A high-adhesion epoxy mortar steel bridge deck paving material and preparation method thereof

By combining the modified epoxy resin and the modified curing agent, a high adhesion epoxy mortar material is formed, which solves the insufficient impact resistance, hardness, water resistance and metal adhesion of steel bridge deck paving materials in the prior art. The problem has achieved improvement in the performance of the material and simplification of the preparation process.

CN118420267BActive Publication Date: 2024-11-05FUJIAN CORNERSTONE TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410497003.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-11-05
Estimated Expiration
2044-04-24

AI Technical Summary

Technical Problem

The existing steel bridge deck paving materials have shortcomings in impact resistance, hardness, waterproofness and metal adhesion, and the preparation process is complicated and the operation is inconvenient.

Method used

Adhesives composed of modified epoxy resin, epoxy resin, diluent and modified curing agent are mixed with gravel in a specific proportion to form high adhesion epoxy mortar material, and good impact resistance is obtained through a simple preparation process. , steel bridge deck paving materials with hardness and waterproof properties.

Benefits of technology

It has achieved the improvement of the material's high adhesion, impact resistance, waterproof performance and coating hardness, simplified the production process, reduced production time, and met the high-performance needs of steel bridge deck paving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004807467960000031
    Figure BDA0004807467960000031
Patent Text Reader

Abstract

The present invention belongs to the field of engineering materials, and specifically discloses a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof, wherein the high-adhesion epoxy mortar steel bridge deck paving material is mixed with an adhesive and crushed stone in a mass ratio of 1: (6-10); each weight portion of the adhesive is mixed with an A component and a B component in a mass ratio of 1: (1-1.5); the A component includes the following weight portions of raw materials: 40-60 parts of modified epoxy resin, 60-70 parts of epoxy resin, and 10-20 parts of diluent; the B component includes the following weight portions of raw materials: 100-150 parts of modified curing agent, and 100-150 parts of aminoethylpiperazine. The preparation process of the high-adhesion epoxy mortar steel bridge deck paving material of the present invention is simple, and production time can be greatly saved; and the paving material has good comprehensive performance, excellent metal adhesion, and a large coating hardness and strong impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering materials, and in particular to a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. Background Art

[0002] Bridge construction has entered a peak period with the rapid development of road construction. More and more large-span steel structure bridges are being built. The bridge deck pavement has the functions of protecting the steel plate, bearing the load together with the steel bridge deck structure, resisting the corrosion damage of the steel bridge structure, and improving the durability of the steel structure. It is an important part affecting the quality of steel bridge projects and should have good anti-wear performance and anti-shear deformation performance. The pavement surface should be solid and flat to meet the requirements of safe and comfortable driving.

[0003] The paving materials used in my country in the early days were mainly mastic asphalt crushed stone mixtures. This material is prone to paving defects such as cracks, rutting, lumps, potholes and delamination, which seriously affect driving safety. Through the continuous exploration of scientific researchers, four major steel bridge deck paving material systems have been formed, including mastic asphalt crushed stone mixtures, cast asphalt concrete, epoxy asphalt concrete and modified dense graded asphalt concrete. Among the many steel bridge deck paving materials, epoxy asphalt concrete paving is a paving method that has been widely used in steel bridge deck asphalt paving projects in recent years. However, the expensive cost and high parameters of epoxy asphalt materials and the strict process requirements for them in paving construction have strictly limited their application. Therefore, finding alternative steel bridge deck paving materials with excellent performance and low price is a hot topic of research.

[0004] Patent No. CN113526917A discloses a flexible epoxy mortar for steel bridge deck paving and its preparation method. The flexible epoxy mortar provided by the invention has high compressive strength and flexural strength, and has good flexibility. When applied to the steel bridge deck paving structure, it has good steel plate tracking deformation ability, can adapt to the large deflection deformation of the steel bridge deck, ensure the deformation coordination between the paving layer structure and the steel plate, and at the same time increase the adhesion and friction resistance between the paving layer interface, effectively resist interlayer shear deformation, and can significantly reduce the probability of high temperature stability diseases such as displacement, bulging, sliding, and rutting of the traditional SMA paving structure system, and extend the service life of the steel bridge deck paving structure. The steel bridge deck paving material needs to have both flexibility and hardness, but the invention only tests and explains the flexibility and waterproof performance of the material, and does not explore the material hardness and metal adhesion.

[0005] The patent invention with patent number CN115029011A discloses an epoxy asphalt steel bridge deck paving pothole repair material and its application. The raw materials of the epoxy asphalt steel bridge deck paving pothole repair material include: epoxy resin main agent, epoxy resin curing agent, rubber composite modified asphalt and compatibilizer. The tensile strength of the epoxy asphalt material meets the requirements of the specification and also has the advantage of good deformation coordination. However, the preparation of the material is complicated and needs to be heated and stirred multiple times at different temperatures, which is not easy to operate.

[0006] In view of the current technical problems, it is of practical significance to develop an epoxy mortar steel bridge deck paving material with a simple synthesis method, strong adhesion, good impact resistance, high hardness and waterproofness. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The high-adhesion epoxy mortar steel bridge deck paving material of the present invention has a simple preparation process, does not require cumbersome production and processing, can greatly save production time, and has good impact resistance, hardness, waterproof performance and excellent metal adhesion.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] The first aspect of the present invention provides a high-adhesion epoxy mortar steel bridge deck paving material, wherein the high-adhesion epoxy mortar steel bridge deck paving material is formed by mixing an adhesive and crushed stone in a weight ratio of 1: (6-10); the adhesive is formed by mixing component A and component B in a weight ratio of 1: (1-1.5); each part of the component A comprises the following raw materials in parts by weight: 40-60 parts of modified epoxy resin, 60-70 parts of epoxy resin, and 10-20 parts of diluent; each part of the component B comprises the following raw materials in parts by weight: 100-150 parts of modified curing agent and 100-150 parts of aminoethylpiperazine.

[0010] In some embodiments, the crushed stones have a diameter of 5.0 mm to 10.0 mm.

[0011] Crushed stone is the aggregate of mortar and plays a supporting role for the material. Crushed stone with a diameter of 5.0mm-10.0mm is finer and can increase the hardness of the material, reduce the shrinkage of the material and avoid cracking.

[0012] In some embodiments, the epoxy resin is bisphenol A epoxy resin, the epoxy value is 0.38 to 0.56 eq / 100 g, and the viscosity at 40° C. is ≤3000 mPa.S.

[0013] Preferably, the epoxy resin is bisphenol A epoxy resin E-51, with an epoxy value of 0.48 to 0.54 eq / 100 g and a viscosity of ≤2500 mPa.S at 40°C.

[0014] The present invention does not impose any special restrictions on the source of the bisphenol A epoxy resin E-51, which can be purchased from commercial sources, including but not limited to Hubei Tosoh Chemical Technology Co., Ltd.

[0015] The epoxy value and viscosity of bisphenol A epoxy resin are in this range. The epoxy value is high, the fluidity is large, and the cross-linking reaction with the curing agent occurs. The cross-linked network structure is tight, resulting in a large hardness and lack of toughness. After modification, the epoxy value of the modified epoxy resin is reduced, and the fluidity is weakened. When used in combination with bisphenol A epoxy resin, the epoxy value and viscosity reach the optimal use range, and the cross-linking reaction with the curing agent occurs. The cross-linked network structure is moderate, with both hardness and flexibility.

[0016] In some embodiments, the structural formula of the modified epoxy resin is:

[0017]

[0018] In some embodiments, the modified epoxy resin comprises the following preparation steps:

[0019] Weigh bisphenol A epoxy resin and dissolve it in an organic solvent. Under the protection of inert gas, add triethylamine and oxalyl chloride dropwise in sequence, and stir at room temperature for 1-4 hours. After the reaction is completed, adjust the pH to 6-7 with glacial acetic acid at 40-60°C, wash the reaction solution with water, combine the organic layers, vacuum spin dry, and dry to obtain the modified epoxy resin.

[0020] Preferably, the preparation steps of the modified epoxy resin are:

[0021] Weigh bisphenol A epoxy resin and dissolve it in an organic solvent. Under the protection of inert gas, add triethylamine and oxalyl chloride dropwise in sequence, and stir at room temperature for 2 hours. After the reaction is completed, adjust the pH to 7 at 50°C with glacial acetic acid, wash the reaction solution with water, combine the organic layers, spin dry in vacuum, and dry to obtain the modified epoxy resin.

[0022] Since bisphenol A epoxy resin has a certain rigidity in its molecular structure, it has poor toughness after use and is prone to breakage. The applicant uses oxalyl chloride to connect two bisphenol A epoxy resin molecules, thereby extending the alkyl carbon chain of the bisphenol A epoxy resin, and making the modified bisphenol A epoxy resin have good flexibility. In addition, in order to enhance the adhesion of bisphenol A epoxy resin to metal materials, the present application introduces an ortho-diketone structure into the bisphenol A epoxy resin. The lone electron pair of the oxygen atom in the ortho-diketone structure can coordinate with the metal ions on the metal surface to form a stable five-membered ring structure, thereby changing the surface properties of the epoxy resin and the metal and increasing the adhesion of the epoxy resin.

[0023] In some embodiments, the ratio of the bisphenol A epoxy resin, oxalyl chloride and triethylamine is 1:

[0024] (0.4-0.6):(1-2).

[0025] Preferably, the ratio of the bisphenol A epoxy resin, oxalyl chloride and triethylamine is 1:0.5:1.2.

[0026] In some embodiments, the diluent is ethylene glycol diglycidyl ether or allyl glycidyl ether.

[0027] Preferably, the diluent is ethylene glycol diglycidyl ether.

[0028] In some embodiments, the structural formula of the modified curing agent is:

[0029]

[0030] In some embodiments, the modified curing agent comprises the following preparation steps:

[0031] 3,5-diaminobenzoic acid, cyclohexane, tetrahydropyran-4-ol and sodium hydroxide solid are mixed evenly, heated to 70-90° C. and stirred for 1-4 hours. After the reaction is completed, column chromatography is performed to separate the mixture, thereby obtaining a modified curing agent.

[0032] Preferably, the preparation steps of the modified curing agent are:

[0033] 3,5-diaminobenzoic acid, cyclohexane, tetrahydropyran-4-ol and sodium hydroxide solid were mixed evenly, heated to 80°C and stirred for 3 hours. After the reaction was completed, column chromatography was performed to separate the mixture, thereby obtaining a modified curing agent.

[0034] Aromatic amines are inconvenient to use as curing agents when undergoing cross-linking reactions with epoxy resins, and they have poor flexibility due to their high viscosity. The applicant modified the aromatic amines and introduced aliphatic rings to increase the flexibility of the epoxy resin paving materials while retaining the hardness of the epoxy resin paving materials. At the same time, the oxygen atoms contained in the curing agent coordinate with the metal cations on the metal surface, thereby increasing the adsorption of the paving material to the steel plate.

[0035] In some embodiments, the molar ratio of 3,5-diaminobenzoic acid, tetrahydropyran-4-ol and sodium hydroxide solid is 1:(1-6):(1.5-3).

[0036] Preferably, the molar ratio of 3,5-diaminobenzoic acid, tetrahydropyran-4-ol and sodium hydroxide solid is 1:1.2:2.

[0037] Another aspect of the present invention provides a method for preparing a high-adhesion epoxy mortar steel bridge deck paving material, comprising the following steps:

[0038] (1) Weigh the raw materials of each component A according to the corresponding weight parts: 40-60 parts of modified epoxy resin, 60-70 parts of epoxy resin, and 10-20 parts of diluent, mix them, and stir them at room temperature for 10-20 minutes to obtain component A;

[0039] (2) weighing the raw materials of each component of component B according to corresponding weight parts: 100-150 parts of modified curing agent and 100-150 parts of aminoethylpiperazine, and mixing them to obtain component B;

[0040] (3) Component A and component B are mixed according to a mass ratio, stirred for 2-6 minutes to obtain an adhesive, poured into a mortar mixer, and mixed evenly with crushed stone in a mass ratio of 1:(6-10) to obtain a mortar material, which is laid on a steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

[0041] Preferably, the method for preparing the epoxy mortar steel bridge deck paving material comprises the following steps:

[0042] (1) Weigh the raw materials of each component A according to the corresponding weight parts: 50 parts of modified epoxy resin, 62 parts of epoxy resin, and 15 parts of diluent, mix them, and stir them at room temperature for 20 minutes to obtain component A;

[0043] (2) weighing the raw materials of each component of component B according to corresponding weight parts: 120 parts of modified curing agent and 110 parts of aminoethylpiperazine, and mixing them to obtain component B;

[0044] (3) Component A and component B are mixed according to a mass ratio and stirred for 5 minutes to obtain an adhesive. The adhesive is poured into a mortar mixer and mixed evenly with crushed stone in a mass ratio of 1:8 to obtain a mortar. The mortar is laid on a steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] 1. The high-adhesion epoxy mortar steel bridge deck paving material of the present invention has a simple preparation method and has good adhesion, impact resistance, waterproof performance and coating hardness.

[0047] 2. The modified epoxy resin prepared by the present invention has a relatively long alkyl single chain, which makes up for the defects of epoxy resin in toughness and impact resistance. At the same time, the modified epoxy resin has an ortho-diketone structure that can coordinate with metal ions on the metal surface and has extremely strong metal adhesion.

[0048] 3. The modified curing agent of the present invention has a rigid aromatic ring and an aliphatic ring, and when used in combination with a modified epoxy resin, it can coordinate the hardness and impact resistance of the paving material, so that the paving material has excellent performance. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0050] In order to better illustrate the specific implementation of the present invention, the following examples are further illustrated. The weight parts described in the following examples are in grams, that is, 1 weight part is 1g.

[0051] The epoxy resin used in the embodiments and comparative examples of the present invention is bisphenol A epoxy resin E51, with an epoxy value of 0.48 to 0.54 eq / 100 g and a viscosity of ≤2500 mPa.S at 40° C., purchased from Hubei Tosoh Chemical Technology Co., Ltd.

[0052] Preparation Example 1

[0053] The preparation method of modified epoxy resin comprises the following steps:

[0054] Weigh 10g of bisphenol A epoxy resin E51 and dissolve it in dichloromethane. Under nitrogen protection, add 3.1g of triethylamine and 1.6g of oxalyl chloride dropwise in sequence, and stir at room temperature for 2h. After the reaction is completed, adjust the pH to 7 at 50°C with glacial acetic acid, wash the reaction solution with water, combine the organic layers, vacuum dry, and dry to obtain the modified epoxy resin.

[0055] Preparation Example 2

[0056] The preparation method of the modified epoxy resin is the same as that of Preparation Example 1, except that the mass of the oxalyl chloride used is 2.3 g.

[0057] Preparation Example 3

[0058] The preparation method of the modified epoxy resin is the same as that of Preparation Example 1, except that the mass of the oxalyl chloride used is 1.2 g.

[0059] Preparation Example 4

[0060] The preparation method of the modified curing agent comprises the following steps:

[0061] 10 g of 3,5-diaminobenzoic acid, 3.2 g of sodium hydroxide solid, 13.8 g of tetrahydropyran-4-ol and 500 mL of cyclohexane were mixed evenly, heated to 80° C. and stirred for 3 h. After the reaction was completed, column chromatography was performed to separate the mixture, thereby obtaining a modified curing agent.

[0062] Example 1

[0063] The present embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material, which is composed of 1 part of adhesive and 8 parts of crushed stone, by weight; each part of adhesive is mixed with 1 part of component A and 1.2 parts of component B; each part of component A includes the following raw materials in parts by weight: 50 parts of modified epoxy resin, 62 parts of bisphenol A epoxy resin, and 15 parts of diluent; each part of component B includes the following raw materials in parts by weight: 120 parts of modified curing agent and 110 parts of aminoethylpiperazine.

[0064] Wherein, the modified epoxy resin is prepared by Preparation Example 1; and the modified curing agent is prepared by Preparation Example 4.

[0065] The preparation method of the high-adhesion epoxy mortar steel bridge deck paving material of this embodiment comprises the following steps:

[0066] (1) Weighing the raw materials of each component A according to corresponding weight parts: modified epoxy resin, epoxy resin, and diluent, mixing, and stirring at room temperature for 20 minutes to obtain component A;

[0067] (2) weighing the raw materials of each component B according to corresponding weight parts: modified curing agent, aminoethylpiperazine, and mixing them to obtain component B;

[0068] (3) Component A and component B are mixed in a certain mass ratio and stirred for 5 minutes to obtain an adhesive. The adhesive is poured into a mortar mixer and mixed with crushed stones having a diameter of 8.0 mm in a mass ratio of 1:8. The mixture is stirred evenly to obtain a mortar. The mortar having a thickness of 12 mm is laid on the steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

[0069] Example 2

[0070] The present embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material, which is composed of 1 part of adhesive and 6 parts of crushed stone, by weight; each part of adhesive is mixed with 1 part of component A and 1 part of component B; each part of component A includes the following components in parts by weight: 40 parts of modified epoxy resin, 60 parts of bisphenol A epoxy resin, and 10 parts of diluent; each part of component B includes the following components in parts by weight: 100 parts of modified curing agent and 100 parts of aminoethylpiperazine.

[0071] Wherein, the modified epoxy resin is prepared by Preparation Example 1; and the modified curing agent is prepared by Preparation Example 4.

[0072] The preparation method of the high-adhesion epoxy mortar steel bridge deck paving material of this embodiment comprises the following steps:

[0073] (1) Weighing the raw materials of each component A according to corresponding weight parts: modified epoxy resin, epoxy resin, and diluent, mixing, and stirring at room temperature for 20 minutes to obtain component A;

[0074] (2) weighing the raw materials of each component B according to corresponding weight parts: modified curing agent, aminoethylpiperazine, and mixing them to obtain component B;

[0075] (3) Component A and component B are mixed in a mass ratio of 1:1, stirred for 5 minutes to obtain an adhesive, poured into a mortar mixer, mixed with crushed stone with a diameter of 8.0 mm in a mass ratio of 1:6, and stirred evenly to obtain a mortar material, and the mortar material with a thickness of 12 mm is laid on the steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

[0076] Example 3

[0077] The present embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material, which is composed of 1 part of adhesive and 10 parts of crushed stone, by weight; each part of adhesive is mixed with 1 part of component A and 1.5 parts of component B; each part of component A includes the following components in parts by weight: 60 parts of modified epoxy resin, 70 parts of bisphenol A epoxy resin, and 20 parts of diluent; each part of component B includes the following components in parts by weight: 150 parts of modified curing agent and 150 parts of aminoethyl piperazine.

[0078] Wherein, the modified epoxy resin is prepared by Preparation Example 1; and the modified curing agent is prepared by Preparation Example 4.

[0079] The preparation method of the high-adhesion epoxy mortar steel bridge deck paving material of this embodiment comprises the following steps:

[0080] (1) Weighing the raw materials of each component A according to corresponding weight parts: modified epoxy resin, epoxy resin, and diluent, mixing, and stirring at room temperature for 20 minutes to obtain component A;

[0081] (2) weighing the raw materials of each component B according to corresponding weight parts: modified curing agent, aminoethylpiperazine, and mixing them to obtain component B;

[0082] (3) Component A and component B are mixed at a mass ratio of 1:1.5, stirred for 5 minutes to obtain an adhesive, poured into a mortar mixer, mixed with crushed stone with a diameter of 8.0 mm at a mass ratio of 1:10, and stirred evenly to obtain a mortar material, and the mortar material with a thickness of 12 mm is laid on the steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

[0083] Example 4

[0084] This embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified epoxy resin is prepared by Preparation Example 2.

[0085] Example 5

[0086] This embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified epoxy resin is prepared by Preparation Example 3.

[0087] Example 6

[0088] This embodiment provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that in step (3), crushed stones with a diameter of 12.0 mm are used instead of crushed stones with a diameter of 8.0 mm.

[0089] Comparative Example 1

[0090] This comparative example provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of bisphenol A epoxy resin E51 is used instead of modified epoxy resin.

[0091] Comparative Example 2

[0092] This comparative example provides a high-adhesion epoxy mortar steel bridge deck paving material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of m-phenylenediamine is used instead of the modified curing agent.

[0093] Performance test of epoxy mortar steel bridge deck paving material

[0094] (1) Adhesion test: The test was conducted in accordance with standard GB / T9286-1998. The test results were graded according to integers from 0 to 5. The increasing value indicates poorer adhesion. Grade 0 indicates intact. Grade 4 indicates that the layer has peeled off in large pieces along the cutting edge and / or some squares have partially or completely peeled off. The affected cross-cut area is significantly greater than 35% but not significantly greater than 65%. Grade 5 indicates that the degree of peeling exceeds Grade 4.

[0095] (2) Hardness test: Tested according to standard GB / T6739-2006;

[0096] (3) Impact strength test: Tested according to standard GB / T1732-1993;

[0097] The paving materials prepared in Examples 1-6 and Comparative Examples 1-2 were evenly spread on the cleaned base surface, and the paving thickness was controlled to be 12 mm. After curing for 8 hours, they were tested according to the above test method. The test results are shown in Table 1.

[0098] (4) Water absorption test: Soak the 50*50*50mm epoxy mortar steel bridge deck paving material in water for 48 hours, test the weight of the mortar block before and after soaking, and calculate the water absorption rate according to the following formula:

[0099] Water absorption rate WX (%) = (m1-m0) / m0;

[0100] Wherein, m0 represents the weight of the mortar block before immersion; m1 represents the weight of the mortar block after immersion; WX represents the water absorption rate of the mortar (%).

[0101] Table 1

[0102]

[0103] It can be seen from Table 1 that the epoxy mortar steel bridge deck paving materials prepared in Examples 1-3 have the strongest adhesion to the steel base surface, and the material has the characteristics of high hardness, good waterproof performance and strong impact resistance, meeting the requirements for steel bridge deck paving materials; Example 4 changes the molar ratio of bisphenol A epoxy resin, oxalyl chloride and triethylamine, thereby increasing the carbon chain of the synthesized epoxy resin, reducing the epoxy content, and weakening the cross-linking reaction with the curing agent. The paving material has slightly enhanced impact strength, but the coating hardness and waterproof performance of the epoxy mortar steel bridge deck paving material are reduced; Example 5 changes the molar ratio of bisphenol A epoxy resin, oxalyl chloride and triethylamine, thereby reducing the number of molecules of the long-chain epoxy resin, resulting in a decrease in the impact resistance of the epoxy mortar steel bridge deck paving material; Example 6 uses crushed particles with a diameter exceeding the preferred range Stone weakens its bond with cement paste, increases the discontinuity of the internal structure of the concrete material, and leads to reduced impact strength and waterproof performance of the epoxy mortar steel bridge deck paving material; in Comparative Example 1, ordinary epoxy resin is used instead of modified epoxy resin, which leads to reduced adhesion and impact strength of the epoxy mortar steel bridge deck paving material, and the waterproof performance is also greatly reduced; in Comparative Example 2, m-phenylenediamine is used instead of modified curing agent, which leads to reduced adhesion, coating hardness, waterproof performance and impact strength of the epoxy mortar steel bridge deck paving material, which indicates that the modified epoxy resin and modified curing agent are not effective when used alone, and only the two can be used in combination to achieve the best effect; the test results show that the epoxy mortar steel bridge deck paving material prepared by the present invention has good adhesion, coating hardness, waterproofness and impact resistance.

[0104] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A high-adhesion epoxy mortar steel bridge deck paving material, characterized by: The high-adhesion epoxy mortar steel bridge deck paving material is prepared by mixing an adhesive and crushed stone in a weight ratio of 1: (6-10); the adhesive is prepared by mixing component A and component B in a weight ratio of 1: (1-1.5); Each portion of the A component comprises the following raw materials in parts by weight: 40-60 parts of modified epoxy resin, 60-70 parts of epoxy resin, and 10-20 parts of diluent; Each portion of the B component includes the following raw materials in parts by weight: 100-150 parts of a modified curing agent, 100-150 parts of aminoethylpiperazine, The epoxy resin is bisphenol A epoxy resin, the epoxy value is 0.38-0.56 eq / 100 g, and the viscosity at 40° C. is ≤3000 mPa.S; The modified epoxy resin comprises the following preparation steps: Weigh bisphenol A epoxy resin and dissolve it in an organic solvent. Under the protection of inert gas, add triethylamine and oxalyl chloride dropwise in sequence. Stir at room temperature for 1-4 hours. After the reaction is completed, adjust the pH to 6-7 with glacial acetic acid at 40-60 °C. Wash the reaction solution with water, combine the organic layers, vacuum spin dry, and dry to obtain the modified epoxy resin. Wherein, the molar ratio of bisphenol A epoxy resin, oxalyl chloride and triethylamine is 1:(0.4-0.6):(1-2); The modified curing agent comprises the following preparation steps: Evenly mix 3,5-diaminobenzoic acid, cyclohexane, tetrahydropyran-4-ol and sodium hydroxide solid, heat to 70-90°C and stir for 1-4 h. After the reaction is completed, separate by column chromatography to obtain a modified curing agent.

2. The high-adhesion epoxy mortar steel bridge deck paving material according to claim 1, characterized in that: The diameter of the crushed stone is 5.0mm-10.0mm.

3. The high-adhesion epoxy mortar steel bridge deck paving material according to claim 1, characterized in that: The structural formula of the modified epoxy resin is: 。 4. The high-adhesion epoxy mortar steel bridge deck paving material according to claim 1, characterized in that: The diluent is ethylene glycol diglycidyl ether or allyl glycidyl ether.

5. The high-adhesion epoxy mortar steel bridge deck paving material according to claim 1, characterized in that: The structural formula of the modified curing agent is: 。 6. A method for preparing a high-adhesion epoxy mortar steel bridge deck paving material according to any one of claims 1 to 5, characterized in that: The steps include: (1) Weigh the raw materials of each component A according to the corresponding weight parts: modified epoxy resin, epoxy resin, and diluent, mix them, and stir them at room temperature for 10-20 minutes to obtain component A; (2) Weighing the raw materials of each component of component B according to corresponding weight parts: modified curing agent, aminoethylpiperazine, and mixing them to obtain component B; (3) Component A and component B are mixed in a weight ratio and stirred for 2-6 minutes to obtain an adhesive. The adhesive is poured into a mortar mixer and mixed evenly with crushed stone in a mass ratio of 1:(6-10) to obtain a mortar. The mortar is laid on the steel bridge deck. After the adhesive is cured, a high-adhesion epoxy mortar steel bridge deck paving material is obtained.

Citation Information

Patent Citations

  • Flexible epoxy mortar for steel bridge deck paving and preparation method thereof

    CN113526917A

  • Epoxy asphalt steel bridge deck pavement pit slot repairing material and application thereof

    CN115029011A

  • Cold spraying type epoxy thin bridge deck paving material and preparation method thereof

    CN102173654A

  • Composite modified epoxy resin structural adhesive and preparation methods of composite modifier and structural adhesive

    CN108048007A

  • Medium-and-low-temperature curing high-temperature-resistant flexible epoxy adhesive and application thereof