 has a smaller width and a smaller compression recovery rate, wherein the compression recovery rate refers to the ratio of the thickness of the filament layer block recovered after the compression rate is removed to the thickness before compression.
[0044] In the present invention, by controlling the width and compression recovery rate of the two fibril layer blocks, the two fibril layer blocks with different properties can achieve segmented effects during polishing, thereby extending the service life of the CMP polishing pad.
[0045] In the present invention, the wear-resistant polyurethane elastomer polishing top layer 2 is a polyurethane elastomer with a cavity structure made of any material selected from polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene. The polyurethane elastomer with a cavity structure is formed by mixing and curing at least three components: an isocyanate polyol prepolymer with an unreacted isocyanate (NCO) concentration of not less than 5.4%, hollow microspheres, polyol or polyamine alone or in combination with a curing agent; the isocyanate polyol prepolymer with an unreacted isocyanate (NCO) concentration of not less than 5.4% is formed by the reaction of isocyanate and polymer polyol. The polishing top layer and its preparation process of the present invention are not particularly limited, and reference may be made to the prior art, such as reference patent US2004 / 094855 A1.
[0046] In the present invention, the heat-sensitive upper adhesive layer 3 is a heat-sensitive adhesive layer; for example, it is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; the substrate is usually PET (polyethylene terephthalate), preferably, the thickness of the substrate is 20-120 µm, for example, 20µm, 30µm, 40µm, 50µm, 60µm, 70µm, 80µm, 90µm, 100µm, 110µm, 120µm, etc., the thickness of the adhesive coating on both sides of the substrate is 10-150 µm, for example, 10µm, 20µm, 30µm, 40µm, 50µm, 60µm, 70µm, 80µm, 90µm, 100µm, 110µm, 120µm, 130µm, 140µm, 150µm, etc., and the overall thickness of the heat-sensitive adhesive layer is 40-420 µm, such as 40µm, 60µm, 80µm, 100µm, 150µm, 200µm, 250µm, 300µm, 350µm, 400µm, etc.
[0047] In the present invention, the pressure-sensitive lower adhesive layer 4 is a pressure-sensitive adhesive layer; for example, it is a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 µm, for example, 20µm, 30µm, 40µm, 50µm, 60µm, 70µm, 80µm, 90µm, 100µm, 110µm, 120µm, etc., the thickness of the adhesive coating on the upper side of the substrate is 10-150 µm, for example, 10µm, 20µm, 30µm, 40µm, 50µm, 60µm, 70µm, 80µm, 90µm, 100µm, 110µm, 120µm, 130µm, 140µm, 150µm, etc., and the thickness of the adhesive coating on the lower side of the substrate is 5-50 The pressure-sensitive adhesive layer has an overall thickness of 35-320 µm, such as 35µm, 40µm, 60µm, 80µm, 100µm, 150µm, 200µm, 250µm, 300µm, 320µm, etc.
[0048] In the present invention, the supporting bottom layer 5 is a protective structure with high tensile strength and smooth surface, for example, any one of polyethylene terephthalate film, polyethylene film, and polyvinyl chloride film with a release agent coated on the surface, more preferably a polyethylene terephthalate film with a release agent coated on the surface.
[0049] The method for preparing a CMP polishing pad with an extended service life of the present invention, for example, includes the steps of bonding and laminating the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer in sequence, wherein the buffer middle layer is formed by annular filament layer blocks C1 and / or C arranged in increasing diameter from the center of the circle outward, and in some examples, the filament layer block C1 and / or the filament layer block C are carved into a specified annular shape and are bonded to the pressure-sensitive adhesive lower layer 4 using a spliced abrasive tool bonding machine at a pressure of 0.1 MPa.
[0050] The polishing pad of the present invention is used in chemical mechanical polishing, and the polishing pad rotates continuously during the chemical mechanical polishing process; the semiconductor wafer is pressed on the rotating polishing pad and rotates in the same direction as the polishing pad at a speed different from that of the polishing pad. The polishing liquid enters at an eccentric position of the rotating polishing pad, participates in the grinding and polishing of the semiconductor wafer and the CMP polishing pad, and is finally discharged at the edge area of the polishing pad. The compressive elasticity of the buffer middle layer of the polishing pad is mainly beneficial to relieve the stress when the wafer contacts the polishing pad when pressure acts on the back of the wafer during the polishing process, and increases the area of uniform contact between the wafer and the polishing pad. The polishing head will set different downward pressures in different areas from the center to the edge. The effective compressibility of the polishing pad can achieve parallel contact between the wafer surface and the polishing pad surface when responding to downward pressures in different areas. The parallel contact helps to maintain the flattening uniformity (Range) of the wafer surface removal and ensure the polishing efficiency.
[0051] Specifically, the polishing pad of the present invention can be applied to the polishing pressure and rotation speed commonly used in the art, for example, the polishing pressure is 1-5 psi, preferably 1-2 psi, the polishing disk and / or polishing head rotation speed is 50-300 rpm, preferably 80-100 rpm; preferably, the flattening uniformity Range of the wafer surface removed is <50Å, the polishing efficiency RR>5000Å / min, and the end life of the polishing pad Lifetime>20h. By using the polishing pad of the present invention, the flattening uniformity Range of the wafer surface removed can be <50Å, the polishing efficiency RR>5000Å / min, and the end life of the polishing pad Lifetime~45h, which is longer than the life of the conventional polishing pad of 24-30h.
[0052] In order to effectively remove wafer materials and flatten the surface, chemical mechanical polishing (CMP) achieves mechanical action by directly contacting the wafer with the polishing layer of the polishing pad during polishing. The micro-convexities on the surface of the polishing layer must directly or semi-directly contact the substrate surface and provide controllable pressure between the wafer and the polishing pad. The polishing pad rotates at a certain speed, and the wafer rotates at a speed different from the polishing pad. When the polishing pad and the wafer rotate, the contact area is usually a circular polishing track or polishing area. At the same time, the polishing medium (such as polishing liquid) is distributed from the center of the polishing pad to the polishing pad through the transmission channel, and enters the gap between the wafer and the polishing layer to achieve effective chemical action. The polishing medium usually contains nano-scale abrasive particles, which are distributed in various areas of the polishing pad with the polishing liquid, and more precise mechanical movement is achieved during the polishing process. Through the chemical and mechanical action of the polishing layer and the polishing medium on the surface on the wafer, the wafer surface material is polished and made into a flat surface.
[0053] The compressive elasticity of the polishing pad buffer middle layer is mainly beneficial to relieve the stress of the wafer and the polishing pad when pressure acts on the back of the wafer during the polishing process, and increase the uniform contact area between the wafer and the polishing pad. The polishing head will set different downward pressures in different areas from the center to the edge. The effective compressibility of the polishing pad can achieve parallel contact between the wafer surface and the polishing pad surface when responding to downward pressures in different areas. Parallel contact helps to maintain the flattening uniformity of the wafer surface removal (Range<50Å) and ensure polishing efficiency (>5000Å / min). As the polishing time increases, the buffer middle layer of the polishing pad will gradually approach the end of its life (~45h), and the deformation mode will change from elastic deformation to plastic deformation. The compression rebound length will decrease and gradually approach 0, which will eventually lead to convex or concave contact between the wafer surface and the polishing pad surface at the end of the polishing pad life, thereby reducing the wafer surface removal efficiency (RR) and flat uniformity (Range). Flatness and cleanliness are the two most important indicators in chemical mechanical polishing (CMP). During the chemical mechanical polishing (CMP) process, the consumption and replacement of polishing consumables are a severe challenge to the stability of wafer shipments. Each round of consumable replacement means that the wafer will face new risks. Therefore, as one of the important consumables in the polishing process, extending the life of the chemical mechanical polishing pad (CMP Pad) is an effective guarantee to ensure wafer shipments and reduce costs.
[0054] The present invention is a CMP polishing pad capable of extending the service life. By controlling the width and compression recovery rate of at least two filament layer blocks in the buffer middle layer, filament layer blocks of different properties can realize segmented effect during polishing. For example, because the width of the annular filament layer block C1 is smaller than that of the annular filament layer block C, the overall compressed area is smaller than that of the filament layer block C, and the compression recovery rate of the filament layer block C is greater than that of the filament layer block C1, that is, the height that can be recovered after compression and decompression is higher. Therefore, during the early stage of PadLifetime compressed polishing, the filament layer block C plays the main buffering role, but when the compression and rebound of the filament layer block C is close to the end of its service life, the filament layer block C1 can still take over the main buffering role from C, thereby extending the service life of the polishing pad by >45h.
[0055] The present invention is further described below with examples and comparative examples, but the present invention is not limited thereto.
[0056] Unless otherwise specified, the polishing pads of the embodiments and comparative examples of the present invention are prepared by the following method:
[0057] The prepolymer (selected from Wanhua Wannate 3H750D) and the curing agent (Hangzhou Chongshun Huang MOCA) are uniformly mixed and poured into the mold to form a polyurethane module, which is then sliced to obtain a wear-resistant polyurethane elastomer polished top layer 2, whose surface is grooved for uniform distribution and outflow of liquid: the groove width is 0.5mm, the depth is 0.8mm, and the interval is 2.5mm. The filament layers C1 and C are cross-arranged and spliced to form a buffer middle layer 1, wherein C1 and C are both selected from the Dow Suba series, and the dimensions and properties are as shown in the width and compression recovery rate of the embodiment and comparative example in Table 1 below; the filament layers C1 and C are carved into specified patterns, referring to Figure 2 The arrangement in the form of a ring-shaped splicing block is placed in the splicing mold. The splicing mold is referred to Figure 1 The buffer middle layer 1 is formed after all the regional splicing blocks are placed. The spliced buffer middle layer 1 is bonded to the pressure-sensitive adhesive lower layer 4 (3M DF1136) by a downward pressing laminating machine using a splicing abrasive. The polyurethane elastomer polishing top layer 2 and the buffer middle layer 1 are bonded by a heat-sensitive adhesive upper layer 3 (3M T24). The bonding method is to use a roller laminating machine to bond, and the bonding temperature is 80℃±5. The pressure-sensitive adhesive lower layer 4 is bonded to the supporting bottom layer 5 (NAGASE Z55). The bonding method is to use a roller laminating machine to bond, and the pressure is 0.1MPa. The polishing pad with a diameter of 300mm is obtained by bonding.
[0058] Table 1 Parameters of two filament layers of the embodiment and the comparative example
[0059] PAD Instance C1 width (mm) C Width(mm) C1 compression recovery rate (%) C Compression recovery rate (%) Example 1 5 20 35 60 Example 2 8 25 45 70 Example 3 11 30 55 80 Example 4 15 40 75 90 Comparative Example 1 4 25 45 70 Comparative Example 2 15 60 75 90 Comparative Example 3 11 30 80 80 Comparative Example 4 11 30 55 95 Comparative Example 1 (two filament layers are the same, both are C1) 11 11 55 55
[0060] Table 1 shows the embodiments and comparative examples of the present invention for achieving effective removal of wafer materials and surface flattening. According to the size and physical properties of the buffer middle layer spliced fiber block provided in the table, the corresponding chemical mechanical polishing pad is made and the polishing experiment is carried out. The polishing conditions are as follows: the polishing pressure is 1.5 psi, the polishing disc and the polishing head speed are 87 / 93 rpm, the polishing liquid is Cu Slurry (11 times diluted, pH 6-7), the polishing pad correction wheel is 3M A165, the polishing liquid flow rate is 250 ml / min, and the polishing machine is E460E / 12 type 300mm chemical mechanical flattening system. A stopwatch is used to count the use time of the polishing pad, and a Four Dimensions four-point detector (333 A) is used to measure the thickness of 81 test points on the copper film, and the average difference is calculated according to the measurement results to determine the copper polishing rate RR and the surface thickness difference Range (Max-Min). The experimental results are shown in Table 2.
[0061] Table 2 Example polishing results
[0062] PAD Instance Pad life (h) RR (Å / min) Range (Å) Example 1 46 5835 32 Example 2 57 6320 30 Example 3 60 7426 21 Example 4 63 7324 16 Comparative Example 1 30 5796 31 Comparative Example 2 31 7456 27 Comparative Example 3 62 6785 72 Comparative Example 4 61 6863 65 Comparative Example 1 42 7522 15
[0063] In order to meet the efficient and high-speed development of integrated circuits and the requirements of the subsequent deposition process of chemical mechanical polishing in the IC process, the requirements for the Cu wafer surface after the Cu CMP process are a copper polishing rate RR≧5000 Å / min and a flattening uniformity of Cu surface removal (Range<50Å). From the polishing experiment results, it can be seen that the chemical mechanical polishing pad embodiment provided by the present invention is verified by the polishing experiment to fully meet or exceed the requirements for the Cu wafer surface after the CMP process, and effectively improves the service life of the polishing pad (>45h).
[0064] The difference between Comparative Example 1 and Example 2 is that the width of the C1 filament block in the buffer middle layer is too small. After comparing the polishing results, it is found that the service life of the polishing pad of Comparative Example 1 is lower than that of Example 2, proving that the width difference between the C1 filament block and the C filament block in the buffer middle layer has a certain influence on the service life of the polishing pad. If the C1 filament block in the buffer middle layer is too narrow, the time for the C1 filament block to play a compression and buffering role in the buffer middle layer is greatly shortened, thus affecting the service life of the polishing pad.
[0065] The difference between Comparative Example 2 and Example 4 is that the width of the C filament block in the buffer middle layer is too large. After comparing the polishing results, it is found that the service life of the polishing pad in Comparative Example 2 is lower than that in Example 4, proving that the width difference between the C1 filament block and the C filament block in the buffer middle layer has a significant impact on the service life of the polishing pad. The C filament block in the buffer middle layer is too wide, resulting in a reduction in the number of C1 filament blocks pasted on the entire polishing pad, thereby shortening the time for the C1 filament block to play a major compression and buffering role, affecting the service life of the polishing pad.
[0066] The difference between Comparative Example 3 and Example 3 is that the compression recovery rate of the buffer middle layer C1 is too large. By comparing the results after polishing, it is found that the flattening uniformity of the surface removed after copper polishing in Comparative Example 3 is lower than that in Example 3, proving that the compression recovery rate of the C1 filament layer block in the buffer middle layer has a very important influence on the copper polishing effect. The excessive compression recovery rate of the C1 filament layer block in the buffer middle layer leads to uneven contact area between the local polishing pad and the copper material during the period when the C1 filament layer block plays the main compression and buffering role as the buffer middle layer, thus affecting the flat uniformity of the copper surface after polishing.
[0067] The difference between Comparative Example 4 and Example 3 is that the C compression recovery rate value is too large. By comparing the results after polishing, it is found that the flattening uniformity of the surface removed after copper polishing in Comparative Example 4 is lower than that in Example 3, proving that the compression recovery rate of the C filament layer block in the buffer middle layer has a very important influence on the copper polishing effect. The excessive compression recovery rate of the filament layer block C leads to uneven contact area between the local polishing pad and the copper material during the period when the C filament layer block plays the main compression and buffering role as the buffer middle layer, thus affecting the flat uniformity of the copper surface after polishing.
[0068] The difference between Comparative Example 1 and Example 4 is that the two filament layer blocks are the same, both are C1 filament layer blocks, and during the polishing process, only one filament layer block with a compression recovery rate plays a compression buffering role, and the compression recovery rates are the same and cannot be segmented to assume the main compression buffering role. Therefore, after the C1 filament layer block reaches the end of its service life, the polishing pad also reaches the end of its service life, and the service life is greatly reduced compared with Example 4.
[0069] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A polishing pad, It is characterized in that It comprises a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer which are bonded in sequence, wherein an annular filament layer block with a first compression recovery rate and an annular filament layer block with a second compression recovery rate are cross-arranged in an increasing diameter manner from the center of a circle outward to form the buffer middle layer, the first compression recovery rate and the second compression recovery rate are different, and there is a gap between at least one group of adjacent filament layer blocks to form an annular groove; the filament layer blocks are selected from one or more of filament layer blocks C1 and filament layer blocks C; the filament layer block C1 has a width of 5-15 mm and a compression recovery rate of 35-75%; the filament layer block C has a width of 20-40 mm and a compression recovery rate of 60-90%.
2. The polishing pad according to claim 1, It is characterized in that There are gaps between the adjacent groups of filament layers to form a plurality of annular grooves, wherein the width of the annular grooves is 1-10 mm; the depth of the annular grooves is 1.2-2 mm; and / or, Each group of adjacent filament layers has an annular groove between them; and / or, The buffer middle layer has a plurality of evenly distributed annular grooves, and / or, The plurality of annular filament layer blocks have the same center.
3. The polishing pad according to claim 1 or 2, It is characterized in that The adjacent filament layer blocks have different widths; The width of the filament layer block C1 is 8-14 mm, and the compression recovery rate is 45-65%; the width of the filament layer block C is 25-35 mm, and the compression recovery rate is 70-90%.
4. The polishing pad according to claim 1, It is characterized in that The filament layer block C1 and the filament layer block C are selected from any one of a felt obtained by impregnating a nonwoven fabric material with polyurethane, a soft polyurethane foam obtained by physical and chemical foaming, and a polyvinyl chloride foam.
5. The polishing pad according to claim 1, It is characterized in that The polishing top layer is a polyurethane elastomer having a cavity structure made of any one of polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene; and / or, The filament layer block C1 and the filament layer block C are felts obtained by impregnating non-woven fabrics with polyurethane; and / or, The upper bonding layer is a heat-sensitive adhesive bonding layer; and / or, The lower adhesive layer is a pressure-sensitive adhesive layer; and / or, The supporting bottom layer is a film with high tensile strength and a smooth surface.
6. The polishing pad according to claim 5, It is characterized in that The upper adhesive layer is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; the thickness of the substrate is 20-120 μm, the thickness of the adhesive coating on both sides of the substrate is 10-150 μm, and the overall thickness of the heat-sensitive adhesive layer is 40-420 μm.
7. The polishing pad according to claim 5, It is characterized in that The lower adhesive layer is a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; the thickness of the substrate is 20-120 µm, the thickness of the adhesive coating on the upper side of the substrate is 10-150 µm, the thickness of the adhesive coating on the lower side of the substrate is 5-50 µm, and the overall thickness of the pressure-sensitive adhesive layer is 35-320 µm.
8. The polishing pad according to claim 5, It is characterized in that The supporting bottom layer is any one of a polyethylene terephthalate film, a polyethylene film and a polyvinyl chloride film with a release agent coated on the surface.
9. The method for preparing the polishing pad according to any one of claims 1 to 8, It is characterized in that The method comprises the steps of sequentially bonding and laminating the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer.
10. Use of the polishing pad according to any one of claims 1 to 8 or the polishing pad prepared by the preparation method according to claim 9 in chemical mechanical polishing.