A high-viscosity, stain-resistant polyurethane hot-melt adhesive and preparation method thereof

By introducing fluorine atoms and photocatalytic nanoparticles into the polyurethane hot melt adhesive, combined with the steric hindrance structure, the problem of stain resistance and water resistance of the polyurethane hot melt adhesive is solved, and the high viscosity, stain resistance and self-cleaning ability are improved. .

CN118406460BActive Publication Date: 2024-10-11SHANDONG HIGHDEV NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410888483.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Polyurethane hot melt adhesive easily absorbs dust, water molecules and other pollutants on the surface of architectural glass, and its stain resistance and water resistance are poor, making it difficult to meet the increasing actual demand.

Method used

Introducing fluorine atoms or long-chain alkane structures with lower surface energy into the polyurethane molecular chain, adding nanoparticles with photocatalytic effect, and protecting the easily hydrolyzable groups in the molecular chain through steric hindrance structures to improve the hydrophobicity of the adhesive film , self-cleaning ability and water resistance.

Benefits of technology

It achieves the high viscosity, stain resistance and water resistance of polyurethane hot melt adhesive, enhances its self-cleaning ability and heat resistance, and significantly improves the ability to degrade pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of hot melt adhesives, and discloses a high-viscosity, stain-resistant polyurethane hot melt adhesive and a preparation method thereof. The polyurethane hot melt adhesive prepared by the present invention includes the following raw materials in parts by weight: 20-30 parts of polyester diols, 25-35 parts of polyether diols, 12-20 parts of functional polyols, 35-45 parts of diisocyanates, 3-6 parts of chain extenders, 0.2-0.5 parts of catalysts, and 2-5 parts of modified titanium dioxide; the polyurethane hot melt adhesive provided by the present invention is a polyurethane hot melt adhesive synthesized with polyols and isocyanates as main raw materials, and then by introducing functional polyols, the hydrophobicity, stain resistance and water resistance of polyurethane are improved; modified titanium dioxide is introduced, and its excellent photocatalytic degradation ability is utilized to improve the self-cleaning ability of the substrate. Therefore, the polyurethane hot melt adhesive prepared by the present invention can be widely used in the fields of architectural glass, plastics, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hot melt adhesives, and in particular to a high-viscosity, stain-resistant polyurethane hot melt adhesive and a preparation method thereof. Background Art

[0002] Polyurethane hot melt adhesive has excellent resilience, wear resistance, high thermal bonding strength with the substrate, environmental protection and safety, simple operation process, and has developed rapidly in recent years. It is widely used in clothing, automobiles, glass, construction, papermaking, etc., and cannot be replaced by ordinary materials. However, with the increase in actual demand, the requirements for certain properties of polyurethane hot melt adhesive have also increased. For example: (1) For hot melt adhesive used on the surface of architectural glass, considering the disadvantage that traditional hot melt adhesive is easy to absorb pollutants such as dust and water molecules, it is necessary to improve the stain resistance and self-cleaning ability of hot melt adhesive; (2) Although polyurethane hot melt adhesive has excellent viscosity, its molecular chain contains a large number of easily hydrolyzed urethane bonds, resulting in relatively poor water resistance of polyurethane hot melt adhesive. Therefore, it is also necessary to improve the water resistance of polyurethane hot melt adhesive.

[0003] In view of the above shortcomings of the hot melt adhesive, it is modified: fluorine atoms or long-chain alkane structures with low surface energy are introduced into the polyurethane molecular chain. These will migrate to the surface of the film during the curing process of the hot melt adhesive, making the surface of the film have a certain hydrophobicity, thereby making the film stain-resistant; nanoparticles with photocatalytic effect are added to the polyurethane hot melt adhesive, so that it has the ability to photocatalytically degrade organic matter, dust and other substances on the surface of the film, thereby making the film self-cleaning; in addition, a structure with large steric hindrance is introduced into the polyurethane molecular chain, and the steric hindrance effect is used to protect the easily hydrolyzed groups in the molecular chain, thereby improving the water resistance of the film. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a high-viscosity and stain-resistant polyurethane hot melt adhesive and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-viscosity, stain-resistant polyurethane hot melt adhesive comprises the following raw materials in parts by weight: 20-30 parts of polyester diol, 25-35 parts of polyether diol, 12-20 parts of functional polyol, 35-45 parts of diisocyanate, 3-6 parts of chain extender, 0.2-0.5 parts of catalyst, and 2-5 parts of modified titanium dioxide;

[0007] The functional polyol is prepared by the following steps:

[0008] Step A1, add cyanuric chloride and acetonitrile to a flask, stir for 30 minutes in an ice water bath, and record it as solution A; add perfluorohexylethyl alcohol and sodium hydroxide to a beaker containing acetonitrile, ultrasonically disperse for 20 minutes, and record it as solution B. Slowly drop half of solution B into solution A, and adjust the system temperature to 0-5°C. After the dropwise addition is completed, continue to react for 3-4 hours, then heat to 45-55°C, and then slowly drop the remaining solution B. After the dropwise addition is completed, continue to react for 8-10 hours to obtain intermediate product 1;

[0009] Further, the dosage ratio of cyanuric chloride and acetonitrile in solution A is 0.01-0.02 mol: 100 mL, and the dosage ratio of perfluorohexylethyl alcohol, sodium hydroxide and acetonitrile in solution B is 0.02-0.04 mol: 0.8-1.6 g: 100 mL;

[0010] Step A2, add tris(hydroxymethyl)aminomethane and sodium hydroxide into deionized water, stir and mix evenly, then slowly drop the mixture into the intermediate product 1, and maintain the system temperature at 80-90°C. After the dropwise addition is completed, keep the temperature under reflux for 10-12h. After the reaction is completed, cool to room temperature, filter, wash, and place in a vacuum drying oven at 80°C for 10h to obtain a functional polyol;

[0011] Furthermore, the usage ratio of tris(hydroxymethyl)aminomethane, sodium hydroxide and deionized water is 0.01-0.02 mol: 0.01-0.02 mol: 100 mL.

[0012] The modified titanium dioxide is prepared by the following steps:

[0013] Step B1, adding thiourea to a reactor containing deionized water and stirring and mixing uniformly, recorded as solution C; then dispersing titanium dioxide in a flask containing deionized water and stirring and mixing uniformly, adding solution C and nickel chloride hexahydrate and ultrasonically dispersing for 30 minutes, then adding ethanol, and raising the system temperature to 35-45°C for ultrasonic treatment for 30 minutes, adjusting the pH to 3-7, transferring the mixed solution to an autoclave, and hydrothermally treating at 160-180°C for 6-8 hours, after the reaction is completed, centrifuging, washing, and drying to obtain S / Ni-TiO2 nanomaterials;

[0014] Further, the dosage ratio of titanium dioxide, deionized water, solution C, nickel chloride hexahydrate and ethanol is 1-3 g: 20 mL: 25 mL: 0.48-1.2 g: 20 mL, and the dosage ratio of thiourea and deionized water in solution C is 0.01-0.03 mol: 25 mL;

[0015] Step B2, dispersing the hydrotalcite in a beaker containing deionized water, stirring for 20 minutes, and then ultrasonically treating for 1-2 hours, and then slowly dropping the polyethyleneimine solution, stirring for 30 minutes after the dropping is completed, and then ultrasonically dispersing for 1 hour, and then adding the S / Ni-TiO2 nanomaterial and stirring for 20-40 minutes, and then ultrasonically treating for 1-2 hours, centrifuging, washing, and drying to obtain modified titanium dioxide;

[0016] Furthermore, the dosage ratio of hydrotalcite, deionized water, polyethyleneimine solution and S / Ni-TiO2 nanomaterial is 1g:50mL:10mL:0.5-1.5g, and the polyethyleneimine solution is prepared by mixing polyethyleneimine and deionized water in a dosage ratio of 0.1-0.5g:10mL.

[0017] A method for preparing a high-viscosity, stain-resistant polyurethane hot melt adhesive comprises the following steps:

[0018] Step S1, adding polyester diol, polyether diol, functional polyol and chain extender into a stirrer, stirring at 110-130° C. for 20-40 min, and then dehydrating the mixture under vacuum conditions for 2-3 h to obtain a mixture;

[0019] Step S2, lowering the temperature of the mixture to 50-60°C, adding diisocyanate under nitrogen, then raising the temperature to 90-120°C, stirring and reacting for 2-3 hours, adding a catalyst, and continuing the reaction for 30-50 minutes. After the reaction is completed, adding modified titanium dioxide, and continuing stirring for 30-60 minutes. After the reaction is completed, discharging the material to obtain a polyurethane hot melt adhesive.

[0020] Beneficial effects of the present invention:

[0021] The hot melt adhesive prepared by the present invention is a polyurethane hot melt adhesive synthesized with polyols and isocyanates as main raw materials, and then the hydrophobicity, stain resistance and water resistance of the polyurethane are improved by introducing functional polyols; modified titanium dioxide is introduced, and its excellent photocatalytic degradation ability is utilized to improve the self-cleaning ability of the substrate.

[0022] In the functional polyol, the chlorine atom on melamine is firstly used to undergo a substitution reaction with the hydroxyl group in perfluorohexylethyl alcohol to obtain an intermediate product 1; and then the remaining chlorine atom in the intermediate product 1 is used to react with the amino group in trishydroxymethylaminomethane to generate a functional polyol. Functional polyols use cyanuric chloride as an intermediate, and utilize the chlorine atoms contained in it to react with the hydroxyl or amino groups in the compound (perfluorohexylethyl alcohol, trishydroxymethylaminomethane), thereby introducing fluorinated segments and polyhydroxy structures; the introduction of fluorinated segments improves the stain resistance of the substrate, because fluorine atoms have a lower surface energy, and fluorine atoms migrate to the surface of the substrate during the formation of the hot melt adhesive, thereby reducing the surface energy of the substrate and improving the hydrophobicity and stain resistance of the substrate; in addition, since fluorine atoms have a large steric hindrance and shielding effect, they can effectively protect the surrounding urethane bonds from hydrolysis, thereby improving the water resistance of the polyurethane, and at the same time increase the steric hindrance of the relative movement of fluorine atoms in the polyurethane molecular chain during the heating process, keep the molecular chains relatively dense, reduce the penetration of water molecules, and further improve the water resistance of the substrate; cyanuric chloride, as an intermediate, introduces a triazine structure into the polyurethane molecular chain, thereby improving the heat resistance of the substrate.

[0023] Modified titanium dioxide is based on titanium dioxide, and is doped and modified with thiourea as a sulfur source and nickel chloride hexahydrate as a nickel source to prepare S / Ni-TiO2 nanomaterials; polyethyleneimine is then used as a crosslinking agent to react with the amino groups contained in hydrotalcite and the hydroxyl groups in S / Ni-TiO2 nanomaterials to form a crosslinking structure, and then the S / Ni-TiO2 nanomaterials are loaded on the hydrotalcite to obtain modified titanium dioxide. Modified titanium dioxide is to use titanium dioxide as the catalytic main body of the photocatalyst and then modify it; among them, the doping of the two elements improves the separation efficiency of the photogenerated carriers in titanium dioxide, prolongs the transmission time of the carriers, increases the life span of the photogenerated charges, and further improves the photocatalytic activity of titanium dioxide. The improvement of the photocatalytic activity means that the matrix has better self-cleaning ability; due to its special layered structure, hydrotalcite is rich in water molecules and hydroxyl groups between its layers and on its surface, and these water molecules and hydroxyl groups can react with h + The reaction generates hydroxyl radicals, which can oxidize organic pollutants on the surface of the substrate, thus having a certain self-cleaning ability. At the same time, the layered structure of hydrotalcite prolongs the penetration of water molecules into the substrate and improves the water resistance of the substrate. In addition, the introduction of polyethyleneimine also improves the heat resistance of the substrate. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] Functional polyols are prepared by the following steps:

[0027] Step A1, add 0.01 mol of cyanuric chloride and 100 mL of acetonitrile to a flask, stir for 30 min in an ice-water bath, and record it as solution A; add 0.02 mol of perfluorohexylethyl alcohol and 0.8 g of sodium hydroxide to a beaker containing 100 mL of acetonitrile, and ultrasonically disperse for 20 min, record it as solution B, slowly drop one half of solution B into solution A, and adjust the system temperature to 0°C. After the dropwise addition is completed, continue to react for 3 hours, then heat to 45°C, and slowly drop the remaining solution B. After the dropwise addition is completed, continue to react for 8 hours to obtain intermediate product 1;

[0028] Step A2, add 0.01 mol of tris(hydroxymethyl)aminomethane and 0.01 mol of sodium hydroxide to 100 mL of deionized water, stir and mix evenly, then slowly drop the mixture into the intermediate product 1, and maintain the system temperature at 80 ° C. After the addition is completed, keep the temperature under reflux for 10 hours. After the reaction is completed, cool to room temperature, filter, wash, and place in a vacuum drying oven at 80 ° C. for 10 hours to obtain a functional polyol.

[0029] Modified titanium dioxide is prepared by the following steps:

[0030] Step B1, add 0.01 mol of thiourea to a reactor containing 25 mL of deionized water and stir and mix evenly, record it as solution C; then disperse 1 g of titanium dioxide in a flask containing 20 mL of deionized water and stir and mix evenly, add 25 mL of solution C and 0.48 g of nickel chloride hexahydrate and ultrasonically disperse for 30 minutes, then add 20 mL of ethanol, and increase the system temperature to 35°C and ultrasonically treat for 30 minutes, adjust the pH to 3, transfer the mixed solution to an autoclave, and hydrothermally treat it at 160°C for 6 hours. After the reaction is completed, centrifuge, wash, and dry to obtain S / Ni-TiO2 nanomaterials;

[0031] Step B2, disperse 1g of hydrotalcite in a beaker containing 50mL of deionized water, stir for 20min, then ultrasonically treat for 1h, then slowly add 10mL of polyethyleneimine solution, after the addition is completed, stir for 30min, then ultrasonically disperse for 1h, then add 0.5g of S / Ni-TiO2 nanomaterial and stir for 20min, ultrasonically treat for 1h, centrifuge, wash and dry to obtain modified titanium dioxide. The polyethyleneimine solution is prepared by mixing polyethyleneimine and deionized water in a dosage ratio of 0.1g:10mL.

[0032] Example 2

[0033] Functional polyols are prepared by the following steps:

[0034] Step A1, add 0.015 mol of cyanuric chloride and 100 mL of acetonitrile to a flask, stir for 30 min in an ice-water bath, and record it as solution A; add 0.03 mol of perfluorohexylethyl alcohol and 1.2 g of sodium hydroxide to a beaker containing 100 mL of acetonitrile, and ultrasonically disperse for 20 min, record it as solution B, slowly drop one half of solution B into solution A, and adjust the system temperature to 2°C. After the dropwise addition is completed, continue to react for 3.5 hours, then heat to 50°C, and slowly drop the remaining solution B. After the dropwise addition is completed, continue to react for 9 hours to obtain intermediate product 1;

[0035] Step A2, add 0.015 mol of tris(hydroxymethyl)aminomethane and 0.015 mol of sodium hydroxide to 100 mL of deionized water, stir and mix evenly, then slowly drop the mixture into the intermediate product 1, and maintain the system temperature at 85 ° C. After the addition is completed, keep the temperature under reflux for 11 hours. After the reaction is completed, cool to room temperature, filter, wash, and place in a vacuum drying oven at 80 ° C. for 10 hours to obtain a functional polyol.

[0036] Modified titanium dioxide is prepared by the following steps:

[0037] Step B1, add 0.02 mol of thiourea to a reactor containing 25 mL of deionized water and stir and mix evenly, record it as solution C; then disperse 2 g of titanium dioxide in a flask containing 20 mL of deionized water and stir and mix evenly, add 25 mL of solution C and 0.75 g of nickel chloride hexahydrate and ultrasonically disperse for 30 minutes, then add 20 mL of ethanol, and increase the system temperature to 40°C for ultrasonic treatment for 30 minutes, adjust the pH to 5, transfer the mixed solution to an autoclave, and hydrothermally treat it at 170°C for 7 hours. After the reaction is completed, centrifuge, wash, and dry to obtain S / Ni-TiO2 nanomaterials;

[0038] Step B2, disperse 1g of hydrotalcite in a beaker containing 50mL of deionized water, stir for 20min, then ultrasonically treat for 1.5h, then slowly add 10mL of polyethyleneimine solution, after the addition is completed, stir for 30min, then ultrasonically disperse for 1h, then add 1g of S / Ni-TiO2 nanomaterial and stir for 30min, ultrasonically treat for 1.5h, centrifuge, wash and dry to obtain modified titanium dioxide. The polyethyleneimine solution is prepared by mixing and stirring polyethyleneimine and deionized water in a dosage ratio of 0.3g:10mL.

[0039] Example 3

[0040] Functional polyols are prepared by the following steps:

[0041] Step A1, add 0.02 mol of cyanuric chloride and 100 mL of acetonitrile to a flask, stir for 30 min in an ice-water bath, and record it as solution A; add 0.04 mol of perfluorohexylethyl alcohol and 1.6 g of sodium hydroxide to a beaker containing 100 mL of acetonitrile, and ultrasonically disperse for 20 min, record it as solution B, slowly drop one half of solution B into solution A, and adjust the system temperature to 5°C. After the dropwise addition is completed, continue to react for 4 hours, then heat to 55°C, and slowly drop the remaining solution B. After the dropwise addition is completed, continue to react for 10 hours to obtain intermediate product 1;

[0042] Step A2, add 0.02 mol of tris(hydroxymethyl)aminomethane and 0.02 mol of sodium hydroxide to 100 mL of deionized water, stir and mix evenly, then slowly drop the mixture into the intermediate product 1, and maintain the system temperature at 90 ° C. After the addition is completed, keep the temperature under reflux for 12 hours. After the reaction is completed, cool to room temperature, filter, wash, and place in a vacuum drying oven at 80 ° C. for 10 hours to obtain a functional polyol.

[0043] Modified titanium dioxide is prepared by the following steps:

[0044] Step B1, add 0.03 mol of thiourea to a reactor containing 25 mL of deionized water and stir and mix evenly, record it as solution C; then disperse 3 g of titanium dioxide in a flask containing 20 mL of deionized water and stir and mix evenly, add 25 mL of solution C and 1.2 g of nickel chloride hexahydrate and ultrasonically disperse for 30 minutes, then add 20 mL of ethanol, and increase the system temperature to 45 ° C and ultrasonically treat for 30 minutes, adjust the pH to 7, transfer the mixed solution to an autoclave, and hydrothermally treat it at 180 ° C for 8 hours. After the reaction is completed, centrifuge, wash, and dry to obtain S / Ni-TiO2 nanomaterials;

[0045] Step B2, disperse 1g of hydrotalcite in a beaker containing 50mL of deionized water, stir for 20min, then ultrasonically treat for 2h, then slowly add 10mL of polyethyleneimine solution, after the addition is completed, stir for 30min, then ultrasonically disperse for 1h, then add 1.5g of S / Ni-TiO2 nanomaterial and stir for 40min, then ultrasonically treat for 2h, centrifuge, wash and dry to obtain modified titanium dioxide. The polyethyleneimine solution is prepared by mixing and stirring polyethyleneimine and deionized water in a dosage ratio of 0.5g:10mL.

[0046] Example 4

[0047] A method for preparing a high-viscosity, stain-resistant polyurethane hot melt adhesive comprises the following steps:

[0048] 20 parts of ethylene glycol-propylene glycol adipate diol, 25 parts of polyethylene glycol, 12 parts of the functional polyol prepared in Example 1, 35 parts of hexamethylene diisocyanate, 3 parts of propylene glycol, 0.2 parts of dibutyltin dilaurate, and 2 parts of the modified titanium dioxide prepared in Example 1;

[0049] Step S1, adding ethylene glycol adipate diol, polyethylene glycol, the functional polyol prepared in Example 1 and propylene glycol into a stirrer, stirring at 110° C. for 20 min, and then dehydrating the mixture under vacuum conditions for 2 h to obtain a mixed material;

[0050] Step S2, lowering the temperature of the mixture to 50°C, adding hexamethylene diisocyanate under nitrogen conditions, then raising the temperature to 90°C, stirring and reacting for 2 hours, adding dibutyltin dilaurate, and continuing the reaction for 30 minutes. After the reaction is completed, adding the modified titanium dioxide prepared in Example 1, and continuing to stir for 30 minutes. After the reaction is completed, discharging the material to obtain a polyurethane hot melt adhesive.

[0051] Example 5

[0052] A method for preparing a high-viscosity, stain-resistant polyurethane hot melt adhesive comprises the following steps:

[0053] 25 parts of ethylene glycol-propylene glycol adipate diol, 30 parts of polyethylene glycol, 15 parts of the functional polyol prepared in Example 2, 40 parts of hexamethylene diisocyanate, 5 parts of propylene glycol, 0.3 parts of dibutyltin dilaurate, and 4 parts of the modified titanium dioxide prepared in Example 2;

[0054] Step S1, adding ethylene glycol adipate diol, polyethylene glycol, the functional polyol prepared in Example 2 and propylene glycol into a stirrer, stirring at 120° C. for 30 min, and then dehydrating the mixture under vacuum conditions for 2.5 h to obtain a mixed material;

[0055] Step S2, lowering the temperature of the mixture to 55°C, adding hexamethylene diisocyanate under nitrogen conditions, then raising the temperature to 110°C, stirring and reacting for 2.5 hours, adding dibutyltin dilaurate, and continuing the reaction for 40 minutes. After the reaction is completed, adding the modified titanium dioxide prepared in Example 2, and continuing to stir for 45 minutes. After the reaction is completed, discharging the material to obtain a polyurethane hot melt adhesive.

[0056] Example 6

[0057] A method for preparing a high-viscosity, stain-resistant polyurethane hot melt adhesive comprises the following steps:

[0058] 30 parts of ethylene glycol-propylene glycol adipate diol, 35 parts of polyethylene glycol, 20 parts of the functional polyol prepared in Example 3, 45 parts of hexamethylene diisocyanate, 6 parts of propylene glycol, 0.5 parts of dibutyltin dilaurate, and 5 parts of the modified titanium dioxide prepared in Example 3;

[0059] Step S1, adding ethylene glycol adipate diol, polyethylene glycol, the functional polyol prepared in Example 3 and propylene glycol into a stirrer, stirring at 130° C. for 40 min, and then dehydrating the mixture under vacuum conditions for 3 h to obtain a mixture;

[0060] Step S2, lowering the temperature of the mixture to 60°C, adding hexamethylene diisocyanate under nitrogen conditions, then raising the temperature to 120°C, stirring and reacting for 3 hours, adding dibutyltin dilaurate, and continuing the reaction for 50 minutes. After the reaction is completed, adding the modified titanium dioxide prepared in Example 3, and continuing to stir for 60 minutes. After the reaction is completed, discharging the material to obtain a polyurethane hot melt adhesive.

[0061] Comparative Example 1

[0062] This comparative example is a polyurethane hot melt adhesive, which differs from Example 6 in that an equal amount of propylene glycol is used to replace the functional polyol prepared in Example 3, and the rest are the same.

[0063] Comparative Example 2

[0064] This comparative example is a polyurethane hot melt adhesive, which differs from Example 6 in that an equal amount of titanium dioxide is used to replace the modified titanium dioxide prepared in Example 3, and the rest are the same.

[0065] The polyurethane hot melt adhesives prepared in Examples 4-6 and Comparative Examples 1-2 were subjected to performance tests:

[0066] Hydrophobicity test: Tested in accordance with GB / T 30693-2014 standard;

[0067] Heat resistance test: Samples were prepared and tested according to GB / T 7124-2008 standard to test the heat resistance of hot melt adhesive. After the sample was cured for 7 days at 25℃ / 50%RH, it was placed in a 120℃ oven for 24 hours, and then its tensile shear strength was tested in a 120℃ high and low temperature tensile testing machine;

[0068] Water resistance test: Through the patch hydrolysis test, soak in 70℃ water bath for 7 days, test the peel strength retention rate;

[0069] Self-cleaning performance: The polyurethane hot melt adhesive was coated on the glass surface, and the samples were obtained after curing. Then, the samples were immersed in a culture dish containing 50 mL of the target solution (20 mg / L methyl orange was used as the target degradation product for the test), and the culture dish was placed in a photocatalytic reaction device. The light source was a 300W xenon lamp. The distance between the sample and the light source was 20 cm. The absorbance of the target degradation product was measured with a 722 visible spectrophotometer. The maximum absorption wavelength of the methyl orange solution at 465 nm was used as the reference position. The absorbance of each sample after irradiation with the xenon lamp was measured regularly to calculate the residual concentration percentage of the methyl orange solution.

[0070] The test results are shown in the following table:

[0071]

[0072] As can be seen from the above table, after the water contact angle test of the polyurethane hot melt adhesive prepared by the present invention, the water contact angle is 108°-115°, and the adhesive film after the surface hot melt adhesive is cured has excellent hydrophobicity, thereby showing excellent stain resistance; after the shear strength and peel strength tests, the shear strength is 8.9-9.1MPa, and the peel strength retention rate is 68%-73%, indicating that the adhesive film has high viscosity, excellent water resistance and heat resistance; after the photocatalytic degradation test with methyl orange as the target degradation product, the residual concentration of methyl orange (after immersion for 14 hours) is 4%-11%, indicating that the adhesive film has excellent self-cleaning ability.

[0073] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A high-viscosity, stain-resistant polyurethane hot melt adhesive, characterized in that: The invention comprises the following raw materials in parts by weight: 20-30 parts of polyester diol, 25-35 parts of polyether diol, 12-20 parts of functional polyol, 35-45 parts of diisocyanate, 3-6 parts of chain extender, 0.2-0.5 parts of catalyst and 2-5 parts of modified titanium dioxide; The functional polyol is prepared by the following steps: Step A1, add cyanuric chloride and acetonitrile to a flask, stir for 30 minutes in an ice water bath, and record it as solution A; add perfluorohexylethyl alcohol and sodium hydroxide to a beaker containing acetonitrile, ultrasonically disperse for 20 minutes, and record it as solution B. Slowly drop half of solution B into solution A, and adjust the system temperature to 0-5°C. After the dropwise addition is completed, continue to react for 3-4 hours, then heat to 45-55°C, and then slowly drop the remaining solution B. After the dropwise addition is completed, continue to react for 8-10 hours to obtain intermediate product 1; Step A2, add tris(hydroxymethyl)aminomethane and sodium hydroxide into deionized water, stir and mix evenly, then slowly drop the mixture into the intermediate product 1, and maintain the system temperature at 80-90°C. After the dropwise addition is completed, keep the temperature under reflux for 10-12h. After the reaction is completed, cool to room temperature, filter, wash, and place in a vacuum drying oven at 80°C for 10h to obtain a functional polyol; The modified titanium dioxide is prepared by the following steps: Step B1, adding thiourea to a reactor containing deionized water and stirring and mixing uniformly, recorded as solution C; then dispersing titanium dioxide in a flask containing deionized water and stirring and mixing uniformly, adding solution C and nickel chloride hexahydrate and ultrasonically dispersing for 30 minutes, then adding ethanol, and raising the system temperature to 35-45°C for ultrasonic treatment for 30 minutes, adjusting the pH to 3-7, transferring the mixed solution to an autoclave, and hydrothermally treating at 160-180°C for 6-8 hours, after the reaction is completed, centrifuging, washing, and drying to obtain S / Ni-TiO2 nanomaterials; Step B2, disperse the hydrotalcite in a beaker containing deionized water, stir for 20 minutes, and then ultrasonically treat for 1-2 hours, then slowly add the polyethyleneimine solution, after the addition is completed, stir for 30 minutes, and then ultrasonically disperse for 1 hour, then add the S / Ni-TiO2 nanomaterial and stir for 20-40 minutes, ultrasonically treat for 1-2 hours, centrifuge, wash, and dry to obtain modified titanium dioxide.

2. A high-viscosity, stain-resistant polyurethane hot melt adhesive according to claim 1, characterized in that: In step A1, the usage ratio of cyanuric chloride and acetonitrile in solution A is 0.01-0.02 mol:100 mL, and the usage ratio of perfluorohexylethyl alcohol, sodium hydroxide and acetonitrile in solution B is 0.02-0.04 mol:0.8-1.6 g:100 mL.

3. The high-viscosity, stain-resistant polyurethane hot melt adhesive according to claim 1, characterized in that: In step A2, the usage ratio of tris(hydroxymethyl)aminomethane, sodium hydroxide and deionized water is 0.01-0.02 mol: 0.01-0.02 mol: 100 mL.

4. The high-viscosity, stain-resistant polyurethane hot melt adhesive according to claim 1, characterized in that: In step B1, the usage ratio of titanium dioxide, deionized water, solution C, nickel chloride hexahydrate and ethanol is 1-3 g: 20 mL: 25 mL: 0.48-1.2 g: 20 mL, and the usage ratio of thiourea and deionized water in solution C is 0.01-0.03 mol: 25 mL.

5. The high-viscosity, stain-resistant polyurethane hot melt adhesive according to claim 1, characterized in that: In step B2, the dosage ratio of hydrotalcite, deionized water, polyethyleneimine solution and S / Ni-TiO2 nanomaterial is 1g:50mL:10mL:0.5-1.5g, and the polyethyleneimine solution is prepared by mixing polyethyleneimine and deionized water in a dosage ratio of 0.1-0.5g:10mL.

6. A method for preparing the high-viscosity, stain-resistant polyurethane hot melt adhesive according to claim 1, characterized in that: The following steps are involved: Step S1, adding polyester diol, polyether diol, functional polyol and chain extender into a stirrer, stirring at 110-130° C. for 20-40 min, and then dehydrating the mixture under vacuum conditions for 2-3 h to obtain a mixture; Step S2, lowering the temperature of the mixture to 50-60°C, adding diisocyanate under nitrogen, then raising the temperature to 90-120°C, stirring and reacting for 2-3 hours, adding a catalyst, and continuing the reaction for 30-50 minutes. After the reaction is completed, adding modified titanium dioxide, and continuing stirring for 30-60 minutes. After the reaction is completed, discharging the material to obtain a polyurethane hot melt adhesive.