A high-strength and high-density multi-component alloy and its preparation method and application

Through the design and rapid sintering process of high-strength high-density multi-component alloys, a multiphase heterostructure is formed, which solves the problems of growth of tungsten grains and long sintering processes, and realizes high-density, high-strength and good deformation capabilities of materials, simplifying Process and performance enhancement, suitable for high-performance applications.

CN118422027BActive Publication Date: 2024-11-26CENT SOUTH UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410602889.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-11-26
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

The existing high-density alloy materials have a high temperature and long time during the liquid phase sintering process, which limits the improvement of their mechanical properties. At the same time, the sintering process is long, making it difficult to meet the needs of industrialization efficiency, and it is brittle at room temperature. , it is difficult to have both high density, high strength and good deformation ability.

Method used

High-strength and high-density multi-component alloys are composed of W, Mo, Fe, and Ni. Through ball milling and rapid sintering technology under the protection of inert gas, a multiphase heterostructure is formed, including body-centered cubes, face-centered cubes and tetragonal structures. , combined with vacuum or plasma sintering technology, control the sintering temperature and time, inhibit the growth of tungsten grains and improve the density of the alloy.

Benefits of technology

Materials with high density, high strength and good deformation ability are achieved, the preparation process is simplified, the sintering time is shortened, the comprehensive performance of the material is improved, and the rapid densification is achieved at low temperatures, effectively inhibiting the growth of tungsten grains, suitable for Aerospace, national defense and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422027B_ABST
    Figure CN118422027B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-strength and high-density multi-component alloy and its preparation method and application. The high-strength and high-density multi-component alloy is composed of the following components in atomic percentage: W 48-62%, Mo 23-27%, Fe 7-13%, Ni 7-13%, and each component powder is prepared according to the designed atomic ratio of each component of the alloy, and the alloy material is obtained after ball milling and rapid solid phase sintering. The high-strength and high-density multi-component alloy provided by the present invention is composed of body-centered cubic structure, face-centered cubic structure and tetragonal structure phase, presenting a multi-phase heterogeneous structure, and has high density, high strength and good deformation ability; at the same time, the process is simple, the sintering cycle is short, and the time is shortened by 90% compared with traditional liquid phase sintering. It can be used as a high-performance heavy alloy in many fields such as aerospace, national defense equipment, nuclear industry, etc., such as gyroscope rotors, kinetic energy penetrators, counterweights, and medical radiation protection instruments and equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal material preparation, and in particular relates to a high-strength and high-density multi-component alloy and a preparation method and application thereof. Background Art

[0002] High-density alloy materials with high mechanical strength are widely used in many fields such as aerospace, defense equipment, and nuclear industry. Their composition design and preparation technology have always been a hot issue in basic science and applied technology. Existing high-density materials are mainly composed of more than 80wt.% tungsten elements and a small amount of other metal elements, such as nickel, iron and copper, obtained by ball milling combined with liquid phase sintering process. However, due to the high liquid phase sintering temperature and long time, the tungsten grain growth phenomenon caused by the phenomenon limits the further improvement of its mechanical properties, and the liquid phase sintering process is long. For example: A. Upadhyaya et al. [A. Upadhyaya, SK Tiwari, P. Mishra, Scripta Materialia. 56 (2007) 5-8] compared traditional liquid phase sintering with microwave sintering. The former only takes about 350 minutes for the sintering process, which cannot meet the growing demand for industrial efficiency. At the same time, most single-phase BCC alloys with high density characteristics are brittle at room temperature. Therefore, the development of a new type of high-density material with high density, high strength and good deformation ability, and a simple and efficient preparation process has become the focus of this field.

[0003] The multi-component high entropy alloys (HEAs) proposed in recent years show excellent comprehensive mechanical properties, which provides a new idea for the composition design and performance optimization of high-density alloys. Among the existing multi-component high-entropy alloy systems, alloys with high-density characteristics mainly involve refractory elements, which are difficult to melt and hot-form, and are usually prepared by powder metallurgy. Since tungsten grains tend to grow during high-temperature sintering, rapid sintering techniques such as microwave sintering and spark plasma sintering (SPS) are often used to alleviate the problem of grain growth, and suitable and efficient powder metallurgy processes still need to be explored. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0006] One of the purposes of the present invention is to provide a high-strength and high-density multi-component alloy, which is composed of face-centered cubic structure, body-centered cubic structure and tetragonal structure phases, presenting a multi-phase heterogeneous structure.

[0007] To solve the above technical problems, the present invention provides the following technical solution: a high-strength and high-density multi-component alloy, composed of the following components in atomic percentage: W 48-62%, Mo 23-27%, Fe 7-13%, Ni 7-13%; the sum of the atomic percentages of W and Mo is 74-86%, the sum of the atomic percentages of Fe and Ni is 14-26%, and the sum of the atomic percentages of each component is 100%.

[0008] As a preferred solution of the high-strength and high-density multi-component alloy of the present invention, the atomic ratio of Fe to Ni is 1:1.

[0009] As a preferred embodiment of the high-strength and high-density multi-component alloy of the present invention, it is composed of the following components in atomic percentage: W 55%, Mo 25%, Fe 10%, Ni 10%; or, W 50%, Mo 25%, Fe 12.5%, Ni 12.5%; or, W 60%, Mo 25%, Fe 7.5%, Ni 7.5%.

[0010] As a preferred embodiment of the high-strength and high-density multi-component alloy of the present invention, the high-strength and high-density multi-component alloy has the following characteristics:

[0011] (i) Mass density is 14.0 to 15.5 g cm -3 ;

[0012] (ii) compressive yield strength at room temperature is 1090-1660 MPa;

[0013] (iii) Ultimate compressive strength is 1810 to 2960 MPa;

[0014] (iv) compressive strain value greater than 25%;

[0015] (v) Vickers hardness value is 4 to 5.5 GPa.

[0016] Another object of the present invention is to provide a method for preparing the high-strength and high-density multi-component alloy as described above, comprising: preparing the raw materials of each component according to the atomic percentage of the alloy, ball milling under inert gas protection, and sintering under vacuum or inert gas protection conditions to obtain the alloy material.

[0017] As a preferred solution of the method for preparing the high-strength and high-density multi-component alloy of the present invention, the sintering is carried out by vacuum hot pressing sintering or spark plasma sintering.

[0018] As a preferred solution of the method for preparing the high-strength and high-density multi-component alloy of the present invention, wherein: the sintering is carried out under vacuum or inert gas protection conditions, and the gas pressure in the furnace is maintained at 0.0001-1 bar.

[0019] As a preferred solution of the preparation method of the high-strength and high-density multi-component alloy of the present invention, wherein: the sintering pressure is 20-50MPa; the sintering heating rate is 80-100℃ / min, the sintering temperature is 1150-1350℃, and the sintering holding time is 3-20min.

[0020] As a preferred solution of the method for preparing the high-strength and high-density multi-component alloy of the present invention, wherein: the ball-to-material ratio of the ball mill is 8 to 10:1, the ball milling time is 0.25 to 15 hours, and the ball mill speed is 200 to 500 revolutions per minute.

[0021] As a preferred solution of the method for preparing the high-strength and high-density multi-component alloy of the present invention, the raw materials of each component are pure metal powders with a purity higher than 98wt.%.

[0022] Another object of the present invention is to provide the use of the high-strength and high-density multi-component alloy as described above in the preparation of gyroscope rotors, kinetic energy penetrators, counterweights, and medical radiation protection instruments and equipment.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention introduces a certain amount of Fe and Ni elements into the high-density multi-component alloy to ensure the plasticity of the alloy. At the same time, the W element content is relatively small, the theoretical melting point of the alloy is reduced, and full densification can be achieved quickly at a lower temperature; and the rapid solid-phase sintering method can almost completely retain the low-melting point elements, and effectively inhibit the growth of tungsten grains, and the process is simple and the cycle is short. Thanks to the complementary composition design and process, the present invention finally obtains a structure with a suitable proportion of soft and hard phases and uniform distribution, which improves the comprehensive performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0026] Figure 1 This is the X-ray diffraction pattern of the high-strength and high-density multi-component alloy material provided in Example 1 of the present invention.

[0027] Figure 2This is a scanning electron microscope microstructure diagram and grain size distribution diagram of the high-strength and high-density multi-component alloy material provided in Example 1 of the present invention.

[0028] Figure 3 This is a scanning electron microscope energy spectrum distribution diagram of the high-strength and high-density multi-component alloy material provided in Example 1 of the present invention.

[0029] Figure 4 This is a compression mechanical properties curve diagram of the high-strength and high-density multi-component alloy material provided in Example 1 of the present invention.

[0030] Figure 5 This is the X-ray diffraction pattern of the high-strength and high-density multi-component alloy material provided in Example 2 of the present invention.

[0031] Figure 6 This is a scanning electron microscope microstructure diagram and grain size distribution diagram of the high-strength and high-density multi-component alloy material provided in Example 2 of the present invention.

[0032] Figure 7 This is a compression mechanical properties curve diagram of the high-strength and high-density multi-component alloy material provided in Example 2 of the present invention.

[0033] Figure 8 This is the X-ray diffraction pattern of the high-strength and high-density multi-component alloy material provided in Example 3 of the present invention.

[0034] Fig. 9 This is a scanning electron microscope microstructure diagram and grain size distribution diagram of the high-strength and high-density multi-component alloy material provided in Example 3 of the present invention.

[0035] Fig.10 This is a compression mechanical properties curve diagram of the high-strength and high-density multi-component alloy material provided in Example 3 of the present invention.

[0036] Fig.11 This is the X-ray diffraction pattern of the high-strength and high-density multi-component alloy material provided by Example 4 of the present invention.

[0037] Fig.12 This is a scanning electron microscope microstructure diagram of the high-strength and high-density multi-component alloy material provided in Example 4 of the present invention.

[0038] Fig.13 This is a compression mechanical properties curve diagram of the high-strength and high-density multi-component alloy material provided in Example 4 of the present invention.

[0039] Fig.14 This is the X-ray diffraction pattern of the high-strength and high-density multi-component alloy material provided in Example 5 of the present invention.

[0040] Fig.15 This is a scanning electron microscope microstructure diagram of the high-strength and high-density multi-component alloy material provided in Example 5 of the present invention.

[0041] Fig.16 This is a compression mechanical properties curve diagram of the high-strength and high-density multi-component alloy material provided in Example 5 of the present invention.

[0042] Fig.17 This is a diagram of the compressive mechanical properties of the high-strength and high-density multi-component alloy material provided in Example 1. DETAILED DESCRIPTION

[0043] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0044] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0045] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0046] Unless otherwise specified, the raw materials used in the examples were purchased commercially.

[0047] Example 1

[0048] According to the chemical formula W 55 Mo 25 Fe 10 Ni 10 (atomic percentage) for batching, the raw materials are metal powders corresponding to the pure elements, the metal powders are placed in a ball mill with grinding balls under inert gas protection and sealed, the ball mill with the metal powders is placed in a ball mill and run for 8.5 hours; the ball-to-material ratio during ball milling is 10:1, and the speed of the ball mill is 250 revolutions per minute;

[0049] Then, the metal powder is taken out under inert gas protection conditions, loaded into a sintering mold and compacted; the compacted embryo is sintered under vacuum conditions using a discharge plasma method, the sintering temperature is 1250°C, and the sintering time is 7 minutes; after sintering, a dense block material is obtained, namely the alloy in Example 1.

[0050] By the attached Figure 1 The X-ray diffraction pattern shows that the alloy is composed of mostly BCC phase and a small amount of FCC phase and tetragonal phase. Figure 2From the scanning electron microscope image, it can be seen that the microstructure of the bulk alloy material is evenly distributed, the BCC grains are embedded in the FCC phase in a spherical state, the tetragonal phase is either concentrated or distributed between the BCC and FCC phases, and the average size of the BCC grains is about 1.9μm. Figure 3 The energy spectrum analysis results show that the BCC phase is rich in W and Mo elements, the FCC phase is rich in Fe and Ni elements, and the tetragonal phase is rich in Fe, Ni, Mo, and W elements. Figure 4 From the compression mechanical property curve, it can be seen that the yield strength of the bulk alloy material obtained in Example 1 is ~1250MPa, the compressive strength is ~2449MPa, and the compression strain is ~34.9%, showing excellent mechanical properties.

[0051] Example 2

[0052] According to the chemical formula W 55 Mo 25 Fe 10 Ni 10 (atomic percentage) for batching, the raw materials are metal powders corresponding to the pure elements, the metal powders are placed in a ball mill with grinding balls under inert gas protection and sealed, the ball mill with the metal powders is placed in a ball mill and run for 8.5 hours; the ball-to-material ratio during ball milling is 10:1, and the speed of the ball mill is 250 revolutions per minute;

[0053] Then, the metal powder is taken out under inert gas protection conditions, loaded into a sintering mold and compacted; the compacted embryo is sintered under vacuum conditions using a discharge plasma method, the sintering temperature is 1300°C, and the sintering time is 7 minutes; after sintering, a dense block material is obtained, namely the alloy in Example 2.

[0054] By the attached Figure 5 The X-ray diffraction pattern shows that the alloy is composed of mostly BCC phase and a small amount of FCC phase and tetragonal phase. Figure 6 From the scanning electron microscope image, it can be seen that the microstructure of the bulk alloy material is evenly distributed, the BCC grains are embedded in the FCC phase in a spherical state, the tetragonal phase is either concentrated or distributed between the BCC and FCC phases, and the average size of the BCC grains is about 2.5μm. Figure 7 From the compression mechanical property curve, it can be seen that the yield strength of the bulk alloy material obtained in Example 2 is ~1282MPa, the compressive strength is ~2737MPa, and the compression strain is ~35.04%, showing excellent mechanical properties.

[0055] Example 3

[0056] According to the chemical formula W 55 Mo 25 Fe 10 Ni 10(atomic percentage) for batching, the raw materials are metal powders corresponding to the pure elements, the metal powders are placed in a ball mill with grinding balls under inert gas protection and sealed, the ball mill with the metal powders is placed in a ball mill and run for 8.5 hours; the ball-to-material ratio during ball milling is 10:1, and the speed of the ball mill is 250 revolutions per minute;

[0057] Then, the metal powder is taken out under inert gas protection conditions, loaded into a sintering mold and compacted; the compacted embryo is sintered under vacuum conditions using a discharge plasma method, the sintering temperature is 1350°C, and the sintering time is 7 minutes; after sintering, a dense block material is obtained, namely the alloy in Example 3.

[0058] By the attached Figure 8 The X-ray diffraction pattern shows that the alloy is composed of mostly BCC phase and a small amount of FCC phase and tetragonal phase. Fig. 9 From the scanning electron microscope image, it can be seen that the microstructure of the bulk alloy material is evenly distributed, the BCC grains are embedded in the FCC phase in a spherical state, the tetragonal phase is either concentrated or distributed between the BCC and FCC phases, and the average size of the BCC grains is about 2.9μm. Fig.10 From the compression mechanical property curve, it can be seen that the yield strength of the bulk alloy material obtained in Example 3 is ~1270MPa, the compressive strength is ~2762MPa, and the compression strain is ~35.4%, showing excellent mechanical properties.

[0059] Example 4

[0060] According to the chemical formula W 50 Mo 25 Fe 12.5 Ni 12.5 (atomic percentage) for batching, the raw materials are metal powders corresponding to the pure elements, the metal powders are placed in a ball mill with grinding balls under inert gas protection and sealed, the ball mill with the metal powders is placed in a ball mill and run for 8.5 hours; the ball-to-material ratio during ball milling is 10:1, and the speed of the ball mill is 250 revolutions per minute;

[0061] Then, the metal powder is taken out under inert gas protection conditions, loaded into a sintering mold and compacted; the compacted embryo is sintered under vacuum conditions using a discharge plasma method, the sintering temperature is 1200°C, and the sintering time is 7 minutes; after sintering, a dense block material is obtained, namely the alloy in Example 4.

[0062] By the attached Fig.11 The X-ray diffraction pattern shows that the alloy is composed of mostly BCC phase and a small amount of FCC phase and tetragonal phase. Fig.12From the scanning electron microscope image, it can be seen that the microstructure of the bulk alloy material is evenly distributed, the BCC grains are embedded in the FCC phase in a spherical state, the tetragonal phase is either concentrated or distributed between the BCC and FCC phases, and there is also a structure morphology in which the tetragonal phase and the FCC phase are alternately distributed in lamellar form. Fig.13 From the compression mechanical property curve, it can be seen that the yield strength of the bulk alloy material obtained in Example 4 is ~1200MPa, the compressive strength is ~2703MPa, and the compression strain is ~34%, showing excellent mechanical properties.

[0063] Example 5

[0064] According to the chemical formula W 60 Mo 25 Fe 7.5 Ni 7.5 (atomic percentage) for batching, the raw materials are metal powders corresponding to the pure elements, the metal powders are placed in a ball mill with grinding balls under inert gas protection and sealed, the ball mill with the metal powders is placed in a ball mill and run for 8.5 hours; the ball-to-material ratio during ball milling is 10:1, and the speed of the ball mill is 250 revolutions per minute;

[0065] Then, the metal powder is taken out under inert gas protection conditions, loaded into a sintering mold and compacted; the compacted embryo is sintered under vacuum conditions using a discharge plasma method, the sintering temperature is 1200°C, and the sintering time is 7 minutes; after sintering, a dense block material is obtained, namely the alloy in Example 5.

[0066] By the attached Fig.14 The X-ray diffraction pattern shows that the alloy is composed of mostly BCC phase and a small amount of FCC phase and tetragonal phase. Fig.15 From the scanning electron microscope image, it can be seen that the microstructure of the bulk alloy material is evenly distributed, the BCC grains are embedded in the FCC phase in a spherical state, and the tetragonal phase is either concentrated or distributed between the BCC and FCC phases. Fig.16 From the compression mechanical property curve, it can be seen that the yield strength of the bulk alloy material obtained in Example 5 is ~1230MPa, the compressive strength is ~2572MPa, and the compression strain is ~30%, showing excellent mechanical properties.

[0067] Comparative Example 1

[0068] According to the Journal of Alloys and Compounds [Xin Hu, Xin li Liu, Dingshun Yan, Zhi ming Li, A high-density non-equiatomic WTaMoNbV high-entropy alloy: Alloying behavior, microstructure and mechanical properties. Journal of Alloys and Compounds, 2022, 894: 162505], non-equiatomic high-density alloy W 35 Ta 35 Mo 10 Nb 10 V 10 (at.%) was prepared by ball milling the powder for 55 hours and then by spark plasma sintering (1600℃-1800℃, 1min-10min). The room temperature compression mechanical properties of the prepared high-density alloy were tested. Fig.17 As shown, the maximum compressive strength is about 2500MPa, but the compression deformation capacity at room temperature is poor.

[0069] By comparing Examples 1, 2, 3, 4 and 5 with Comparative Example 1, it can be seen that the high-density alloys outside the composition range of the present invention have lower comprehensive performance than the high-strength and high-density multi-component alloy of the present invention under the same or similar sintering process.

[0070] The present invention does not involve long-term ball milling and sintering, as well as complex heat treatment processes, and its preparation process is short and efficient. The performance of the high-strength and high-density multi-component alloy of the present invention is improved due to the reasonable design of the alloy composition, which makes the FCC phase effectively distributed between the BCC grains. This uniformly distributed organization greatly improves the room temperature deformation ability of the material.

[0071] The high-strength and high-density multi-component alloy provided by the present invention introduces appropriate amounts of Fe and Ni elements to ensure the plasticity of the alloy, and through a reasonable sintering process, the alloy is almost completely retained during low-temperature rapid sintering, thereby obtaining an alloy composed of a body-centered cubic structure, a face-centered cubic structure and a tetragonal structure phase, presenting a multi-phase heterogeneous structure, wherein the face-centered cubic structure is effectively distributed between W grains with weak mutual bonding force, and part of the tetragonal structure phase is distributed between the body-centered cubic structure and the face-centered cubic structure. This uniform organization with appropriate soft and hard phase distribution and proportion enables the alloy of the present invention to have good deformation ability while having high strength and high density.

[0072] The short-process preparation process for a high-strength and high-density multi-component alloy provided by the present invention specifically adopts ball milling and rapid solid-phase sintering methods, wherein the W content is relatively small, the Fe and Ni content is relatively high, the theoretical melting point of the alloy is reduced, and the proportion of the body-centered cubic structure and the face-centered cubic structure is reasonable, and full densification can be achieved quickly at a relatively low temperature, and the growth of tungsten grains is effectively suppressed, and the process is simple and the process is short. In addition, the comprehensive mechanical properties of the alloy vary little with changes in sintering conditions, indicating that the alloy has a high degree of flexibility in production conditions. The present invention combines new alloy design concepts and advanced preparation technologies to achieve short-process preparation of high-strength and high-density multi-component alloys.

[0073] The process of the present invention is simple and the sintering cycle is short. Compared with traditional liquid phase sintering, the time is shortened by 90%. The present invention can be used as a high-performance heavy alloy in many fields such as aerospace, national defense equipment, nuclear industry, etc., such as gyroscope rotors, kinetic energy penetrators, counterweights and medical radiation protection instruments and equipment.

[0074] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A high-strength and high-density multi-component alloy, characterized in that: The invention is composed of the following components in atomic percentage: W 48-62%, Mo 23-27%, Fe 7-13%, Ni 7-13%; the sum of the atomic percentages of W and Mo is 74-86%, the sum of the atomic percentages of Fe and Ni is 14-26%, and the sum of the atomic percentages of each component is 100%; the atomic ratio of Fe to Ni is 1:1; The alloy consists of a majority of BCC phases and a small amount of FCC phases and tetragonal phases; the BCC grains are embedded and distributed in the FCC phase in a spherical state, and the tetragonal phase is concentratedly distributed or distributed between the BCC and FCC phases.

2. The high-strength and high-density multi-component alloy according to claim 1, characterized in that: The high-strength and high-density multi-component alloy has the following characteristics: (i) Mass density is 14.0 to 15.5 g cm -3 ; (ii) compressive yield strength at room temperature is 1090-1660 MPa; (iii) Ultimate compressive strength is 1810-2960 MPa; (iv) compressive strain value greater than 25%; (v) Vickers hardness value is 4 to 5.5 GPa.

3. The method for preparing a high-strength and high-density multi-component alloy according to any one of claims 1 to 2, characterized in that: The process includes: preparing raw materials of various components according to the atomic percentage of the alloy, ball milling under the protection of an inert gas, and sintering under vacuum or inert gas protection conditions to obtain the alloy material.

4. The method for preparing a high-strength and high-density multi-component alloy according to claim 3, characterized in that: The sintering is carried out by vacuum hot pressing sintering or spark plasma sintering.

5. The method for preparing a high-strength and high-density multi-component alloy according to claim 3, characterized in that: The sintering is carried out under vacuum or inert gas protection conditions, and the gas pressure in the furnace is maintained at 0.0001~1 bar.

6. The method for preparing a high-strength and high-density multi-component alloy according to claim 3, characterized in that: The sintering has a sintering pressure of 20-50 MPa, a sintering heating rate of 80-100°C / min, a sintering temperature of 1150-1350°C, and a sintering holding time of 3-20 min.

7. The method for preparing a high-strength and high-density multi-component alloy according to claim 3, characterized in that: The ball-to-material ratio of the ball mill is 8-10:1, the ball milling time is 0.25-15 h, and the ball mill speed is 200-500 revolutions per minute.

8. The method for preparing a high-strength and high-density multi-component alloy according to claim 3, characterized in that: The raw materials for each component are pure metal powders with a purity higher than 98 wt. %.

9. Use of the high-strength and high-density multi-component alloy according to any one of claims 1 to 2 in the preparation of gyroscope rotors, kinetic energy penetrators, counterweights, and medical radiation protection instruments and equipment.

Citation Information

Patent Citations

  • Castable and forgeable solid solution tungsten alloy and preparation method

    CN109338160A

  • Tungsten high-entropy alloy with armor-piercing self-sharpening effect and preparation method thereof

    CN109536817A

  • High-toughness high-density multi-component alloy and preparation method thereof

    CN114855045A

  • Single-phase tungsten alloy for explosive-formed projectile shaped charge liner and preparation method of single-phase tungsten alloy

    CN114959395A

  • Multi-component alloy powder as well as preparation method, compact and application thereof

    CN117102474A