A high temperature resistant bentonite grease composition and preparation method thereof
By using modified castor oil and acidic bentonite thickeners, combined with MoS2/CNTs and calcium carbonate, the problem of poor performance of grease at high temperatures is solved, achieving high stability and wear-resistant lubrication effects.
Patent Information
- Application Number
- CN202410742730.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing greases have poor performance under high temperature conditions, low adhesion, and are easy to separate from equipment. There are also stability and corrosion resistance problems during the preparation process.
Use 320 parts of base oil and modified castor oil for epoxidation, combine diphenylmethane diisocyanate and octadecylamine, use acid bentonite and epoxy resin to prepare a modified bentonite thickener, and add MoS2/CNTs and different Calcium carbonate with particle size is used as a solid filler to form a high temperature, acid and alkali resistant grease.
Significantly improves the viscosity, stability, high temperature resistance, water resistance, wear resistance and friction reduction performance of the grease, extends the service life, and improves the lubrication effect.
Smart Images

Figure CN118406519B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricating grease, in particular to a high temperature resistant bentonite lubricating grease composition and a preparation method thereof. Background Art
[0002] Grease is an important component of industrial lubricants. Grease technology has been continuously developing since its birth, and has formed a series of rich varieties of lubricating products. In recent years, with the development of science and technology and industry, mechanical equipment has developed in the direction of large-scale, miniature, high-speed, heavy-load, vacuum, low temperature, ultra-high precision, automation and intelligence. People's demand for new high-performance lubricating products is also increasing. The development of high-performance grease products with long service life and reliable lubrication in special occasions has huge market prospects and economic benefits, and has become a research and development hotspot in the grease industry in various countries in the world. With the rapid development of my country's economy, many mechanical equipment work under high temperature and high pressure conditions. The lubrication of its parts and components cannot meet the lubrication requirements with general grease, which has accelerated the pace of renewal of my country's grease products. The research and development of high-temperature and high-performance grease is a development trend of grease products.
[0003] The use of traditional grease is below 120℃, such as calcium-based grease, the use temperature is not higher than 60℃, and the use temperature of lithium-based grease is not higher than 120℃. Greases with a maximum use temperature exceeding 120℃ are generally called high-temperature greases, such as composite lithium-based grease, composite barium-based grease, composite aluminum-based grease, polyurea grease, bentonite grease, silicone grease, fluoroether grease, etc. The maximum use temperature limit of composite soap high-temperature grease generally does not exceed 200℃.
[0004] Patent ZL201410026925.3 reports a food-grade grease composition and a preparation method thereof, using base oil, benzoic acid, stearic acid and aluminum isopropoxide trimer as thickeners, adding silicone oil, calcium carbonate, antioxidants, rust inhibitors as auxiliary materials to prepare a food-grade composite aluminum-based grease. However, this type of grease will become thinner, its adhesion will decrease, oil will separate, and it will drip at high temperatures. The grease is easy to separate from the equipment, which will not only cause poor lubrication and damage to the equipment, but may also contaminate food and cause food safety accidents.
[0005] Patent ZL201510206670.3 reports a thickener for thickening high-temperature grease. Ultrafine bentonite is obtained by acidifying and grinding sodium bentonite, and the thickener is obtained after dissolving to prepare high-temperature grease. This improves the disadvantage of grease not being resistant to high temperatures to a certain extent. However, bentonite grease has the disadvantages of poor mechanical stability and poor stability during use, which limits the application of grease.
[0006] Since polyurea grease was discovered in 1954 when investigating the properties of silicone oil, urea-based grease has been rapidly developed and widely used due to its series of excellent properties. However, urea-based grease also has obvious disadvantages, namely, hardening tendency, poor rust resistance, large change in cone penetration after shearing, and severe softening at low shear rates. Patent ZL201210039683.2 reports a urea-based grease composition with excellent shear stability and a preparation method thereof. The urea-based grease provided by the invention includes a base oil, a urea-based thickener, and a surfactant. The thickener is prepared by a one-step saponification reaction of two isocyanates and two amines, and the corresponding additives are added to obtain a diurea-based grease. However, due to the activity difference of amines during the preparation of the thickener, the amines remain in the grease, affecting the corrosion resistance of the grease, and the presence of alkaline substances reduces the stability of the grease.
[0007] Patent ZL201310084582.1 reports a high-performance composite calcium sulfonate-based grease and a preparation method thereof. The composite calcium sulfonate-based grease is formed by high-alkalinity calcium sulfonate, base oil, lauric acid, low-molecular alcohol, high-purity water, boric acid, calcium hydroxide, antioxidant and HL-functional agent. However, during the storage process, the composite calcium sulfonate-based grease has a tendency to decrease in the total surface area of the particle phase due to uneven particle size distribution, thereby accelerating the surface hardening of such grease, while reducing the wear resistance of the grease and the lubrication effect.
[0008] In summary, different types of greases are used in the prior art to improve the performance of the grease and increase its practicality, but there are still shortcomings that need to be improved. The grease has poor high temperature resistance and low adhesion, and the grease is easy to detach from the equipment, reducing the lubrication effect; the residual alkali in the preparation process of urea-based grease has poor oxidation stability, which affects the corrosion resistance of the grease and has low stability; at the same time, it has a tendency to harden, poor rust resistance, and large changes in high-temperature cone penetration; it has poor wear resistance and poor lubrication effect.
[0009] Therefore, a high temperature resistant bentonite grease composition and a preparation method are proposed. Summary of the invention
[0010] The object of the present invention is to provide a high temperature resistant bentonite grease composition and a preparation method thereof. By using 320 parts of base oil and ensuring that the epoxy value of modified castor oil is 2.2 mol / kg, the viscosity of the prepared grease is optimal, the working cone penetration is 245, the oxygen pressure drop is 0.02 KPa, and the stability is optimal; using diphenylmethane diisocyanate, controlling the isocyanate to 20 parts, the obtained grease composition has a dropping point of 260°C and a high temperature cone penetration of 232, and has obvious high temperature resistance; using 20 parts of octadecylamine, 20 parts of KH-550, adding 30 parts of polyurea thickener to the grease to obtain a grease, and the remaining amount of drum water is 2 8g, the water contact angle is 96.8°, and it has good water resistance; 20 parts of modified bentonite thickener prepared by using 20 parts of acidic bentonite and 2 parts of epoxy resin E42, the prepared grease has acid and alkali standard copper sheet corrosion colorimetry of 1a and 1a respectively, and has good corrosion resistance; MoS2 / CNTs is compounded in a mass ratio of 1:4, and 10 parts of calcium carbonate of two different particle sizes are added synergistically as solid fillers, added to the grease, the sintering load value reaches 6080N, the friction coefficient of the grease reaches 0.052, and the average wear spot diameter is 0.35mm, which significantly improves the wear resistance and friction reduction properties of the grease and improves the lubricating effect of the grease.
[0011] To achieve the above object, the present invention provides the following technical solutions:
[0012] A method for preparing a high temperature resistant bentonite grease composition, characterized in that: the high temperature resistant bentonite grease composition comprises 220-420 parts of base oil, 20-50 parts of modified polyurea thickener, 10-40 parts of modified bentonite thickener, 4-40 parts of solid filler, and 12 parts of other additives;
[0013] The base oil is selected from one of base silicone oil, synthetic base oil and modified base oil;
[0014] The modified base oil is prepared by epoxidation of conventional oil with 6-48 parts of 30% H2O2 solution under the action of glacial acetic acid and phosphoric acid;
[0015] The polyurea thickener comprises 10-40 parts of isocyanate and 10-30 parts of octadecylamine, and is prepared by modification with 10-30 parts of a silane coupling agent;
[0016] The modified bentonite thickener comprises 10-40 parts of acidic bentonite, which is modified by 0.5-3 parts of epoxy resin;
[0017] The preparation method of the high temperature resistant bentonite grease composition comprises the following steps:
[0018] The base oil is added into a high-temperature micro-pressure reactor, the temperature of the high-temperature micro-pressure reactor is raised to 100° C., the modified polyurea thickener is added, and the mixture is reacted for 2 hours to obtain a mixed solution; the temperature of the mixed solution is raised to 180° C., the base oil is slowly added again, and the mixture is kept warm for 30 minutes to obtain a reaction solution; the base oil is added into the reaction solution, the mixture is rapidly cooled to 120° C., the mixture is kept warm and stirred for 1 hour, the modified bentonite thickener is added, and the mixture is stirred and expanded at a low speed for 3 hours to obtain a reaction system; the reaction system is cooled to 90° C., the solid filler and the other additives are added, and the stirring is continued for 30 minutes, the mixture is fully mixed and dissolved, and the mixture is stirred evenly to obtain a mixture; the mixture is transferred to a degassing kettle for degassing, filtered, and then packaged to obtain a grease composition.
[0019] Preferably, the base silicone oil is selected from one of methylphenyl silicone oil, methyl silicone oil, ethyl silicone oil and fluorosilicone oil; the synthetic base oil is selected from one of PAO10 and PAO40; and the conventional oil is selected from one of oleic acid and castor oil.
[0020] Preferably, the preparation method of the modified base oil comprises the following steps:
[0021] 60 parts of conventional oil, 9 parts of glacial acetic acid and 0.6 parts of phosphoric acid are added into a three-necked flask, and equipped with a thermometer, a reflux condenser and a dropping funnel to obtain a mixture; the mixture is stirred until the oil bath temperature reaches 70°C, 6-48 parts of 30% H2O2 solution are slowly added dropwise to the mixture, and the mixture is kept warm for reaction for 4 hours to obtain a reaction liquid; the reaction liquid is extracted with petroleum ether, rotary evaporated, and vacuum dried to obtain a modified base oil.
[0022] Preferably, the isocyanate is selected from toluene diisocyanate, diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, p-xylylene diisocyanate, and 4,4-dicyclohexylmethane diisocyanate; and the silane coupling agent is selected from KH-550.
[0023] Preferably, the preparation method of the modified polyurea thickener comprises the following steps:
[0024] Toluene diisocyanate is added to 50 ml of anhydrous tetrahydrofuran solvent, the temperature is raised to 60° C., and the solution is uniformly stirred to obtain an ester solution; octadecylamine is added to the ester solution, the temperature is raised to 90° C., and the reaction is carried out for 1 hour to obtain a reaction solution; KH-550 is slowly added to the reaction solution under heat preservation conditions, and the reaction is carried out for 1 hour to obtain a modified polyurea solution; the modified polyurea solution is cooled to room temperature, washed with methanol 3 times, washed with water 2 times, centrifuged, and vacuum dried to obtain a modified polyurea thickener.
[0025] Preferably, the epoxy resin is selected from one of E42, E44, E51, E52, and bisphenol F epoxy resin.
[0026] Preferably, the preparation method of the modified bentonite thickener comprises the following steps.
[0027] 10 parts of sodium bentonite were calcined at 350°C for 1 hour to prepare dry bentonite; 5 parts of 15% sulfuric acid solution were added to the dry bentonite at a solid-liquid ratio of 2:1, and stirred at 90°C for 30 minutes for acidification treatment, and acidified bentonite was obtained by flocculation, slag removal and filtration; the acidified bentonite was added to 50 parts of distilled water to prepare a bentonite suspension; 1% hexadecyltrimethylammonium bromide was weighed and added to the bentonite suspension to prepare a suspension; epoxy resin was ... an acidified bentonite; epoxy resin was added to the bentonite suspension to prepare an acidified bentonite. Resin, 1.8 parts of curing agent diethylenetriamine, 2 parts of accelerator tetramethyldiamine disulfide, and 2 parts of diluent isoamyl acetate are added to the suspension and stirred at high speed to be evenly dispersed, stirred in a constant temperature oil bath at 80°C for 6 hours, and vacuum degassed to obtain a reaction system; the reaction system is dried in a vacuum drying oven at 90°C for 2 hours until it is dry and agglomerated, and the modified bentonite thickener is obtained by crushing, grinding, and sieving; preferably, the particle size of the modified bentonite thickener is 0.1~200μm.
[0028] Preferably, the solid filler is selected from one or more of molybdenum disulfide, carbon nanotubes, calcium carbonate, polytetrafluoroethylene, melamine cyanurate, graphite, organic molybdenum, zinc oxide, and boron nitride; the other additives include dispersants, antioxidants, and rust inhibitors; preferably, the dispersant is 8 parts, the antioxidant is 2 parts, and the rust inhibitor is 2 parts.
[0029] Preferably, the solid filler is selected from a mixture of molybdenum disulfide, carbon nanotubes and calcium carbonate; the molybdenum disulfide is 0.4-4 parts, the carbon nanotubes are 1.6-16 parts, and the calcium carbonate is 4-40 parts; the calcium carbonate is selected from a mixture of calcium carbonates with particle sizes of 2 to 3 microns and 0.1 microns; the mixture is mixed in a weight ratio of 1:4; the particle size of the solid filler is less than 10μm.
[0030] Preferably, the dispersant is one or more of alcohols, esters, and ketones; further preferably, the dispersant is selected from one or more of triethylhexyl phosphate, methyl amyl alcohol, polyacrylamide, fatty acid polyethylene glycol ester, and stearic acid monoglyceride; more preferably, the dispersant is selected from stearic acid monoglyceride.
[0031] Preferably, the antioxidant is one of a free radical scavenger, a hydroperoxide decomposer, an antioxidant synergist, a metal passivator, and a deposit inhibitor; further preferably, the antioxidant is selected from one of 2,6-tert-butyl-4-methylphenol, β-carotene, N-phenyl a-naphthylamine (PANA), and N,N'-disalicylidene-1,2-propylenediamine; more preferably, the antioxidant is selected from 2,6-tert-butyl-4-methylphenol.
[0032] Preferably, the rust inhibitor is selected from one of sulfonates, esters, carboxylic acids, sulfur, nitrogen heterocyclic compounds, and amines; further preferably, the rust inhibitor is selected from one of stearic acid cyclohexylamine, sorbitan monooleate, stearic acid, and barium petroleum sulfonate; more preferably, the rust inhibitor is selected from stearic acid cyclohexylamine.
[0033] A high temperature resistant bentonite grease composition, characterized in that the grease composition comprises the base oil, the modified polyurea thickener, the modified bentonite thickener, the solid filler, and the other additives; the grease composition is prepared by the preparation method as described above; the working cone penetration of the grease is 245, and the oxygen pressure drop is 0.02KPa; the dropping point of the grease is 260°C, and the high temperature cone penetration is 232; the water residual amount of the grease drum is 28g, and the water contact angle is 96.8°; the grease is placed at 50°C for 48h, and its acid and alkali standard copper sheet corrosion colorimetry is 1a and 1a respectively; the grease sintering load value reaches 6080N, the friction coefficient of the grease reaches 0.052, and the average wear spot diameter is 0.35mm.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The present invention uses 60 parts of castor oil as conventional oil, and performs epoxidation modification by using 48 parts of 30% hydrogen peroxide aqueous solution. The epoxidation degree of the prepared modified base oil reaches 2.2 mol / kg. The prepared grease has significantly improved viscosity, and shows significantly improved oxidation stability compared with grease made of synthetic base oil and silicone oil. At the same time, the working cone penetration is 220-250, and it can be used for lubrication of mechanical parts. The oxygen pressure is reduced to 0.02 KPa, which significantly improves the stability of the grease and prolongs its service life.
[0036] 2. The present invention uses diphenylmethane diisocyanate as a reaction raw material, controls the isocyanate to be 20 parts, and synergizes with bentonite to improve the high temperature resistance of the grease. Since the ring structure has a more stable bond energy and a stronger conjugated system, the high temperature resistance of the molecule is enhanced. The obtained grease composition has a dropping point of 260°C and a high temperature cone penetration of 232, has obvious high temperature resistance, and the cone penetration can be maintained under high temperature conditions.
[0037] 3. The present invention uses a silane coupling agent as a modifier of the polyurea molecule, and the silane is loaded into the polyurea molecule through cross-linking of the -NCO group with the amine structure in the coupling agent. Since the long-chain alkyl group and the silane are arranged at both ends of the polyurea, the obtained grease has obvious hydrophobicity. The grease prepared by adding 20 parts of octadecylamine, 20 parts of KH-550, and 30 parts of polyurea thickener to the grease has a drum water residue of 28g and a water contact angle of 96.8°, showing obvious water resistance.
[0038] 4. The present invention acidifies bentonite to increase the voids in bentonite crystal cells and enhance surface activity. At the same time, the epoxy resin is filled between the organic bentonites to form a cross-linked network structure, and the remaining epoxy resin is cured outside the sheet to form a cross-linked structure. 20 parts of acidic bentonite and 2 parts of epoxy resin E42 are used to prepare a modified bentonite thickener. The grease prepared by using 20 parts of the modified bentonite thickener is placed at 50°C for 48 hours, and its acid and alkali standard copper sheet corrosion colorimetry is 1a and 1a, respectively, showing obvious corrosion resistance.
[0039] 5. The present invention uses MoS2 / CNTs in a mass ratio of 1:4, and adds 10 parts of calcium carbonate of two different particle sizes for synergistic effect. When added to the grease, the sintering load value reaches 6080N, the friction coefficient of the grease reaches 0.052, and the average wear spot diameter is 0.35mm, which significantly improves the wear resistance and friction reduction performance of the grease and improves the lubricating effect of the grease. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The SEM images of untreated bentonite and modified bentonite;
[0041] Figure 2 A graph showing the sintering load values of the lubricating greases prepared in various embodiments of the present invention; DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0044] See also Figure 1 to Figure 2The present invention provides a high temperature resistant bentonite grease composition and a preparation method, and the technical scheme is as follows:
[0045] Example 1
[0046] Preparation of epoxy modified base oil:
[0047] 60 parts of castor oil, 9 parts of glacial acetic acid and 0.6 parts of phosphoric acid are added into a three-necked flask equipped with a thermometer, a reflux condenser and a dropping funnel to obtain a mixture, the mixture is stirred until the oil bath temperature reaches 70°C, 48 parts of 30% H2O2 solution are slowly added dropwise to the mixture, and the mixture is kept warm for reaction for 4 hours to obtain a reaction solution, the reaction solution is extracted with petroleum ether, rotary evaporated, and vacuum dried to obtain epoxidized castor oil, and the epoxidation degree of the castor oil is quantified according to ISO 3001:1999 standard.
[0048] Preparation of modified polyurea thickener:
[0049] 20 parts of toluene diisocyanate were added to 50 ml of anhydrous tetrahydrofuran solvent, the temperature was raised to 60° C., and the mixture was uniformly stirred and dissolved to obtain an ester solution; 20 parts of octadecylamine were added to the ester solution, the temperature was raised to 90° C., and the mixture was reacted for 1 hour to obtain a reaction solution; 20 parts of KH-550 were slowly added to the reaction solution under heat preservation conditions, and the mixture was reacted for 1 hour to obtain a modified polyurea solution; the modified polyurea solution was cooled to room temperature, washed with methanol 3 times, washed with water 2 times, centrifuged, and vacuum dried to obtain a modified polyurea thickener.
[0050] Preparation of modified bentonite thickener:
[0051] 10 parts of sodium bentonite were calcined at 350°C for 1 hour to prepare dry bentonite; 5 parts of 15% sulfuric acid solution were added to the dry bentonite at a solid-liquid ratio of 2:1, and stirred at 90°C for 30 minutes for acidification treatment, and acidified bentonite was obtained by flocculation, slag removal and filtration; 20 parts of the acidified bentonite were added to 50 parts of distilled water to prepare a bentonite suspension; then hexadecyltrimethylammonium bromide was weighed and added to the bentonite suspension, A suspension is prepared, and 2 parts of epoxy resin E42, 1.8 parts of curing agent diethylenetriamine, 2 parts of accelerator tetramethyl diamine disulfide, and 2 parts of diluent isoamyl acetate are added to the suspension and stirred at high speed to obtain a uniformly dispersed mixed system, which is stirred in a constant temperature oil bath at 80°C for 6 hours and vacuum degassed to obtain a reaction system; the reaction system is dried in a vacuum drying oven at 90°C for 2 hours until it is dry and agglomerated, and then crushed, ground, and sieved to obtain a modified bentonite thickener.
[0052] Preparation of grease composition:
[0053] 200 parts of epoxidized castor oil and 30 parts of modified polyurea thickener were added to a high-temperature micro-pressure reactor, the temperature of the high-temperature micro-pressure reactor was raised to 100°C, and the reaction was carried out for 2 hours to obtain reaction system 1, then the temperature of reaction system 1 was raised to 180°C, 60 parts of epoxidized castor oil were slowly added again, and the mixture was kept warm for 30 minutes to obtain system 2, 60 parts of epoxidized castor oil were added to reaction system 2 as quenching oil, the mixture was quenched to 120°C, and the mixture was kept warm for 1 hour, 20 parts of organic bentonite were added, and the mixture was expanded at a low speed for 3 hours to obtain system 3, the temperature of system 3 was lowered to 90°C, 20 parts of solid filler, 8 parts of dispersant, 2 parts of antioxidant, and 2 parts of rust inhibitor were added, and the stirring was continued for 30 minutes to fully dissolve and stir to obtain a mixture, and the mixture was transferred to a degassing kettle for degassing, filtered, and packaged to obtain a grease composition.
[0054] Example 2 The preparation method and parameter conditions are the same as those of Example 1, except that the base oil used is selected from an equal amount of PAO10.
[0055] Example 3 The preparation method and parameter conditions are the same as those of Example 1, except that the base oil used is selected from an equal amount of PAO40.
[0056] Example 4 The preparation method and parameter conditions are the same as those of Example 1, except that the base oil used is selected from an equal amount of methylphenyl silicone oil.
[0057] Example 5-11 Refer to the preparation method and parameter conditions of Example 1, the specific differences are listed in Table 1
[0058] Table 1 The difference in dosage of components in each embodiment
[0059] Example Base oil glacial acetic acid Phosphoric acid <![CDATA[30% H2O2 solution]]> Epoxy Degree Example 5 Oleic acid 9 0.6 6 0.3 Example 6 Oleic acid 9 0.6 12 0.9 Example 7 Oleic acid 9 0.6 24 1.2 Example 8 castor oil 9 0.6 6 0.5 Example 9 castor oil 9 0.6 12 1.2 Example 10 castor oil 9 0.6 24 1.6 Embodiment 11 castor oil 9 0.6 36 1.9
[0060] Examples 12-15 refer to the preparation methods and parameter conditions of Example 1, and the specific differences are listed in Table 2
[0061] Comparative Example 1 The preparation method and parameter conditions are the same as those of Example 1, except that the base oil used is castor oil that has not been epoxy-modified.
[0062] Example 16 Stability Performance Determination
[0063] The greases prepared in Examples 1-15 and Comparative Example 1 were tested for working cone penetration, extended cone penetration, and oxidation stability to evaluate the stability of the prepared greases. The test results are shown in Table 2.
[0064] Working cone penetration: Place the grease sample in a standard working device. At 25°C, after 60 shears, the measured cone penetration is 0.1 mm. This is determined in accordance with ASTM D217-2017.
[0065] Extended working cone penetration: The cone penetration of the grease is measured after 100,000 shear cycles in a standard working machine at 25°C, 0.1 mm; measured in accordance with ASTM D217-2017 standard.
[0066] The cone penetration tester model is SYD-2801C.
[0067] Oxidation stability: A certain amount of grease is placed in an oxygen bomb filled with oxygen pressure and subjected to oxidation at 99°C. The oxidation stability of the grease is determined by the corresponding oxygen pressure drop after 30 hours; this is determined in accordance with SH / T 0193-2008 standard.
[0068] Table 2 Stability results of Examples 1-15 and Comparative Example 1
[0069] Example Epoxy degree (mol / kg) Viscosity (Pa s) Epoxy modified base oil dosage Working cone penetration Extended cone penetration Oxidation stability (KPa) Example 1 2.2 548 320 245 278 0.02 Example 2 / 488 320 268 295 0.15 Example 3 / 512 320 288 312 0.13 Example 4 / 553 320 256 284 0.12 Example 5 0.3 262 320 356 384 0.09 Example 6 0.9 394 320 325 348 0.08 Example 7 1.2 415 320 316 338 0.06 Example 8 0.5 212 320 188 212 0.18 Example 9 1.2 325 320 220 246 0.12 Example 10 1.6 432 320 235 265 0.08 Embodiment 11 1.9 496 320 238 266 0.04 Example 12 2.2 356 220 182 215 0.08 Embodiment 13 2.2 428 270 212 228 0.10 Embodiment 14 2.2 532 370 325 354 0.12 Embodiment 15 2.2 612 420 358 398 0.15 Comparative Example 1 / 166 320 152 174 0.24
[0070] Conclusion: From the results in Table 2, it can be seen that castor oil without epoxy modification shows significantly reduced viscosity, the prepared grease has low working cone penetration and high hardness, and cannot be used for lubrication of daily mechanical bearings. At the same time, the oxidation stability is low, which greatly reduces the stability of the grease; from the results of Comparative Examples 1-7, it can be seen that the use of different base oils as the base oil of the grease has obvious differences in the stability of the grease due to the difference in viscosity of the prepared lubricating oil. The working cone penetration and extended cone penetration of the grease prepared using synthetic base oils PAO10, PAO40 or methyl silicone oil are not much different from those of epoxy castor oil, but the oxidation stability is significantly reduced and the stability is poor; the use of synthetic base oil modified with oleic acid epoxy improves the oxidation stability of the grease, but the lower viscosity further affects the cone penetration of the grease; from Comparative Examples 8-11, by using modified castor oils with different epoxy values as base oils, the greases prepared have a lower viscosity as the epoxy value increases, as shown in Table 1. The cone penetration is significantly improved, and the application of the grease in mechanical lubrication is improved. At the same time, due to the increase in different oxidation values, the cross-linking of castor oil in the thickener and the modified bentonite is increased. Due to the presence of epoxy bonds, the hydrogen bonding effect in the grease is enhanced, the cohesive force of the grease molecules is increased, and the base oil is fully wrapped in the polyurea group and the bentonite-epoxy resin to form a three-dimensional skeleton structure, which further improves the oxidation stability of the grease and enhances the stability of the grease. It can be seen from the results of Examples 12-15 that the addition of different amounts of base oil affects the viscosity of the grease. When the base oil content is low, the rigid network structure reduces the viscosity of the grease, the grease is hard, the lubrication effect is poor, and the stability is low. Excessive base oil can increase the viscosity of the grease, but too high a viscosity leads to high fluidity of the grease, poor lubrication, and inability to be fully adsorbed by the skeleton structure. The exposed epoxy groups are easily affected by the environment, which reduces the oxidation stability of the grease and deteriorates the stability. From the results in Table 2, it can be seen that when 320 parts of base oil is used and the epoxy value of the modified castor oil is guaranteed to be 2.2 mol / kg, the viscosity of the prepared grease is optimal, the working cone penetration is 245, the oxygen pressure drop is 0.02 KPa, and the stability is optimal.
[0071] Embodiment 17
[0072] Preparation of epoxy modified base oil:
[0073] 60 parts of castor oil, 9 parts of glacial acetic acid and 0.6 parts of phosphoric acid are added into a three-necked flask, and equipped with a thermometer, a reflux condenser and a dropping funnel to obtain a mixture, and the mixture is stirred until the oil bath temperature reaches 70°C; 48 parts of 30% H2O2 solution are slowly added dropwise to the mixture, and the mixture is kept warm for 4 hours to obtain a reaction solution, and the reaction solution is extracted with petroleum ether, rotary evaporated, and vacuum dried to obtain epoxidized castor oil. The epoxidation degree of the castor oil is quantified according to ISO 3001:1999 standard.
[0074] Preparation of modified polyurea thickener:
[0075] 20 parts of diphenylmethane diisocyanate were added to 50 ml of anhydrous tetrahydrofuran solvent, the temperature was raised to 60° C., and the mixture was uniformly stirred and dissolved to obtain an ester solution; 20 parts of octadecylamine were added to the ester solution, the temperature was raised to 90° C., and the mixture was reacted for 1 hour to obtain a reaction solution; 20 parts of KH-550 were slowly added to the reaction solution under heat preservation conditions, and the reaction was carried out under heat preservation conditions for 1 hour to obtain a modified polyurea solution; the modified polyurea solution was cooled to room temperature, washed with methanol 3 times, washed with water 2 times, centrifuged, and vacuum dried to obtain a modified polyurea thickener.
[0076] Preparation of modified bentonite thickener:
[0077] 10 parts of sodium bentonite were calcined at 350°C for 1 hour to prepare dry bentonite; 5 parts of 15% sulfuric acid solution were added to the dry bentonite at a solid-liquid ratio of 2:1, and stirred at 90°C for 30 minutes for acidification treatment, and acidified bentonite was obtained by flocculation, slag removal and filtration; 20 parts of the acidified bentonite were added to 50 parts of distilled water to prepare a bentonite suspension; then 1 part of hexadecyltrimethylammonium bromide was weighed and added to the bentonite suspension. , prepare a suspension, add 2 parts of epoxy resin E42, 1.8 parts of curing agent diethylenetriamine, 2 parts of accelerator tetramethyl diamine disulfide, and 2 parts of diluent isoamyl acetate into the suspension and stir at high speed to obtain a uniformly dispersed mixed system, stir in a constant temperature oil bath at 80°C for 6 hours, and vacuum degassing to obtain a reaction system; dry the reaction system in a vacuum drying oven at 90°C for 2 hours until dry and agglomerated, and crush, grind, and sieve to obtain a modified bentonite thickener.
[0078] Preparation of grease composition:
[0079] 200 parts of epoxidized castor oil and 30 parts of modified polyurea thickener were added to a high-temperature micro-pressure reactor. The temperature of the high-temperature micro-pressure reactor was raised to 100° C. and the reaction was carried out for 2 hours to obtain a reaction system 1. Then the temperature of the reaction system 1 was raised to 180° C. and 60 parts of epoxidized castor oil were slowly added again. The reaction system 2 was kept warm for 30 minutes to obtain a system 2. 60 parts of epoxidized castor oil were added to the reaction system 2 as quenching oil, and the reaction system 2 was quenched to 120° C. and kept warm for 1 hour. 20 parts of solid filler, 8 parts of dispersant, 2 parts of antioxidant and 2 parts of rust inhibitor were added. The mixture was stirred for 30 minutes to fully dissolve and stirred to obtain a mixture. The mixture was transferred to a degassing kettle for degassing, filtered and packaged to obtain a grease composition.
[0080] Examples 18-26 Refer to the preparation method and parameter conditions of Example 17, the specific differences are listed in Table 3
[0081] Comparative Example 2 The preparation method and parameter conditions are the same as those of Example 17, except that no modified polyurea thickener is added.
[0082] Comparative Example 3 The preparation method and parameter conditions are the same as those of Example 17, except that a modified bentonite thickener is added. The operation steps and parameter conditions are the same as those of Example 1.
[0083] Example 27 High temperature resistance test of lubricating grease
[0084] The dropping points of the greases prepared in Example 1, Examples 17-26, and Comparative Examples 2-3 were measured using a grease wide temperature range dropping point tester (SYD-3498-I), and the test standard was ASTM D2265-2022.
[0085] High temperature cone penetration: The grease sample was placed in a standard working chamber and subjected to 250°C for 4 hours to measure the high temperature cone penetration; the test was carried out in accordance with ASTM D217-2017. The experimental results are shown in Table 3.
[0086] Table 3 High temperature resistance test results of Example 1, Examples 17-26, and Comparative Examples 2-3
[0087] Example Isocyanate Isocyanate dosage Dropping point(℃) High temperature cone penetration Example 1 Toluene diisocyanate 20 More than 300 244 Embodiment 17 Methylene diphenyl diisocyanate 20 260 282 Embodiment 18 Toluene diisocyanate 20 246 310 Embodiment 19 Hexamethylene diisocyanate 20 220 325 Embodiment 20 Isophorone diisocyanate 20 232 316 Embodiment 21 p-Terephthalylene diisocyanate 20 245 312 Embodiment 22 4,4-Dicyclohexylmethane diisocyanate 20 240 305 Embodiment 23 Methylene diphenyl diisocyanate 10 198 348 Embodiment 24 Methylene diphenyl diisocyanate 15 210 336 Embodiment 25 Methylene diphenyl diisocyanate 25 258 298 Embodiment 25 Methylene diphenyl diisocyanate 30 255 302 Embodiment 26 Methylene diphenyl diisocyanate 40 216 328 Comparative Example 2 / / 126 412 Comparative Example 3 Methylene diphenyl diisocyanate 20 More than 300 232
[0088] Conclusion: It can be seen from the results in Table 1 that when a polyurea-based thickener is used, the grease in Comparative Example 1 that does not use a polyurea-based thickener has a significantly improved dropping point temperature, and the maximum dropping point temperature can reach 260°C; from the results of Comparative Examples 17-22, it can be seen that the dropping point temperatures of polyurea thickeners synthesized using different diisocyanates are quite different. When aliphatic isocyanates are used, the dropping point decreases significantly compared to aromatic isocyanates. At the same time, the dropping point temperature of fatty alkyl isocyanates is lower than that of fatty cycloalkyl isocyanates. Since the cyclic structure has a more stable bond energy and a stronger conjugated system, the thermal stability of aromatic isocyanates is stronger than that of aliphatic isocyanates. At the same time, the cyclic rigid structure in the aliphatic cycloalkyl structure increases the stress of the molecule and enhances the high temperature resistance of the molecule; Comparative Examples 23-25 The results show that the amount of isocyanate used determines the stability of the urea structure in the grease. When the isocyanate content in the system is low, a large amount of amines remain, which reduces the temperature resistance of the system. However, if the isocyanate content is too high, the unreacted isocyanate is exposed on the surface of the grease, which is easily destroyed under high temperature conditions, thereby affecting the high temperature resistance of the grease. Since the urea molecules in polyurea grease are connected by hydrogen bonds, these molecules, which are initially arranged in a disorderly manner, are slowly connected by hydrogen bonds to form long chains under high temperature conditions. As the temperature rises, the chains become longer and longer, and the molecules will also produce bond flipping in the process of being connected by hydrogen bonds, causing distortion and forming a spatial spiral tubular structure. At the same time, the long chains are also cross-linked by hydrogen bonds to form an interwoven network structure. Finally, when a certain temperature is reached and the spatial network structure is basically formed, the base oil will slowly be absorbed into the hollow tube surrounded by urea molecules. After a certain period of expansion, the hollow tube becomes a solid tube. At this time, the colloidal structure of the polyurea grease reaches a stable state, which significantly improves the high temperature resistance of the grease. At the same time, by comparing the structures of Example 1, Examples 17-18 and Comparative Example 3, it can be seen that since the bentonite grease has the characteristic of no dropping point, the lubrication dropping point of the modified bentonite is not reflected, but the high temperature cone penetration test results show that the addition of the modified bentonite thickener can stabilize the high temperature cone penetration of the grease, ensure that the lubrication state of the grease remains unchanged, and increase the service life of the grease. Comprehensive Table 1 results show that the use of 20 parts of diphenylmethane diisocyanate and the use of epoxy resin grafted organic bentonite can effectively improve the dropping point of the grease, and the state of the grease does not change under high temperature conditions, and it has obvious high temperature resistance.
[0089] Embodiment 28
[0090] Preparation of epoxy modified base oil:
[0091] 60 parts of castor oil, 9 parts of glacial acetic acid and 0.6 parts of phosphoric acid are added into a three-necked flask equipped with a thermometer, a reflux condenser and a dropping funnel to obtain a mixture, the mixture is stirred until the oil bath temperature reaches 70°C, 48 parts of 30% H2O2 solution are slowly added dropwise to the mixture, and the mixture is kept warm for reaction for 4 hours to obtain a reaction solution, the reaction solution is extracted with petroleum ether, rotary evaporated, and vacuum dried to obtain epoxidized castor oil, and the epoxidation degree of the castor oil is quantified according to ISO 3001:1999 standard.
[0092] Preparation of modified polyurea thickener:
[0093] 20 parts of diphenylmethane diisocyanate were added to 50 ml of anhydrous tetrahydrofuran solvent, the temperature was raised to 60° C., and the mixture was uniformly stirred and dissolved to obtain an ester solution; 20 parts of octadecylamine were added to the ester solution, the temperature was raised to 90° C., and the mixture was reacted for 1 hour to obtain a reaction solution; 20 parts of KH-550 were slowly added to the reaction solution under heat preservation conditions, and the reaction was carried out under heat preservation conditions for 1 hour to obtain a modified polyurea solution; the modified polyurea solution was cooled to room temperature, washed with methanol 3 times, washed with water 2 times, centrifuged, and vacuum dried to obtain a modified polyurea thickener.
[0094] Preparation of modified bentonite thickener:
[0095] 10 parts of sodium bentonite were calcined at 350°C for 1 hour to prepare dry bentonite; 5 parts of 15% sulfuric acid solution were added to the dry bentonite at a solid-liquid ratio of 2:1, and stirred at 90°C for 30 minutes for acidification treatment, and acidified bentonite was obtained by flocculation, slag removal and filtration; 20 parts of the acidified bentonite were added to 50 parts of distilled water to prepare a bentonite suspension; then 1 part of hexadecyltrimethylammonium bromide was weighed and added to the bentonite suspension. , prepare a suspension, add 2 parts of epoxy resin E42, 1.8 parts of curing agent diethylenetriamine, 2 parts of accelerator tetramethyl diamine disulfide, and 2 parts of diluent isoamyl acetate into the suspension and stir at high speed to obtain a uniformly dispersed mixed system, stir in a constant temperature oil bath at 80°C for 6 hours, and vacuum degassing to obtain a reaction system; dry the reaction system in a vacuum drying oven at 90°C for 2 hours until dry and agglomerated, and crush, grind, and sieve to obtain a modified bentonite thickener.
[0096] Preparation of grease composition:
[0097] 200 parts of epoxidized castor oil and 30 parts of modified polyurea thickener were added to a high-temperature micro-pressure reactor, the temperature of the high-temperature micro-pressure reactor was raised to 100° C., and the reaction was carried out for 2 hours to obtain a reaction system 1, then the temperature of the reaction system 1 was raised to 180° C., 60 parts of epoxidized castor oil were slowly added again, and the mixture was kept warm for 30 minutes to obtain a system 2, 60 parts of epoxidized castor oil were added to the reaction system 2 as quenching oil, the mixture was quenched to 120° C., and the mixture was kept warm for 1 hour, 20 parts of modified bentonite thickener were added, and the mixture was expanded at a low speed for 3 hours to obtain a system 3, the system 3 was cooled to 90° C., 20 parts of solid filler, 8 parts of dispersant, 2 parts of antioxidant, and 2 parts of rust inhibitor were added, and the stirring was continued for 30 minutes to fully dissolve and uniformly obtain a mixture, and the mixture was transferred to a degassing kettle for degassing, filtered, and packaged to obtain a grease composition.
[0098] Examples 29-40 refer to the preparation method and parameter conditions of Example 28, and the specific differences are listed in Table 4
[0099] Comparative Example 4 The preparation method and parameter conditions are the same as those of Example 28, except that KH-550 is not added.
[0100] Comparative Example 5 The preparation method and parameter conditions are the same as those of Example 28, except that KH-550 and octadecylamine are not added, and an equal amount of ethylenediamine is added.
[0101] Example 41 Determination of water resistance of grease
[0102] The water resistance of the grease prepared in Examples 28-40 and Comparative Examples 4-5 was determined using a grease roller test. The test conditions were as follows: 20 parts of grease; 30 parts of water; temperature 50°C; time 30 hours. After the test, the remaining water in the roller was poured out and weighed to determine the water resistance of the grease. An appropriate amount of the grease after the test was taken and vacuum dried at 50°C for 1 hour. The water contact angle was measured to evaluate its hydrophobicity. The contact angle was measured using a contact angle tester (OC A50). The experimental results are shown in Table 4.
[0103] Table 4 Waterproof performance test of Examples 28-40 and Comparative Examples 4-5
[0104] Example Dosage of Octadecylamine KH-550 dosage Modified thickener addition amount Remaining water (g) Water contact angle (°) Embodiment 28 20 20 30 28 96.8° Embodiment 29 10 30 30 22 97.5° Embodiment 30 15 25 30 21 97.2° Embodiment 31 25 15 30 25 95.4° Embodiment 32 30 10 30 24 94.6° Embodiment 33 10 10 30 18 88.4° Embodiment 34 15 15 30 21 93.2° Embodiment 35 25 25 30 24 95.6° Embodiment 36 30 30 30 23 94.4° Embodiment 37 20 20 20 18 89.8° Embodiment 38 20 20 25 21 92.4° Embodiment 39 20 20 40 21 95.8° Embodiment 40 20 20 50 20 96.2° Comparative Example 4 40 / 30 15 80.6° Comparative Example 5 / / 30 10 60.4°
[0105] Conclusion: From the results in Table 4, it can be seen that compared with Example 20, the water resistance of the grease prepared in Comparative Examples 4-5 without adding silane coupling agent or replacing it with ethylenediamine in equal amount is significantly improved, the residual water in the drum is significantly increased, and the water contact angle is also significantly increased, showing excellent hydrophobicity; From the results of Examples 28-32, it can be seen that changing the proportion of octadecylamine and KH-550 will affect the long-term water resistance of the grease. Due to the excessive presence of Si-O bonds, water molecules form weak hydrogen bonds with Si-O bonds. Under long-term use conditions, water molecules will be adsorbed on the surface of the grease, affecting further waterproof effect. Increasing the amount of octadecylamine can improve the above situation, but excessive long-chain alkylamine molecules will reduce the high temperature resistance of the grease. The addition of Si-OC bonds will further increase the thermal stability of the grease; From the results of Examples 33-36, it can be seen that reducing the proportion of octadecylamine and KH-550 , which will lead to less urea formation in the grease, and a large number of unstable -NCO groups are exposed on the surface of the grease, which increases the hydrophilicity of the grease. Excessive amines will reduce the stability of the polyurea thickener, and unstable amine substances will affect the overall performance of the grease. Comparative Examples 37-40, different added amounts of polyurea thickeners will also affect the hydrophobicity of the grease. Less thickener makes it impossible for the modified oil to be evenly dispersed in the polyurea structural material, which causes the hardness of the grease to increase under long-term conditions and reduce the use effect. Excessive thickener increases the urea groups in the skeleton structure, increasing the chance of contact with water, and the hydrophilic urea groups reduce the hydrophobicity of the grease. From the results of Table 4, it can be seen that the grease prepared by using 20 parts of octadecylamine, 20 parts of KH-550, and adding 30 parts of polyurea thickener to the grease has a drum water residue of 28 parts and a water contact angle of 96.8°, showing a high hydrophobicity.
[0106] Examples 42-57 Refer to the preparation method and parameter conditions of Example 28, with specific differences as shown in Table 5.
[0107] Comparative Example 6 The preparation method and parameter conditions are the same as those of Example 28, except that the modified bentonite thickener is not subjected to acidification treatment before preparation.
[0108] Comparative Example 7 The preparation method and parameter conditions are the same as those of Example 28, except that no epoxy resin is added for curing modification during the preparation of the modified bentonite thickener.
[0109] Experimental Example 58 Corrosion Resistance Test
[0110] A copper sheet with a size of 20×50×3mm was used to test the corrosion resistance of the grease. Before the experiment, the copper sheet was polished, ultrasonically cleaned several times and dried. The grease prepared in Examples 42-57 was evenly applied to the dry copper sheet with a spoon to a thickness of 2mm. The copper sheet was placed obliquely in a beaker, and a 10% by mass NaOH solution and a 3% by mass HCl solution were added to the beaker respectively, and the mixture was placed at 50°C for 48h. After the experiment, the grease on the metal surface was thoroughly cleaned and dried, and compared with the standard copper sheet corrosion colorimetric card according to GB / T7326-1987. The experimental results are shown in Table 5. The SEM images of the untreated bentonite and the modified bentonite are shown in Table 5. Figure 1 shown.
[0111] Among them, 1a is a copper sheet with a light yellow color, 1b is a light orange color, 2a is an orange-red color, and 2b is a purple-red color.
[0112] Table 5 Corrosion resistance test of Example 28, Examples 42-57, Comparative Examples 6-7
[0113] Example Epoxy resin Epoxy resin dosage Acidified bentonite dosage Modified bentonite addition amount 10% NaOH solution 3% HCl solution Embodiment 28 E42 2 20 20 1a 1a Embodiment 42 E44 2 20 20 1a 1b Embodiment 43 E51 2 20 20 1a 1b Embodiment 44 E52 2 20 20 1b 1b Embodiment 45 Bisphenol F 2 20 20 1b 2a Embodiment 46 E42 0.5 20 20 2a 2a Embodiment 47 E42 1 20 20 1b 2a Embodiment 48 E42 1.5 20 20 1b 1b Embodiment 49 E42 2.5 20 20 1a 1a Embodiment 50 E42 3 20 20 1a 1b Embodiment 51 E42 2 20 10 1b 2a Embodiment 52 E42 2 20 15 1b 1b Embodiment 53 E42 2 20 30 1b 1b Embodiment 54 E42 2 20 40 1b 2a Embodiment 55 E42 2 10 20 1a 1b Embodiment 56 E42 2 30 20 1b 2a Embodiment 57 E42 2 40 20 2a 2b Comparative Example 6 E42 2 20 1b 1b Comparative Example 7 / / 20 2b 2b
[0114] Conclusion: Pass Figure 1 The results of Table 5 show that the untreated bentonite particles are irregular particles of different sizes, and some bentonite particles are agglomerated. The modified bentonite is clearly a lamellar structure, which indicates that the intercalation agent has successfully entered the bentonite interlayer to form a cross-linked network structure. The results of Comparative Example 7 show that the grease prepared without epoxy resin modification has poor corrosion resistance, while the grease prepared by the bentonite without acid treatment in Comparative Example 6 has poor corrosion resistance relative to Example 28. The grease is activated by sulfuric acid and H2O2 with an inorganic acid. + Replacement of Na between bentonite layers +, increasing the gaps in the unit cells, expanding the cavities, clearing the voids, increasing the specific surface area, enhancing the surface activity, and increasing the ion exchange properties, so that the acidified bentonite has interlayer adsorption, bonding and adsorption of electrons, better epoxy resin bonding, and increased corrosion resistance; the results of Examples 42-45 and Example 28 show that the use of epoxy resin E42 has better corrosion resistance than other epoxy resin types, and there is almost no change in acid and alkali for 48 hours. Compared with the standard copper sheet corrosion colorimetric card, the color is almost unchanged. Bentonite and hydroxy-substituted quaternary ammonium salt are combined with hydrogen bonds. Epoxy molecules have good compatibility with them and can catalyze the curing reaction and increase the interlayer polymerization rate. In addition, epoxy resin and organic soil have good affinity, and epoxy resin is easy to enter the interlayer. The amount of epoxy that can be accommodated in the interlayer has a saturation value. After reaching this value, the system reaches a thermodynamic equilibrium state. Therefore, E42 with a lower epoxy value can be better adsorbed in the cavity structure of bentonite. A part of E42 fills between organic bentonites to form a cross-linked network structure, forming swelling and intercalation of organic bentonite. At the same time, another part of E42 solidifies outside the sheet and also forms a cross-linked network structure, which increases the stability of the grease while reducing the intrusion of environmental ions into the material structure, thereby improving the corrosion resistance of the grease. Comparing Examples 46-50 and Example 28, less epoxy resin cannot be solidified on the surface of bentonite, and the formation of a cross-linked structure not only reduces the corrosion resistance of the grease, but also reduces the solubility of the modified bentonite in epoxy castor oil, affecting the overall properties of the grease. The results of Examples 51-54 and Example 28 show that the modified If the amount of bentonite is too small, the base oil cannot be fully wrapped, thereby reducing the corrosion resistance of the grease, and the excessive amount of modified bentonite will react with the polyurea molecules in the grease to form a cohesive reaction, affecting the overall performance of the grease; in contrast to Examples 55-57 and Example 28, when excessive acidified bentonite is added, the epoxy resin cannot ensure that all organic bentonites are fully infiltrated. At this time, there will be more organic bentonites and dissociated monolayers that have a larger surface energy and regroup to form larger aggregates, affecting the corrosion resistance of the epoxy resin. From the results of Table 5, it can be seen that 20 parts of acidic bentonite, 2 parts of epoxy resin E42, and 20 parts of modified bentonite thickener are added to the grease composition. The grease prepared is placed at 50°C for 48 hours, and its acid and alkali standard copper sheet corrosion colorimetric is 1a and 1a respectively.
[0115] Examples 59-71 Refer to the preparation method and parameter conditions of Example 28, with specific differences as shown in Table 6.
[0116] Comparative Example 8 The preparation method and parameter conditions are the same as those of Example 28, except that MoS2 / CNTs are not added to the grease composition.
[0117] Comparative Example 9 The preparation method and parameter conditions are the same as those of Example 28, except that no calcium carbonate is added to the grease composition.
[0118] Example 72 Friction and Wear Performance Test
[0119] A four-ball friction and wear tester was used to examine the friction and wear properties of the greases prepared in Example 28 and Examples 59-71. The test temperature was 75°C, the test time was 60 min, the rotation speed was 1200 r / min, and the load was not less than 40 kgf; the steel ball was a GGr15 standard steel ball provided by Xiamen Tianji Automation Co., Ltd., with a hardness of 6.37-6.86 GPa and a diameter of 12.7 mm. It was cleaned with petroleum ether and dried with hot air before the test. The average friction coefficient was recorded by a computer, and the average wear spot diameter of the three steel balls was read by an optical microscope. The sintering load value was also recorded. The sintering load value was measured with reference to SH / T 0204 and SH / T 0202 standards. Figure 2 The average friction coefficient and average wear spot diameter results are shown in Table 6.
[0120] Table 6 Friction and wear properties of Example 28, Examples 59-71, and Comparative Example 8
[0121] Example <![CDATA[MoS2]]> CNTs Calcium carbonate Average friction coefficient Average wear spot diameter Embodiment 28 2 8 10 0.052 0.35 Embodiment 59 2 2 10 0.078 0.45 Embodiment 60 2 4 10 0.068 0.42 Embodiment 61 2 6 10 0.055 0.38 Embodiment 62 2 10 10 0.051 0.38 Embodiment 63 2 12 10 0.049 0.44 Embodiment 64 2 8 4 0.056 0.42 Embodiment 65 2 8 8 0.054 0.40 Embodiment 66 2 8 12 0.050 0.36 Embodiment 67 2 8 16 0.051 0.38 Embodiment 68 0.4 1.6 2 0.062 0.46 Embodiment 69 1.2 4.8 6 0.055 0.38 Embodiment 70 3.2 12.8 16 0.061 0.44 Embodiment 71 4 16 20 0.065 0.42 Comparative Example 8 / / 20 0.085 0.62 Comparative Example 9 2 8 / 0.078 0.54
[0122] Conclusion: Pass Figure 1The results show that adding MoS2 / CNTs or calcium carbonate as solid fillers to the grease can effectively improve the sintering load value of the polyurea grease. When the MoS2 / CNTs content is 1:4 and the total solid filler addition amount is 20 parts, the sintering load value reaches 6080N. The results in Table 6 show that compared with comparative examples 7-8 without adding MoS2 / CNTs or calcium carbonate as solid fillers, Example 28 shows significantly reduced friction coefficient and wear spot diameter after adding solid fillers. By comparing the results of Examples 59-63 and Example 28, it can be seen that when using different proportions of MoS2 / CNTs to friction The performance is significantly affected. When the CNTs content is low, the friction coefficient is high. As the CNTs content increases, the friction coefficient tends to be stable, but the wear spot diameter of the grease increases significantly. By comparing the results of Examples 64-67 and Example 28, it can be seen that changing the amount of calcium carbonate has a certain effect on the friction coefficient and the average wear spot diameter of the grease. By compounding two calcium carbonates with different particle sizes, the lubrication performance of the grease can be improved according to the needs under different working conditions. Once pitting occurs on the tooth surface, the two calcium carbonates can fill and remedy the pitting area in time to avoid expansion, thereby extending the service life of the gear. The test results of Examples 68-71 show that the performance of the grease is significantly reduced compared to that of Example 28. Since MoS2 is a close-packed hexagonal layered compound with a typical "sandwich" structure, with two layers of sulfur atoms sandwiching a layer of metal molybdenum atoms, in the early stage of the friction process, the MoS2 / CNTs composite additive enters between the friction layers through deposition and adsorption, filling and repairing the microcracks or defective areas on the surface of the substrate; then, under the action of the mutual movement of the upper and lower friction pairs, the composite additive and the substrate undergo a tribochemical reaction, and then a lubricating film containing inorganic oxides and carbon-containing materials is formed on the surface of the substrate to prevent direct contact of friction, thereby playing a role in reducing friction and resisting wear. At the same time, there is a carbon nanotube deposition film layer inside the inner chemical reaction film, which cooperates with molybdenum disulfide to play the role of a "micro bearing", and the synergistic effect of two calcium carbonates of different particle sizes further reduces friction and resists wear. Comprehensive Table 6 and Figure 2 The results show that when MoS2 / CNTs is used in a mass ratio of 1:4 and 10 parts of calcium carbonate of two different particle sizes are added synergistically to the grease, the sintering load value reaches 6080N, the friction coefficient of the grease reaches 0.052, and the average wear spot diameter is 0.35mm, which significantly improves the wear resistance and friction reduction performance of the grease, improves the lubricating effect of the grease, and extends its service life.
[0123] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a high temperature resistant bentonite grease composition, characterized in that: The high temperature resistant bentonite grease composition comprises 220-420 parts of base oil, 20-50 parts of modified polyurea thickener, 10-40 parts of modified bentonite thickener, 4-40 parts of solid filler and 12 parts of other additives; The base oil is a modified base oil; The modified base oil is prepared by epoxidation of castor oil with 6 to 48 parts of 30% H2O2 solution under the action of glacial acetic acid and phosphoric acid; The modified polyurea thickener is prepared by modifying 10 to 40 parts of isocyanate and 10 to 30 parts of octadecylamine through 10 to 30 parts of a silane coupling agent; The modified bentonite thickener is prepared by modifying 10 to 40 parts of acidic bentonite with 0.5 to 3 parts of epoxy resin; The preparation method of the modified bentonite thickener comprises the following steps: The sodium bentonite is calcined at 350°C for 1 hour to obtain dry bentonite; the dry bentonite is added with 5 parts of a 15% sulfuric acid solution at a solid-liquid ratio of 2:1, stirred at 90°C for 30 minutes for acidification, and acidified bentonite is obtained by flocculation, slag removal and filtration; the acidified bentonite is added to 50 parts of distilled water to prepare a bentonite suspension; hexadecyltrimethylammonium bromide is added to the bentonite suspension to obtain a suspension; epoxy resin, curing agent diethylenetriamine, accelerator tetramethyldiamine disulfide, and diluent isoamyl acetate are added to the suspension, stirred at high speed, dispersed evenly, stirred in a constant temperature oil bath at 80°C for 6 hours, and vacuum degassed to obtain a reaction system; the reaction system is dried at 90°C in a vacuum drying oven for 2 hours until it is dry and agglomerated, crushed, ground, and sieved to obtain the modified bentonite thickener; The solid filler is 0.4-4 parts of molybdenum disulfide, 1.6-16 parts of carbon nanotubes, and 4-40 parts of calcium carbonate; wherein the calcium carbonate is selected from a mixture of calcium carbonates with particle sizes of 2-3 microns and 0.1 microns; the calcium carbonate mixture is mixed at a weight ratio of 1:4; The preparation method of the high temperature resistant bentonite grease composition comprises the following steps: The base oil is added into a high-temperature micro-pressure reactor, the temperature of the high-temperature micro-pressure reactor is raised to 100° C., the modified polyurea thickener is added, and the mixture is reacted for 2 hours to obtain a mixed solution; the temperature of the mixed solution is raised to 180° C., the base oil is slowly added again, and the mixture is kept warm for 30 minutes to obtain a reaction solution; the base oil is added into the reaction solution, the mixture is rapidly cooled to 120° C., the mixture is kept warm and stirred for 1 hour, the modified bentonite thickener is added, and the mixture is stirred and expanded at a low speed for 3 hours to obtain a reaction system; the reaction system is cooled to 90° C., the solid filler and the other additives are added, and the mixture is stirred for 30 minutes to be fully mixed and dissolved, and the mixture is stirred evenly to obtain a mixture; the mixture is transferred to a degassing kettle for degassing, filtering, and packaging to obtain the bentonite grease composition.
2. The method for preparing the high temperature resistant bentonite grease composition according to claim 1, characterized in that: The preparation method of the modified base oil comprises the following steps: 60 parts of the castor oil, 9 parts of the glacial acetic acid and 0.6 parts of the phosphoric acid are added into a three-necked flask, and equipped with a thermometer, a reflux condenser and a dropping funnel to obtain a mixture; the mixture is stirred until the oil bath temperature reaches 70°C, 6-48 parts of a 30% H2O2 solution is slowly added dropwise to the mixture, and the mixture is kept warm for reaction for 4 hours to obtain a reaction liquid; the reaction liquid is extracted with petroleum ether, rotary evaporated, and vacuum dried to obtain a modified base oil.
3. The method for preparing the high temperature resistant bentonite grease composition according to claim 1, characterized in that: The isocyanate is selected from toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, p-xylylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate; and the silane coupling agent is selected from KH-550.
4. The method for preparing the high temperature resistant bentonite grease composition according to claim 3, characterized in that: The preparation method of the modified polyurea thickener comprises the following steps: Toluene diisocyanate is added to 50 ml of anhydrous tetrahydrofuran solvent, the temperature is raised to 60° C., and the solution is uniformly stirred to obtain an ester solution; octadecylamine is added to the ester solution, the temperature is raised to 90° C., and the reaction is carried out for 1 hour to obtain a reaction solution; KH-550 is slowly added to the reaction solution under heat preservation conditions, and the reaction is carried out for 1 hour to obtain a modified polyurea solution; the modified polyurea solution is cooled to room temperature, washed with methanol 3 times, washed with water 2 times, centrifuged, and vacuum dried to obtain a modified polyurea thickener.
5. The method for preparing the high temperature resistant bentonite grease composition according to claim 1, characterized in that: The epoxy resin is selected from one of E42, E44, E51, E52 and bisphenol F epoxy resin.
6. The method for preparing the high temperature resistant bentonite grease composition according to claim 1, characterized in that: The other additives include 8 parts of dispersant, 2 parts of antioxidant and 2 parts of rust inhibitor.
7. A high temperature resistant bentonite grease composition, characterized in that: The bentonite grease composition is prepared by the preparation method according to any one of claims 1 to 6; the working cone penetration of the bentonite grease composition is 245, and the oxygen pressure drop is 0.02 KPa; the dropping point of the bentonite grease composition is 260°C, and the high-temperature cone penetration is 232; the drum water residue of the bentonite grease composition is 28g, and the water contact angle is 96.8°; the bentonite grease composition is placed at 50°C for 48h, and its acid and alkali standard copper sheet corrosion colorimetry is 1a and 1a respectively; the sintering load value of the bentonite grease composition reaches 6080N, the friction coefficient of the bentonite grease composition reaches 0.052, and the average wear spot diameter is 0.35mm.
Citation Information
Patent Citations
Excellent carbamido lubricating grease composition with shear stability and preparation method thereof
CN102604716B
High-performance composite calcium sulfonate based lubricating grease and preparation method thereof
CN103146465A
Composition of food-grade lubricating grease and preparation method thereof
CN103789065A
Thickener for thickening high temperature lubricating grease
CN104830403B
High-temperature-resistant lubricating oil base oil and preparation method thereof
CN104962341A