A method for manufacturing a self-repairing invisible car cover film
By preparing self-healing polyurethane in TPU car coated film and mixing it with TPU pellets to adjust the molecular structure equilibrium dynamic chemical bonds, the contradiction between self-healing and mechanical properties is solved, and the good elasticity, toughness and self-healing of the material are achieved. Repairability, simplifying the preparation process.
Patent Information
- Application Number
- CN202410690895.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-05-30
AI Technical Summary
There is a contradiction between the self-repair function and mechanical properties of the existing TPU car coat film, and it is difficult to take into account both.
Self-healable polyurethane is prepared by reacting polycaprolactone diol with HMDI to form a prepolymer and extending the chain with disulfide bond-containing bis(2-hydroxyethyl) disulfide ether, mixing it with TPU pellets and melting it and cooling it , adjust the molecular structure and proportion to balance dynamic chemical bonds and hydrogen bonds, realize physical crosslinking, and impart good elasticity, toughness and self-healing properties to the material.
The self-healing function of polyurethane materials is realized, and the preparation process of self-healing car coat film is simplified, improving the overall performance of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of self-repairing materials and relates to a method for manufacturing a self-repairing invisible car cover film. Background Art
[0002] TPU car cover is a new type of high-performance environmentally friendly film, which is a common name for transparent paint protection film. It has super high strength and toughness. After installation, it can isolate the car paint from the air, prevent acid rain, insects, bird droppings, etc. from corroding the paint surface. It can be used for long-term protection of the car body and is widely used in the car film beauty and maintenance industry.
[0003] Car cover films are mainly made of three materials: PVC, TPH, and TPU. TPU stands for thermoplastic polyurethane elastomer, which has excellent physical and mechanical properties. It can be plasticized by heating and solidified by cooling. It has both the high elasticity of rubber materials and the high strength of engineering plastics; it has high strength, high toughness, high elasticity, high modulus, as well as excellent comprehensive properties such as chemical corrosion resistance, wear resistance, oil resistance, and strong vibration reduction ability. TPU film can be directly attached to the car paint surface for up to 5 to 10 years. It can also add color and brighten the car paint without damaging the original paint, and has excellent scratch resistance. The existing TPU car cover surface is coated with a self-repairing coating, which enables the TPU film to have an automatic repair function under heating or high temperature after being scratched.
[0004] The molecular structure and aggregation state of TPU are very complex. TPU is a polymer material formed by prepolymerization of diisocyanate and macromolecular diol, and then chain extension of small molecular diol. There are two parts in its molecule: hard segment and soft segment. Therefore, TPU material is a block copolymer composed of alternating hard segments and soft segments. The hard segment is carbamate and the soft segment is polyol. There is a certain incompatibility between the soft segment and the hard segment due to factors such as polarity, rigidity and symmetry, which leads to the aggregation state structure (kinetic concept) tending to phase separation. However, covalent bonds constrain the separation between soft and hard segments. The phase separation structure is also called the island structure. There is a competitive relationship between this structure and the covalent bond, which ultimately leads to the periodic distribution of the formed phase separation structure at the nanometer or micrometer scale, which belongs to a microphase separation structure. These factors work together to affect the mechanical properties of polyurethane materials.
[0005] TPU can be divided into polyether type, polyester type and polyolefin type according to the structural characteristics of the soft segment, and can be divided into aromatic and aliphatic TPU according to the structural characteristics of the hard segment. TPU synthesized using polyester diols has a high cohesive energy of the ester group, which is about 12.1KJ / mol. The ester group has high polarity and is easy to form hydrogen bonds between chains, which effectively inhibits the phase separation structure, making the synthesized TPU high in strength and hardness, but poor in flexibility and hydrolysis resistance. Aromatic TPU contains rigid benzene rings, which are rigid, strong, and heat-resistant, but have poor low-temperature resistance, and the unsaturated double bonds are easily oxidized, causing the material to turn yellow.
[0006] The diol is polycaprolactone, and the resulting TPU material has the comprehensive properties of polyether and polyester, with excellent mechanical strength, oil resistance, wear resistance and tear strength, good flexibility, excellent low-temperature performance, relatively low ester content, and good hydrolysis resistance. The TPU prepared from aliphatic diisocyanate is a new type of elastic plastic, and its molecular density is several times that of aromatics. It has changed a series of problems of traditional aromatic TPU such as easy yellowing, low transparency, and weak light stability. It can maintain its own transparency for a long time without changing color. It is a type of product with good anti-aging and anti-yellowing performance. The car cover TPU currently used is prepared from aliphatic isocyanate and polycaprolactone diol.
[0007] The existing TPU car cover film is a multi-layer composite structure, the most common is five layers, the top and bottom layers are PET protective films, the middle layer is TPU base film, the upper layer of TPU base film is a 1~2 micron repair layer, and the lower layer of TPU base film is an adhesive layer. If the self-repairing layer is made of acrylic resin, a UV curing process needs to be added to the existing manufacturing process.
[0008] It can be seen that such a manufacturing process is relatively cumbersome. The applied self-healing coating needs to be dissolved in a special solvent for treatment, and a special self-healing layer curing method is also required. So why not directly mix the self-healing coating with the TPU matrix material and extrude a TPU film with self-healing function at one time, but use a complex process such as coating self-healing liquid, drying, composite film and then composite to prepare it. This is due to the complexity of the above-mentioned TPU molecular structure and aggregation state and the dynamic chemical bonds contained in the self-healing material itself. The dynamic chemical bonds will form too strong physical cross-links with the hydrogen bonds of the TPU material itself, thereby hindering the movement of the soft segment molecular chain. This results in the self-healing property of the car cover film itself being reduced while achieving the strength of the car cover film, resulting in the problem that the mechanical properties and self-healing properties of the car cover film cannot be taken into account at the same time. Summary of the invention
[0009] The present invention overcomes the deficiencies of the prior art, and proposes a method for manufacturing a self-repairing invisible car cover film, thereby solving the problem that the mechanical properties and self-repairing properties of the car cover film cannot be taken into account when the self-repairing car cover film is prepared by a hybrid method.
[0010] In order to achieve the above object, the present invention is achieved through the following technical solutions:
[0011] A method for manufacturing a self-repairing invisible car cover film comprises the following steps:
[0012] 1) Preparation of prepolymer: Mix polycaprolactone diol PCL-2000 and HMDI and heat to react to obtain a prepolymer;
[0013] 2) preparing self-healing polyurethane: heating bis(2-hydroxyethyl) disulfide and the prepolymer to react to obtain self-healing polyurethane;
[0014] 3) Mix 3% to 8% by mass of self-repairable polyurethane with 92% to 97% of TPU pellets, and obtain a self-repairing invisible car cover film after melt cooling.
[0015] Preferably, in step 1), dibutyltin dilaurate catalyst is added to the mixed system of polycaprolactone diol PCL-2000 and HMDI.
[0016] More preferably, the mixed heating reaction in step 1) is heated under a protective atmosphere, the reaction temperature is 75-85° C., and the reaction time is 1.5-2.5 hours.
[0017] More preferably, the added amount of dibutyltin dilaurate catalyst is 0.03% of the total mass of the mixed system.
[0018] Preferably, in step 2), bis(2-hydroxyethyl) disulfide is first mixed with N,N-dimethylformamide or 1,4-butanediol, and then added to the prepolymer for heating reaction.
[0019] Preferably, the heating reaction in step 2) is carried out under a protective atmosphere, the reaction temperature is 75-85° C., and the reaction time is 1.5-2.5 hours.
[0020] Preferably, after the heating reaction in step 2), the self-healing polyurethane solution is poured into a polytetrafluoroethylene mold and placed in a vacuum oven at 80° C. for 24 hours to obtain the self-healing polyurethane.
[0021] Preferably, the melting in step 3) is to melt the mixed materials in a vacuum oven at 200°C.
[0022] Preferably, in step 3), the melted mixture is repeatedly vacuumed and vented to remove water and air bubbles, and then cooled.
[0023] Preferably, in step 1), the cyanohydroxyl ratio NCO / OH of the polycaprolactone diol PCL-2000 and HMDI is 1.2-1.5.
[0024] The beneficial effects of the present invention compared with the prior art are as follows:
[0025] The present invention adopts HMDI and PCL to react to form a prepolymer, and then uses disulfide-containing diol bis (2-hydroxyethyl) disulfide to extend the chain to prepare aliphatic polycaprolactone diol TPU with self-repairing function. This material is added to TPU car cover pellets, melted to obtain a mixture, and then made into a film. Through the design of molecular structure and molecular weight distribution, and adjusting the ratio of the two TPUs, the internal dynamic chemical bonds are combined with the hydrogen bonds of the TPU material itself to reach the physical cross-linking equilibrium point. The material is given good elasticity, toughness and self-repairing properties through the balance of the physical cross-linking structure, which solves the contradiction between self-repairing and mechanical properties, and realizes the self-repairing function of the polyurethane elastomer material itself; at the same time, it can effectively simplify the preparation process of the existing self-repairing car cover film. DETAILED DESCRIPTION
[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer, the present invention is further described in detail in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The technical solutions of the present invention are described in detail below in conjunction with the embodiments, but the scope of protection is not limited thereto.
[0027] The main raw material sources of the embodiments of the present invention are:
[0028] HMDI (hydrogenated diphenylmethane diisocyanate): Shandong Yantai Wanhua Polyurethane Co., Ltd., industrial grade;
[0029] Polycaprolactone diol PCL-2000 (grade 2102): Hunan Juren New Materials Co., Ltd., industrial grade;
[0030] HEDS bis(2-hydroxyethyl) disulfide: 90%, Shanghai MacLean Biochemical Technology Co., Ltd., reagent;
[0031] The synthesis method of the self-repairable polyurethane used in the following Examples 1 and 3 to 6 is:
[0032] Step 1: Preparation of prepolymer
[0033] Put polycaprolactone diol PCL-2000 into a three-necked flask, evacuate and remove water at 110°C for 2h, when the temperature of polycaprolactone diol PCL-2000 is reduced to below 50°C, weigh the cooled polycaprolactone diol PCL-2000 and HMDI according to NCO / OH of 1.4, put the two into a four-necked bottle, add 0.03% of the total mass of dibutyltin dilaurate catalyst, mix and stir, heat under nitrogen atmosphere protection, control the temperature at 80±2°C, react for 2 hours, and terminate the reaction when the isocyanate content no longer changes. The system is reduced to room temperature and sealed for storage to obtain a prepolymer of polycaprolactone diol and HMDI.
[0034] Step 2: Synthesis of self-repairable polyurethane solution
[0035] HEDS bis(2-hydroxyethyl) disulfide was added to anhydrous magnesium sulfate, dried for 24 hours, and centrifuged to remove magnesium sulfate.
[0036] Then, the dried bis(2-hydroxyethyl) disulfide was weighed according to a chain extension coefficient of 1.05 and added to the N,N-dimethylformamide (DMF) solution, and then added to the prepolymer of polycaprolactone diol and HMDI. The temperature was controlled at 80±2°C and the reaction was carried out for 2 hours under a nitrogen atmosphere to obtain a self-healing polyurethane solution with a stoichiometric ratio of NCO:OH:HEDS=4.2:3:0.5.
[0037] The self-repairable polyurethane solution was poured into a polytetrafluoroethylene mold and placed in a vacuum oven at 80°C for 24 hours to obtain a self-repairable polyurethane. The tensile strength was measured to be 17 MPa and the elongation at break was 380%.
[0038] The obtained self-repairable polyurethane was made into 2mm thick specimens, and a cross scratch with a depth of 2mm was made with a wallpaper knife. Then, it could self-repair in 8 hours at 80°C. A scratch with a depth of 0.1mm was made with a wallpaper knife, and it could self-repair in 20 minutes at 80°C. A scratch with a depth of 0.01mm was made with a wallpaper knife, and it could self-repair in 10 minutes at room temperature.
[0039] Example 1
[0040] A method for manufacturing a self-repairing invisible car cover film, the specific steps are:
[0041] The self-repairable polyurethane is placed in a beaker, and then the beaker is placed in a vacuum oven at 200°C. After the TPU pellets are melted, vacuum is drawn, and then vented (positive pressure is restored). This is repeated three times to form a TPU molten slurry to achieve the purpose of dehydration and degassing.
[0042] In order to prevent the TPU molten slurry from cooling down quickly, an insulating flat wooden board is used as the bottom plate, on which a mirror release paper used to make PU synthetic leather is laid, and stainless steel bars with controlled thickness are placed on both sides of the mirror release paper; then the TPU molten slurry is poured on the mirror release paper and scraped flat with a scraper to obtain a self-healing TPU film.
[0043] Example 2
[0044] A method for manufacturing a self-repairing invisible car cover film, which differs from Example 1 in that TPU pellets used by Lubrizol for manufacturing car covers are used instead of the self-repairing polyurethane, and other conditions are the same as those in Example 1.
[0045] Example 3
[0046] A method for manufacturing a self-repairing invisible car cover film, which differs from Example 1 in that the materials used are 99% by mass of commercially available Lubrizol TPU pellets and 1% by mass of the self-repairable polyurethane, and other conditions are the same as those in Example 1.
[0047] Example 4
[0048] A method for manufacturing a self-repairing invisible car cover film, which differs from Example 1 in that the materials used are 97% by mass of commercially available Lubrizol TPU pellets and 3% by mass of the self-repairable polyurethane, and other conditions are the same as those in Example 1.
[0049] Example 5
[0050] A method for manufacturing a self-repairing invisible car cover film, which differs from Example 1 in that the materials used are 95% by mass of commercially available Lubrizol TPU pellets and 5% by mass of the self-repairable polyurethane, and other conditions are the same as those in Example 1.
[0051] Example 6
[0052] A method for manufacturing a self-repairing invisible car cover film, which differs from Example 1 in that the materials used are 92% by mass of commercially available Lubrizol TPU pellets and 8% by mass of the self-repairable polyurethane, and other conditions are the same as those in Example 1.
[0053] The commercially available Lubrizol TPU pellets in Examples 2-6 are TPU polymerized from HMDI and PCL;
[0054] The commercially available Lubrizol TPU pellets can also be replaced by TPU pellets produced by other TPU suppliers, such as Wanhua Chemical, Meirui New Materials, etc.
[0055] Comparative Example:
[0056] The prepolymer obtained by the reaction of polycaprolactone diol and HMDI was added to the dried mixed solution of bis(2-hydroxyethyl) disulfide and 1,4-butanediol, and the temperature was controlled at 80±5°C and reacted for 2 hours under nitrogen atmosphere protection. A "one-pot" self-healing polyurethane solution was obtained. The molar ratio of bis(2-hydroxyethyl) disulfide to 1,4-butanediol was 1:9.
[0057] The self-healing polyurethane solution was poured into a polytetrafluoroethylene mold and placed in a vacuum oven at 80°C for 24 hours to obtain a self-healing polyurethane. The tensile strength was measured to be 13 MPa and the elongation at break was >450%.
[0058] The obtained self-repairable polyurethane was made into 2mm thick specimens. A cross scratch with a depth of 2mm was made with a wallpaper knife. It could self-repair within 8 hours at 60°C. A scratch with a depth of 0.1mm was made with a wallpaper knife. It could self-repair within 20 minutes at 60°C. A scratch with a depth of 0.01mm was made with a wallpaper knife. It could self-repair within 10 minutes at room temperature.
[0059] The self-repairing properties of the self-repairing TPU films prepared in Examples 1 to 6 and the self-repairing polyurethane prepared in the comparative example were measured: after the surface was scratched 20 times with 1KG 0000# steel wool, a stopwatch was used to observe the scratch recovery process under a 50x optical microscope and record the repair time; the breaking strength and breaking elongation were tested using the test conditions of GB / T1040.3-2006 for tensile properties of plastic films; the results are shown in the following table:
[0060]
[0061] The above content is a further detailed description of the present invention in combination with a specific preferred embodiment. It cannot be determined that the specific embodiments of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the present invention, which should be regarded as belonging to the present invention and the scope of patent protection determined by the submitted claims.
Claims
1. A method for manufacturing a self-repairing invisible car cover film, characterized in that: The following steps are involved: 1) Preparation of prepolymer: Mix polycaprolactone diol PCL-2000 and HMDI and heat to react to obtain a prepolymer; 2) preparing self-healing polyurethane: heating bis(2-hydroxyethyl) disulfide and the prepolymer to react to obtain self-healing polyurethane; 3) Mix 3% to 8% by mass of self-repairable polyurethane with 92% to 97% of TPU pellets, and obtain a self-repairing invisible car cover film after melt cooling.
2. The method for manufacturing a self-repairing invisible car cover film according to claim 1, characterized in that: In step 1), dibutyltin dilaurate catalyst is added to the mixed system of polycaprolactone diol PCL-2000 and HMDI.
3. The method for manufacturing a self-repairing invisible car cover film according to claim 2, characterized in that: The mixed heating reaction in step 1) is heated under a protective atmosphere, the reaction temperature is 75-85° C., and the reaction time is 1.5-2.5 hours.
4. The method for manufacturing a self-repairing invisible car cover film according to claim 2, characterized in that: The added amount of dibutyltin dilaurate catalyst is 0.03% of the total mass of the mixed system.
5. The method for manufacturing a self-repairing invisible car cover film according to claim 1, characterized in that: In step 2), bis(2-hydroxyethyl) disulfide is first mixed with N,N-dimethylformamide or 1,4-butanediol, and then added to the prepolymer for heating reaction.
6. The method for manufacturing a self-repairing invisible car cover film according to claim 1, characterized in that: The heating reaction in step 2) is carried out under a protective atmosphere, the reaction temperature is 75-85°C, and the reaction time is 1.5-2.5 hours.
7. A method for manufacturing a self-repairing invisible car cover film according to claim 1 or 6, characterized in that: After the heating reaction described in step 2), the self-healing polyurethane solution is poured into a polytetrafluoroethylene mold and placed in a vacuum oven at 80° C. for 24 hours to obtain the self-healing polyurethane.
8. The method for manufacturing a self-repairing invisible car cover film according to claim 1, characterized in that: The melting in step 3) is to melt the mixed materials in a vacuum oven at 200°C.
9. A method for manufacturing a self-repairing invisible car cover film according to claim 1 or 8, characterized in that: In step 3), the melted mixture is repeatedly vacuumed and vented to remove water and air bubbles, and then cooled.
10. The method for manufacturing a self-repairing invisible car cover film according to claim 1, characterized in that: In step 1), the cyanohydroxy ratio NCO / OH of polycaprolactone diol PCL-2000 and HMDI is 1.2-1.5.
Citation Information
Patent Citations
Preparation method of self-repairing waterproof material, self-repairing waterproof material and application thereof
CN111234175A
Preparation method of high-strength photoresponse self-repairing nano-composite polyurethane film
CN112898611A
Self-healing polyurethane film with high mechanical property as well as preparation method and application of self-healing polyurethane film
CN115850952A
Preparation method of waterborne polyurethane heat-conducting self-repairing material based on dynamic disulfide bonds
CN117757030A
Cited By
Wear-resistant self-repairing invisible car cover film and production method thereof
CN122541774A
Polycaprolactone composite film with instant self-repairing function and preparation method thereof
CN122939201A