A fast-setting high-strength sludge solidifying agent and sludge solidifying process
By using fast-condensing high-strength sludge curing agent made of slag powder and other materials, the problems of slow curing speed and low strength of sludge are solved, rapid curing and efficient utilization of sludge are achieved, and moisture content and anaerobic growth are reduced. Odor risk, suitable for biomass fuel applications.
Patent Information
- Application Number
- CN202410585028.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-13
AI Technical Summary
In the existing sludge treatment technology, the sludge cures slowly, easily produces anaerobic odor, occupies a large amount of storage and maintenance sites, and the solidified sludge is low, making it difficult to achieve rapid turnover and efficient utilization.
Fast-condensing high-strength sludge curing agent made of slag powder, gypsum powder, calcium carbide slag powder, crystal nucleus promoter, pore-forming agent and composition stabilizer, form ettringite through rapid curing reaction, reduces sludge moisture and strengthens Curing strength, combining pore-forming agent and stabilizer to avoid anaerobic fermentation and structural instability.
The sludge has been quickly cured within 60 minutes, the compressive strength reaches 1500~2500KN/m2, and the water content is reduced to 5~10%, which is easy to ship and store, avoids anaerobic odor, and is suitable for waste incineration power generation and kiln furnaces. Use biomass fuel.
Smart Images

Figure CN118405938B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of urban sludge treatment, and in particular relates to a fast-setting high-strength sludge solidifying agent and a sludge solidification process. Background Art
[0002] Sludge is the product of urban sewage after filter pressing. It has a complex composition and is a collection of organic and inorganic substances. It not only contains up to 85% to 90% water, but also contains fungi, insect eggs, and organic matter that is easy to anaerobic and stink. Because polyacrylamide (PAM) is added in the sewage treatment process to flocculate and settle particles, the water content of the sludge after filter pressing is high. Traditional sludge treatment is to pile it up on the site to reduce the moisture by natural drying, and then enter the kiln for incineration; the other is to dry the sludge in a drying furnace, reduce the moisture, and then incinerate it as biomass fuel. It is difficult to reduce the moisture by natural drying, so the sludge after filter pressing has difficulties in stacking, storage, transportation, and subsequent treatment, and it is easy to produce anaerobic stink, affecting environmental quality.
[0003] In order to solve the problem of high water content in urban sludge, the current disclosed patents and published literature on the solidification of urban sludge mainly focus on the following aspects: (1) Chinese patent application No. 2020110475996 discloses "An inorganic mineral composite dehydrating agent for rapid dehydration of sludge and its preparation method and application". The application scheme uses more than 20% of cement, limestone and other inorganic substances, and composite inorganic and organic flocculants to prepare a dehydrating agent. Its function is to quickly and efficiently dehydrate sewage in the filter press link to obtain sludge with a moisture content of less than 40%, and then dry the sludge by natural drying or drying in a drying field or using drying equipment. (2) The application with Chinese patent application number 2020111122084 discloses "Sludge solidifying agent and its preparation method, sludge solidification and stabilization treatment method". The application scheme uses 35% cement, quicklime, fly ash, bentonite, coal slag, titanium slag and ferrous sulfate to prepare a sludge solidifying agent. After the solidifying agent and sludge are evenly mixed, it needs to be cured in the curing yard for 28 days to obtain solidified sludge. Its main purpose is to use the solidified sludge as engineering soil to improve its anti-freezing and thawing properties. (3) The application with Chinese patent application number 2020113329046 discloses "A composite sludge dehydration solidifying agent and its preparation method and application". The application scheme uses about 50% composite cement, cationic polyacrylamide, nano calcium, polysilicon aluminum sulfate, polyamine, and polyaspartic acid to prepare it. It is used for sludge dehydration. It uses suction filtration to reduce the water content of the sludge and use the sludge as engineering soil.
[0004] At the same time, the following problems exist in the solidification of sludge in the currently disclosed patents and published literature: (1) Most of them use cement, lime, etc. as the main raw materials of the solidifying agent. The solidification reaction is extremely slow and the solidified sludge needs to be cured for more than 28 days, which takes up a lot of space. At the same time, the amount of cement used is large and the carbon emissions are large; (2) The main addition link is during the sludge filtration process. The water content of the sludge produced reaches 40%, and the water content of the sludge is still relatively high; (3) The strength of the solidified sludge is low, only 650KN / m 2 , its stacking and storage still occupy a large amount of space, and it is impossible to achieve the goal of small sludge space occupation, fast turnover, convenient stacking, storage and transportation; (4) Change the current large-scale application of the filter press method to adopt the suction filtration method. The sewage treatment plant needs to dismantle the existing equipment and replace it with the filter press equipment, which requires a large investment and is difficult to apply in practice; (5) The solidified sludge is used as engineering soil, but the technical solution does not solve the harm of viruses and bacteria in the sludge to the environment. At the same time, it wastes the high calorific value of the sludge itself, which is not conducive to my country's "energy conservation" development concept. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention discloses a fast-setting high-strength sludge solidifying agent and a sludge solidification process. Various types of solid waste are used as the main raw materials, and the sludge with high water content can be quickly and highly solidified to prepare granular or brick-shaped sludge biomass fuel with low water content, which can be bagged, stacked, etc., to facilitate the rapid turnover of sludge, solve the problems of slow sludge solidification, easy anaerobic odor, and occupying a large amount of storage and maintenance space, and achieve the goal of "solidification and use" of sludge.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 45-60% slag powder, 25-34% gypsum powder, 1-20% carbide slag powder, 2-5% crystal nucleation accelerator, 3-5% pore former and 0.02-0.04% composition stabilizer.
[0008] Preferably, the crystal nucleus accelerator is made of the following raw materials in weight percentage: 15-25% of 72.5 grade sulphoaluminate clinker powder, 67-74% of calcium hydroxide powder, and 8-11% of sodium metaaluminate.
[0009] Preferably, the specific surface area of the 72.5 grade sulphoaluminate clinker powder is ≥450m 2 / kg, 28-day compressive strength ≥72.5MPa; Ca(OH) in calcium hydroxide powder 2 Content ≥90%; sodium aluminate is powder, NaAlO 2 Content ≥60%.
[0010] Preferably, the pore-forming agent is sodium dodecylbenzene sulfonate powder, and the content of sodium dodecylbenzene sulfonate is ≥80%.
[0011] Preferably, the composition stabilizer is sodium citrate powder, and the sodium citrate content is ≥80%.
[0012] Preferably, the specific surface area of the slag powder is ≥400m 2 / kg,Al 2 O 3 Content ≥16.5%, 7d activity index ≥80%, 28d activity index ≥105%. The main function of slag powder is to provide the glassy active Al required for the curing reaction. 2 O 3 .
[0013] Preferably, the specific surface area of the carbide slag powder is ≥400m 2 / kg.
[0014] Preferably, the specific surface area of the gypsum powder is ≥500m 2 / kg.
[0015] Slag powder, gypsum powder, carbide slag powder, crystal nucleation promoter, pore former and composition stabilizer are mixed according to the set ratio, accurately measured by a measuring scale, and the measurement error of each material is required to be controlled within ±1%. The materials are conveyed into a mixer through a conveying device, stirred and mixed for 20 minutes, and all the materials are evenly mixed to obtain the fast-setting and high-strength sludge solidifying agent of the present invention.
[0016] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent of the present invention comprises the following steps:
[0017] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a conveyor;
[0018] (2) The sludge in the intermediate bin is weighed and then transported to the double-shaft high-power mixer;
[0019] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after being weighed. The amount of solidifying agent is 10% to 20% of the sludge mass. The double-shaft mixer is stirred for 2 to 3 minutes to mix evenly.
[0020] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0021] The conveyor of the present invention can be a belt conveyor or a screw conveyor. The weighing method of the sludge in the present invention is screw weighing.
[0022] The sludge solidification reaction equation in the present invention is as follows:
[0023] CaSO 4 0.5H 2 O+1.5H 2 O→CaSO 4 ·2H 2 O
[0024] Ca 4 Al 6 SO 16 +NaAlO 2 +Ca(OH) 2 +CaSO 4 ·2H 2 O→3CaO·Al 2 O 3 ·3CaSO 4 ·32H 2 O
[0025] 6CaO+3Al 2 O 3 +3CaSO 4 ·2H 2 O+26H 2 O→3CaO·Al 2 O 3 ·3CaSO 4 ·32H 2 O
[0026] The role of the crystal nucleus promoter in the present invention is to provide crystal nucleus seeds for accelerating the sludge solidification reaction, and to achieve a large amount of ettringite (3CaO·Al 2 O 3 ·3CaSO 4 ·32H 2 O) is formed. The crystal structure of ettringite has the following remarkable characteristics: first, it is a coarse needle-shaped crystal that runs through the whole structure of the sludge to form a "interlaced" microstructure. At the same time, the formation of ettringite causes a volume expansion of 125%, which can further squeeze the loose space of the sludge. The above two effects make the sludge solidifying agent have the characteristics of fast setting and high strength; second, the molecular structure of ettringite is a double-layer chemical structure. 1 mol of ettringite can chemically combine with 32 mol of free water. Therefore, it reacts quickly to form ettringite at an extremely fast speed, which can absorb the free water in the sludge very quickly and in large quantities, reduce the free water content of the sludge, and achieve the purpose of "curing and using immediately".
[0027] The pore-forming agent sodium dodecylbenzene sulfonate can quickly form a large number of serial pores with a pore size of ≤0.1mm during the sludge solidification reaction. The pore structure can be connected to the air to ensure that the solidified sludge is breathable inside, thereby inhibiting the anaerobic fermentation of organic matter in the sludge and avoiding the generation of odor, which affects the surrounding environment and personnel health. At the same time, the serial small pores are also conducive to the efficient combustion of solidified sludge particles or bricks.
[0028] Because the reaction speed of calcium sulfonate in the present invention is extremely fast, the solidified sludge is prone to "softening and bleeding" phenomenon, that is, the calcium sulfonate crystal structure formed at an extremely fast speed is unstable. Although it can combine 32 free waters at an extremely fast speed, it is also very easy to lose 32 crystal waters, that is, it absorbs water quickly, but loses water quickly, so that the water form changes from chemically bound water to free water, and the macroscopic "softening and bleeding" phenomenon is shown. Experimental studies have found that the present invention uses sodium citrate as a stabilizer, which can well stabilize the calcium sulfonate crystals formed at an extremely fast speed, and effectively avoid the "softening and bleeding" phenomenon. At the same time, experimental studies have found that sodium citrate can also effectively resist the destructive effects of arid environments and carbon dioxide in the air on the calcium sulfonate crystal structure. Therefore, the solidified sludge of this technical solution can be stored for a long time, avoiding the problems of weathering and strength reduction caused by the unstable calcium sulfonate crystal structure.
[0029] The dosage of the sludge solidifying agent of the present invention is 10-20% of the sludge mass. When in use, after the current traditional sewage treatment plant filter press process equipment, a belt conveyor, a storage intermediate bin, a biaxial strong mixer, a solidifying agent storage bin, a screw conveyor, a granulator or a brick press, a bagging machine, a stacking machine and other equipment can be added to form a complete set of sludge treatment process flow. The sludge particles or bricks treated by the process steps of the present invention can be transported to a waste incineration power plant or a kiln factory, and can also be used as a biomass fuel.
[0030] The beneficial effects of the present invention are as follows:
[0031] 1. The present invention adopts the synergistic effect of a crystal nucleation promoter, a pore former and a composition stabilizer composed of specific components, and utilizes a large amount of metallurgical slag powder and gypsum powder to prepare a fast-setting and high-strength sludge solidifying agent. The solidifying agent can quickly solidify the sludge within 60 minutes, does not occupy too much space and turnover time, and achieves the goal of "solidification and immediate use" of the sludge.
[0032] 2. The present invention innovatively uses sodium dodecylbenzene sulfonate as a pore-forming agent in sludge solidification, which can form serial pores with a pore size of ≤0.1 mm in the solidified sludge, which can avoid anaerobic stink of organic matter in the sludge and avoid harm to the environment and human health. At the same time, the presence of a large number of pores in the solidified sludge is conducive to the efficient combustion of the sludge, which is of great significance for the use of solidified sludge for waste incineration power generation and biomass fuel for kilns.
[0033] 3. The fast-setting high-strength sludge solidifying agent provided by the present invention can final set the sludge within 3 to 10 minutes and completely harden within 30 to 60 minutes, and the compressive strength can reach 1500 to 2500 KN / m 2 The compressive strength is much higher than the currently disclosed technology. The moisture content of the solidified sludge reaches 5~10%, which is also much lower than the currently disclosed sludge solidification technology. It has the characteristics of rapid shipment, storage and use.
[0034] 4. The process of solidifying sludge by using the fast-setting high-strength sludge solidifying agent described in the present invention can be connected to the existing equipment of the current sewage treatment plant, and has the characteristics of simple equipment, low investment, and strong operability. The produced sludge solidified particles or solidified bricks can be used for waste incineration power generation or biomass fuel for kilns, and have high economic value and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a process flow chart of solidifying sludge according to the present invention. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below with reference to specific embodiments.
[0037] In the following embodiments, the slag powder is made from blast furnace slag by the India-Pakistan method. After grinding, its specific surface area is ≥400m 2 / kg,Al 2 O 3 Content ≥16.5%, 7d activity index ≥80%, 28d activity index ≥105%. Specific surface area of carbide slag powder ≥400m 2 / kg. Gypsum powder, specific surface area ≥500m 2 / kg. 72.5 grade sulphoaluminate clinker powder requires a specific surface area of ≥450m 2 / kg, 28-day compressive strength ≥72.5MPa. Ca(OH) 2 Content ≥90%, specific surface area ≥500m 2 / kg. Sodium aluminate is powder, NaAlO 2 Content ≥60%. Content of sodium dodecylbenzene sulfonate in sodium dodecylbenzene sulfonate powder ≥80%. Content of sodium citrate in sodium citrate powder ≥80%.
[0038] Example 1
[0039] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 50% slag powder, 25% gypsum powder, 19.98% carbide slag powder, 2% crystal nucleus accelerator, 3% pore former and 0.02% composition stabilizer.
[0040] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 18% of 72.5 grade sulphoaluminate clinker powder, 74% of calcium hydroxide powder and 8% of sodium metaaluminate.
[0041] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 1, comprising the following steps:
[0042] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0043] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0044] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 10% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-1;
[0045] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0046] Example 2
[0047] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 55% slag powder, 25% gypsum powder, 13.47% carbide slag powder, 3% crystal nucleation accelerator, 3.5% pore former and 0.03% composition stabilizer.
[0048] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 18% of 72.5 grade sulphoaluminate clinker powder, 74% of calcium hydroxide powder and 8% of sodium metaaluminate.
[0049] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 2 comprises the following steps:
[0050] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0051] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0052] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 13% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-2;
[0053] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0054] Example 3
[0055] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 55% slag powder, 30% gypsum powder, 6.97% carbide slag powder, 4% crystal nucleation accelerator, 4% pore former and 0.03% composition stabilizer.
[0056] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 18% of 72.5 grade sulphoaluminate clinker powder, 74% of calcium hydroxide powder and 8% of sodium metaaluminate.
[0057] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 3, comprising the following steps:
[0058] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0059] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0060] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 16% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-3;
[0061] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0062] Example 4
[0063] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 58% slag powder, 31% gypsum powder, 1.46% carbide slag powder, 4.5% crystal nucleation accelerator, 5% pore former and 0.04% composition stabilizer.
[0064] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 18% of 72.5 grade sulphoaluminate clinker powder, 74% of calcium hydroxide powder and 8% of sodium metaaluminate.
[0065] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 4 comprises the following steps:
[0066] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0067] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0068] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 20% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-4.
[0069] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0070] Example 5
[0071] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 58.5% slag powder, 32% gypsum powder, 1.46% carbide slag powder, 4% crystal nucleation accelerator, 4% pore former and 0.04% composition stabilizer.
[0072] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 23% of 72.5 grade sulphoaluminate clinker powder, 68% of calcium hydroxide powder and 9% of sodium metaaluminate.
[0073] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 5 comprises the following steps:
[0074] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0075] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0076] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 13% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-5.
[0077] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0078] Example 6
[0079] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 59.1% slag powder, 31.86% gypsum powder, 1.0% carbide slag powder, 4% crystal nucleation accelerator, 4% pore former and 0.04% composition stabilizer.
[0080] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 23% of 72.5 grade sulphoaluminate clinker powder, 68% of calcium hydroxide powder and 9% of sodium metaaluminate.
[0081] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 6 comprises the following steps:
[0082] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0083] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0084] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 14% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-6;
[0085] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0086] Example 7
[0087] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 59.0% slag powder, 30.96% gypsum powder, 1.0% carbide slag powder, 4.5% crystal nucleation accelerator, 4.5% pore former and 0.04% composition stabilizer.
[0088] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 25% of 72.5 grade sulphoaluminate clinker powder, 64% of calcium hydroxide powder and 11% of sodium metaaluminate.
[0089] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 7, comprising the following steps:
[0090] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0091] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0092] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 17% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-7;
[0093] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0094] Example 8
[0095] A fast-setting high-strength sludge solidifying agent is prepared from the following raw materials in percentage by weight: 59.96% slag powder, 30.0% gypsum powder, 1.0% carbide slag powder, 5% crystal nucleation accelerator, 4.0% pore former and 0.04% composition stabilizer.
[0096] The crystal nucleus accelerator is made of the following raw materials in parts by weight: 25% of 72.5 grade sulphoaluminate clinker powder, 64% of calcium hydroxide powder and 11% of sodium metaaluminate.
[0097] A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent prepared in Example 8 comprises the following steps:
[0098] (1) The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor;
[0099] (2) The sludge in the intermediate bin is weighed by a spiral weighing scale and then transported to a double-shaft high-power mixer;
[0100] (3) The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after spiral weighing. The amount of solidifying agent is 20% of the sludge mass. The double-shaft mixer is stirred for 3 minutes until the mixture is evenly mixed and marked as GHWN-8;
[0101] (4) The evenly mixed solidified sludge is transported to a granulator or brick press via a screw conveyor to be made into granules or standard bricks. It can be stored, transported and used after 60 minutes.
[0102] Comparative Example 1
[0103] A fast-setting high-strength sludge solidifying agent, whose formula composition is basically the same as that of Example 1, except that it does not contain a crystal nucleation promoter; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-1.
[0104] Comparative Example 2
[0105] A fast-setting high-strength sludge solidifying agent, whose formula composition is basically the same as that of Example 1, except that it does not contain a pore-forming agent; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-2.
[0106] Comparative Example 3
[0107] A fast-setting, high-strength sludge solidifying agent, the formulation composition of which is basically the same as that of Example 1, except that it does not contain a composition stabilizer; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-3.
[0108] Comparative Example 4
[0109] A fast-setting, high-strength sludge solidifying agent, the formulation of which is basically the same as that of Example 1, except that it does not contain a pore-forming agent or a composition stabilizer; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-4.
[0110] Comparative Example 5
[0111] A fast-setting, high-strength sludge solidifying agent, the formulation of which is basically the same as that of Example 1, except that it does not contain a crystal nucleation promoter or a composition stabilizer; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-5.
[0112] Comparative Example 6
[0113] A fast-setting, high-strength sludge solidifying agent, the formulation of which is basically the same as that of Example 1, except that it does not contain a crystal nucleation promoter or a pore-forming agent; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-6.
[0114] Comparative Example 7
[0115] A fast-setting, high-strength sludge solidifying agent, the formulation of which is basically the same as that of Example 1, except that it does not contain a crystal nucleation promoter, a pore-forming agent, or a composition stabilizer; and the mixture in step (3) of the sludge solidifying process is marked as DBWN-7.
[0116] In order to clarify the performance characteristics of the products and application products of the present invention, comparative example 8 was prepared according to the proportion in "An inorganic mineral composite dehydrating agent for rapid dehydration of sludge, its preparation method and application" disclosed in Chinese patent CN202011047599.6. The specific composition is as follows: 20% PO52.5 cement, 50% aluminate cement, 10% fly ash, 15% anhydrite, 5% limestone and 5% composite flocculant (a composite of polyaluminum chloride and polyaluminum sulfate in a mass ratio of 1:1). According to the method disclosed in its specification, the curing agent of comparative example 8 prepared was stirred and mixed with each other for 3 minutes at 2.5% of the sludge mass, and marked as DBWN-8.
[0117] The products GHWN-1, GHWN-2, GHWN-3, GHWN-4, GHWN-5, GHWN-6, GHWN-7, GHWN-8 prepared in Examples 1-8 and the curing agents prepared in Comparative Examples 1-8 were tested for the change in setting time using a Vicat instrument, and were molded into 70.7 mm × 70.7 mm × 70.7 mm cubic test molds, and the test pieces were placed under a standard curing system for curing for 60 minutes, and then demolded for compressive strength testing. After the compressive strength test, the test block samples were taken and the moisture content of the solidified sludge was tested in a drying oven at 45°C in a ventilated environment. The results are shown in Table 1.
[0118] Table 1 Performance comparison between the example products and the comparative examples
[0119]
[0120] It can be seen from the data in Table 1 above that the fast-setting high-strength sludge solidifying agent prepared in Examples 1-8 can quickly solidify the sludge in as short as 10 minutes, and has the advantages of shortened coagulation time and high compressive strength. It can be applied to the rapid treatment of urban sludge to achieve the requirement of immediate solidification and immediate use. It can be seen from the data of Comparative Examples 1-3 that on the basis of the formula of the present invention, any two components of the crystal nucleation promoter, pore-forming agent and composition stabilizer are contained, and the use effect of the product of Examples 1-8 is obviously much worse in terms of final setting time, compressive strength and moisture content; it can be seen from the data of Comparative Examples 4-6 that on the basis of the formula of the present invention, any one of the components of the crystal nucleation promoter, pore-forming agent and composition stabilizer is contained, and the use effect of the product is also poor; the data of Comparative Examples 7-8 also show that when the sludge solidifying agent does not contain the crystal nucleation promoter, pore-forming agent and composition stabilizer of the present invention, the effect of solidifying the sludge is poor. This is mainly due to the synergistic effect of the crystal nucleation promoter, pore former and composition stabilizer contained in the present invention. After the combined effect, the curing agent can final coagulate the sludge within 3 to 10 minutes and completely harden within 30 to 60 minutes, and the compressive strength can reach 1500 to 2500 KN / m 2 The moisture content of the solidified sludge is 5~10%, which does not take up too much space and turnover time, and achieves the goal of "solidification and immediate use" of the sludge, and has high economic value and application value.
[0121] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A fast-setting high-strength sludge solidifying agent, characterized in that: It is made of the following raw materials in weight percentage: 45-60% slag powder, 25-34% gypsum powder, 1-20% calcium carbide slag powder, 2-5% crystal nucleation promoter, 3-5% pore former, and 0.02-0.04% composition stabilizer; The crystal nucleus accelerator is made of the following raw materials in weight percentage: 15-25% of 72.5 grade sulphoaluminate clinker powder, 67-74% of calcium hydroxide powder, and 8-11% of sodium metaaluminate; The pore-forming agent is sodium dodecylbenzene sulfonate powder, and the content of sodium dodecylbenzene sulfonate is ≥80%; The composition stabilizer is sodium citrate powder, and the sodium citrate content is ≥80%.
2. The fast-setting high-strength sludge solidifying agent according to claim 1, characterized in that: The specific surface area of the 72.5 grade sulphoaluminate clinker powder is ≥450m 2 / kg, 28-day compressive strength ≥72.5MPa; Ca(OH)2 content in calcium hydroxide powder ≥90%; sodium aluminate is powder, NaAlO2 content ≥60%.
3. The fast-setting and high-strength sludge solidifying agent according to claim 1, characterized in that: The specific surface area of the slag powder is ≥400m 2 / kg, Al2O3 content ≥16.5%, 7d activity index ≥80%, 28d activity index ≥105%.
4. The fast-setting high-strength sludge solidifying agent according to claim 1, characterized in that: The specific surface area of the carbide slag powder is ≥400m 2 / kg.
5. The fast-setting and high-strength sludge solidifying agent according to claim 1, characterized in that: The specific surface area of the gypsum powder is ≥500m 2 / kg.
6. A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent according to any one of claims 1 to 5, characterized in that: It includes the following steps: The sludge after being filtered by the filter press is transported to the sludge storage intermediate bin via a belt conveyor; The sludge in the intermediate bin is transported to the double-shaft high-power mixer after being weighed; The fast-setting high-strength sludge solidifying agent is transported from the solidifying agent storage bin to the double-shaft high-power mixer after being weighed. The amount of the solidifying agent is 10% to 20% of the sludge mass. The double-shaft mixer is stirred for 2 to 3 minutes to mix evenly. The evenly mixed solidified sludge is conveyed to a granulator or brick press via a conveyor to be made into granules or standard bricks, which can be stored, transported and used after 60 minutes.
7. A process for solidifying sludge using the fast-setting high-strength sludge solidifying agent according to claim 6, characterized in that: The conveyor is a belt conveyor or a screw conveyor; the metering and weighing method is screw metering and weighing.