Anticorrosion pipeline with inner coating of corrosion-resistant alloy layer and modified epoxy powder and its connection process

By using an anti-corrosion pipeline connection process with a corrosion-resistant alloy layer and modified epoxy powder on oil field surface pipelines, the problem of anti-corrosion coating damage at pipeline connections is solved, the corrosion resistance and service life of the pipelines are improved, and the The sealing effect is improved.

CN118423515BActive Publication Date: 2024-10-11SHAANXI HUACHEN YALIAN PETROLEUM ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410875213.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-11
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The internal anti-corrosion technology of oil field surface pipelines is not mature enough for oil field applications. Especially, pipeline joints are easily damaged and difficult to detect and repair, which affects the service life of pipelines.

Method used

The anti-corrosion pipeline connection process is adopted, which is covered with a corrosion-resistant alloy layer and modified epoxy powder. By metallurgically coating the base pipe with a corrosion-resistant alloy layer, and setting up an arc-shaped welding groove and an overlapping part at the welding part, the welding groove and The overlapping parts are butt welded to ensure the integrity and flatness of the anti-corrosion coating.

Benefits of technology

It improves the corrosion resistance and impact resistance of the pipeline, extends its service life, enhances the sealing effect and anti-corrosion performance, reduces construction costs and improves laying efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118423515B_ABST
    Figure CN118423515B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of steel pipeline anticorrosion, and relates to an anticorrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder and a connection process thereof, comprising the following steps: surface treatment of a base pipe; metallurgical coating of a corrosion-resistant alloy layer at both ends of the inner periphery of the base pipe, coating an anticorrosion coating on the inner periphery of the base pipe, crimping the anticorrosion coating to the end of the corrosion-resistant alloy layer, and coating an outer anticorrosion layer on the outer periphery of the base pipe; welding the welding parts of two anticorrosion pipelines together, and at the same time forming a to-be-filled area between the opposite surfaces of the base pipes of the two anticorrosion pipelines, and performing cladding welding in the to-be-filled area to form a reinforcement layer, and finally spraying epoxy phenolic powder between the opposite surfaces of the outer anticorrosion layers of the two anticorrosion pipelines for leveling, so as to obtain a complete connection pipeline. By designing the inner anticorrosion layer as a composite structure of the anticorrosion coating and the corrosion-resistant alloy layer, the anticorrosion pipeline will not cause damage to the anticorrosion coating during butt welding, thereby ensuring the integrity and flatness of the anticorrosion layer in the connection pipeline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel pipeline anticorrosion, and in particular relates to an anticorrosion pipeline internally coated with a corrosion-resistant alloy layer and modified epoxy powder and a connection process thereof. Background Art

[0002] With the rapid development of oil fields and the increasing requirements of the country for environmental protection, the corrosion problem in oil field gathering pipelines and produced water reinjection pipelines has been bothering and affecting the development of enterprises. Especially with the improvement of environmental awareness, oil field production is also facing severe environmental pressure, especially crude oil leakage caused by damaged oil pipelines and the resulting environmental pollution, which are all difficult problems for oil field development.

[0003] At present, the traditional anti-corrosion method for oilfield surface pipelines is to spray epoxy powder on the inner and outer walls of the pipelines respectively. Since the steel pipe surface after fusion epoxy powder spraying has good anti-corrosion effect and long service life, it is widely used in oilfield surface gathering and transportation pipelines. However, the internal anti-corrosion technology of pipelines is not mature enough in oilfield applications. When welding the ends of two adjacent pipelines, high temperature will be generated at their joints, which is easy to damage the anti-corrosion coating at the pipeline joints. After welding, it is difficult to detect the internal anti-corrosion layer of the pipeline and spray repair construction on the welding points, so it is impossible to ensure the integrity and flatness of the internal anti-corrosion layer of the pipeline. When the pipeline is conveying fluid, the continuous scouring of the convex and concave surfaces of the internal anti-corrosion layer of the pipeline by the fluid seriously affects the service life of the pipeline. Summary of the invention

[0004] In view of this, the object of the present invention is to provide an anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder and a connection process thereof, so as to solve the technical problems mentioned in the prior art.

[0005] The anti-corrosion pipeline connection process with an inner coating of a corrosion-resistant alloy layer and modified epoxy powder comprises the following steps:

[0006] S1. Surface treatment of the base pipe;

[0007] S2, metallurgically coating the inner circumference of the base tube and the two ends of the opening with a corrosion-resistant alloy layer, wherein;

[0008] One end of the corrosion-resistant alloy layer extends to the outside of the base tube and has a welding portion with a tubular structure, and a circle of welding grooves with an arc-shaped cross section are recessed inwardly on the outer periphery of the welding portion, and the other end of the corrosion-resistant alloy layer protrudes outwardly and is provided with a lap joint;

[0009] S3, applying a layer of anti-corrosion coating on the inner circumference of the base pipe and between the two groups of the corrosion-resistant alloy layers, crimping the overlapped portion with the anti-corrosion coating, and applying an outer anti-corrosion layer on the outer circumference of the base pipe to obtain an anti-corrosion pipeline;

[0010] S4, clamping the outer anti-corrosion layers of the two anti-corrosion pipes on the fixing plates of the welding bracket respectively, and butting the adjacent ends of the welding parts of the two anti-corrosion pipes together to form an annular welding point with a semicircular cross section, and then performing cladding welding along the annular welding point by clamping the welding rod with a welding machine, welding the welding parts of the two anti-corrosion pipes together, and forming a to-be-filled area between the opposite surfaces of the base pipes of the two anti-corrosion pipes;

[0011] S5, clamping the welding rod with the welding machine again to perform cladding welding on the area to be filled to form a reinforcement layer;

[0012] S6. Spray epoxy phenolic powder between the opposite surfaces of the outer anti-corrosion layers of the two anti-corrosion pipes for leveling to obtain a complete connecting pipe.

[0013] Optionally, after the anti-corrosion coating is cast, its inner wall pore size is the same as that of the corrosion-resistant alloy layer.

[0014] Optionally, in S1, the surface treatment process of the substrate pipe is:

[0015] The surface of the base pipe is derusted to a thickness of 0.05 to 0.3 mm; then, an anticorrosive primer with a thickness of 0.3 to 0.4 mm is sprayed on the surface of the base pipe and dried and cured; after the primer is cured, a layer of epoxy resin adhesive is sprayed on the surface of the primer and at the location where the corrosion-resistant alloy layer is to be installed, so as to bond and position the corrosion-resistant alloy layer.

[0016] Optionally, in S3, the coating method of the anti-corrosion coating and the outer anti-corrosion layer includes:

[0017] An inner casting mold is installed on the inner circumference of the base pipe and an outer casting mold is installed on the outer circumference of the base pipe, an anti-corrosion coating is cast on the inner circumference of the base pipe by the inner casting mold to press the overlapping part of the corrosion-resistant alloy layer, and an outer anti-corrosion layer is cast on the outer circumference of the base pipe by the outer casting mold;

[0018] Continuously introducing a fluid at 10°C to 20°C into the cavities of the inner casting mold and the outer casting mold respectively to cool and solidify the anti-corrosion coating and the outer anti-corrosion layer, and after solidification, removing the inner casting mold and the outer casting mold to obtain an anti-corrosion pipeline;

[0019] After being cast, the anti-corrosion coating has the same pore size as the inner wall of the corrosion-resistant alloy layer.

[0020] Optionally, when cladding welding is performed at the annular welding point or the area to be filled, and epoxy phenolic powder is sprayed between the opposite surfaces of the outer anti-corrosion layers of the two anti-corrosion pipes for leveling, the rotating drive mechanism on the welding bracket is controlled to drive the fixed plate to drive the anti-corrosion pipe to rotate, thereby achieving uniform speed cladding welding of the anti-corrosion pipe and uniform spraying of epoxy phenolic powder.

[0021] An anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder, wherein the anti-corrosion pipeline is butt-welded using the anti-corrosion pipeline connection process described above, wherein the anti-corrosion pipeline comprises a base pipe, wherein an inner anti-corrosion layer is arranged on the inner periphery of the base pipe, and an outer anti-corrosion layer is arranged on the outer periphery of the base pipe, wherein the inner anti-corrosion layer comprises:

[0022] An anti-corrosion coating, wherein the anti-corrosion coating is installed at the middle of the inner circumference of the base pipe, and the two ends of the anti-corrosion coating are respectively aligned with the adjacent ends of the outer anti-corrosion layer;

[0023] A corrosion-resistant alloy layer, wherein one end of the corrosion-resistant alloy layer close to the anti-corrosion coating protrudes outward and is provided with a lap joint, and the lap joint is embedded in the anti-corrosion coating; one end of the corrosion-resistant alloy layer away from the anti-corrosion coating extends to the outside of the base pipe and is provided with a welding portion with a tubular structure; a circle of welding grooves is recessed inward on the outer periphery of the welding portion, and the cross-section of the welding groove is an arc-shaped structure, which is used to butt together the adjacent ends of the welding portions of two anti-corrosion pipes to form an annular welding point with a semicircular cross-section, so as to position and align the welding point of the welding rod.

[0024] Optionally, the overlapping portion is an annular structure, and a center line of the overlapping portion coincides with a center line of the corrosion-resistant alloy layer.

[0025] Optionally, the length of the welding portion is greater than the radius of the welding rod, and the length of the welding portion is less than the diameter of the welding rod.

[0026] Optionally, the anti-corrosion coating and the outer anti-corrosion layer are both made of epoxy phenolic powder coating;

[0027] The epoxy phenolic powder coating is made of phenolic epoxy resin, phenolic curing agent, mica powder, filler, degassing agent, leveling agent, first auxiliary agent, second auxiliary agent, 2-methylimidazole and pigment, and the weight percentage of each component is:

[0028] Phenolic epoxy resin 45~55%

[0029] Phenolic curing agent 18~22%

[0030] Mica powder 6~10%

[0031] Filler 18~25%

[0032] Degassing agent 0.2~0.3%

[0033] Leveling agent 0.8~1.2%

[0034] The first auxiliary agent 0.4~0.6%

[0035] Second additive 0.3~0.5%

[0036] The remaining components are 2-methylimidazole and pigment.

[0037] Optionally, the corrosion-resistant alloy layer is a nickel alloy layer or a titanium alloy layer.

[0038] Optionally, the length of the corrosion-resistant alloy layer along the axial direction is greater than the heat conduction distance of the welding groove during cladding welding.

[0039] The beneficial effects that the present invention can produce include:

[0040] The anti-corrosion pipe coated with a corrosion-resistant alloy layer and modified epoxy powder and the connection process thereof provided by the present invention designs the inner anti-corrosion layer to be a composite structure of an anti-corrosion coating and a corrosion-resistant alloy layer, so that during the connection process of the anti-corrosion pipe, the corrosion-resistant alloy layers of two adjacent anti-corrosion pipes are butt-welded, thereby not causing damage to the anti-corrosion coating, and the welding groove is arranged on the outer periphery of the welding part, so that no welding protrusions or grooves are formed on the inner surface of the welding part during the welding process, thereby ensuring the integrity and flatness of the anti-corrosion layer inside the connected pipe. Compared with previous anti-corrosion pipes, the connected pipe has better corrosion resistance and impact resistance, and improves the service life of the connected pipe; at the same time, the inner anti-corrosion layers of two adjacent anti-corrosion pipes are connected together by welding, which further enhances the sealing effect and anti-corrosion performance between the two adjacent anti-corrosion pipes. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic flow diagram of the anti-corrosion pipeline connection process coated with a corrosion-resistant alloy layer and modified epoxy powder according to the present invention;

[0042] Figure 2 It is a structural schematic diagram of the anti-corrosion pipeline of the present invention during pouring construction;

[0043] Figure 3 It is a structural schematic diagram of the connecting pipeline of the present invention;

[0044] Figure 4 This is a schematic diagram of the structure of the anti-corrosion pipeline prefabricated by the casting process of the present invention;

[0045] Figure 5 This is a schematic diagram of the structure of the anti-corrosion pipeline prefabricated by the spraying process of the present invention;

[0046] Figure 6It is a structural schematic diagram of the welding bracket in the present invention;

[0047] Figure 7 For the present invention Figure 6 Sectional view at AA;

[0048] In the figure: 1. base pipe, 2. anti-corrosion coating, 3. corrosion-resistant alloy layer, 4. overlapping part, 5. welding part, 6. welding groove, 7. outer anti-corrosion layer, 8. support frame, 9. fixed plate, 10. electric telescopic rod, 11. arc-shaped clamping plate, 12. base, 13. C-shaped mounting groove, 14. mounting groove, 15. gear, 16. rotating shaft, 17. driving motor, 18. reinforcement layer, 19. inner casting mold, 20. outer casting mold, a is the pouring mouth of the outer casting mold, b is the pouring mouth of the inner casting mold, c is the cavity fluid inlet direction of the outer casting mold, d is the cavity fluid outlet direction of the outer casting mold, e is the cavity fluid inlet direction of the inner casting mold, and f is the cavity fluid outlet direction of the inner casting mold. DETAILED DESCRIPTION

[0049] The present invention is described in detail below with reference to the accompanying drawings and embodiments, but the present invention is not limited to these embodiments.

[0050] Embodiment 1:

[0051] like Figures 1 to 3 As shown, the present invention provides an anti-corrosion pipeline connection process coated with a corrosion-resistant alloy layer and modified epoxy powder, comprising the following steps: step one, surface treatment of a base pipe 1; step two, metallurgically coating the inner circumference of the base pipe 1 and at both ends of the opening with a corrosion-resistant alloy layer 3, wherein one end of the corrosion-resistant alloy layer 3 extends to the outside of the base pipe 1 and has a welding portion 5 with a tubular structure, and a circle of welding grooves 6 with an arc-shaped cross-section is recessed inwardly on the outer circumference of the welding portion 5, and the other end of the corrosion-resistant alloy layer 3 is protruding outwardly and provided with a lap portion 4; step three, applying a layer of anti-corrosion coating 2 on the inner circumference of the base pipe 1 and between the two groups of corrosion-resistant alloy layers 3, and crimping the lap portion 4 with the anti-corrosion coating 2, and coating the outer circumference of the base pipe 1 Apply an outer anti-corrosion layer 7 to obtain an anti-corrosion pipe; Step 4, clamp the outer anti-corrosion layers 7 of the two anti-corrosion pipes on the fixed plate 9 of the welding bracket respectively, and butt the adjacent ends of the welding parts 5 of the two anti-corrosion pipes together to form an annular welding point with a semicircular cross-section, and then use a welding machine to clamp the welding rod to perform cladding welding along the annular welding point to weld the welding parts 5 of the two anti-corrosion pipes together, and at the same time, form a to-be-filled area between the opposite surfaces of the base pipes 1 of the two anti-corrosion pipes; Step 5, clamp the welding rod again by the welding machine to perform cladding welding in the to-be-filled area to form a reinforcement layer 18; Step 6, spray epoxy phenolic powder between the opposite surfaces of the outer anti-corrosion layers 7 of the two anti-corrosion pipes for leveling to obtain a complete connecting pipe.

[0052] In the above, by designing the inner anti-corrosion layer as a composite structure of the anti-corrosion coating 2 and the corrosion-resistant alloy layer 3, the corrosion-resistant alloy layers 3 of two adjacent anti-corrosion pipes are butt-welded during the connection process of the anti-corrosion pipes, thereby not causing damage to the anti-corrosion coating 2. Compared with the previous anti-corrosion coating inside the steel pipe, the anti-corrosion pipe has the advantage of no need for patching after the connection is formed, which greatly reduces the manpower and material investment costs at the construction site and improves the efficiency of pipeline laying construction; and the welding groove 6 is arranged on the outer periphery of the welding portion 5, so that no welding protrusions or grooves are formed on the inner surface of the welding portion 5 during the welding process, thereby ensuring the integrity and flatness of the anti-corrosion layer inside the connected pipe. Compared with the previous anti-corrosion pipes, the connected pipe has better corrosion resistance and impact resistance, and improves the service life of the connected pipe; at the same time, the inner anti-corrosion layers of the two adjacent anti-corrosion pipes are connected together by welding, which further enhances the sealing effect and anti-corrosion performance between the two adjacent anti-corrosion pipes.

[0053] It should be noted that the advantage of the anti-corrosion pipe in this embodiment being free of patching after being connected and formed means that the two groups of anti-corrosion pipes will not cause damage to the internal anti-corrosion coating during the butt welding process, so that after the anti-corrosion pipes are connected and formed, there is no need to repair the internal anti-corrosion coating of the two adjacent groups of anti-corrosion pipes, so that it has the benefit of free of patching.

[0054] Furthermore, the surface treatment process of the base pipe 1 is as follows: the surface of the base pipe 1 is rust-removed by grinding or sandblasting, and the rust-removed thickness of the surface of the base pipe 1 is 0.05-0.3mm; then a 0.3-0.4mm thick anti-corrosion primer is sprayed on the surface of the base pipe 1 and dried and cured; after the primer is cured and formed, a layer of epoxy resin adhesive is sprayed on the surface of the primer and at the installation position of the corrosion-resistant alloy layer 3, which is used to bond and position the corrosion-resistant alloy layer 3; at the same time, the epoxy resin adhesive can fill the installation gap between the corrosion-resistant alloy layer 3 and the base pipe 1, enhance the density between the corrosion-resistant alloy layer 3 and the base pipe 1, thereby reducing the vibration noise generated when the fluid impacts the corrosion-resistant alloy layer 3, and improving the service life of the inner anti-corrosion layer, such as fluid impact corrosion-resistant Alloy layer 3, if the corrosion-resistant alloy layer 3 has warping due to loose filling, the connection surface with the anti-corrosion coating 2 will be damaged, causing the inner anti-corrosion layer to gradually lose its anti-corrosion effect as the fluid continues to flush, thereby causing problems such as pipeline leakage; and, when welding the corrosion-resistant alloy layer 3, there is no need to clamp it with the help of a clamp. The base pipe 1 can be directly installed on the welding bracket to weld the connection between the corrosion-resistant alloy layer 3 and the base pipe 1. Compared with the previous method of clamping the corrosion-resistant alloy layer 3 at the end of the base pipe 1 with a clamp for welding, the steel anti-corrosion pipeline connection process will not be affected by the situation where the welding surface is blocked by the clamp during the welding process. Therefore, there is no need to repeatedly disassemble and install the clamp, which is convenient for the corrosion-resistant alloy layer 3 to be welded and formed in one time, which helps to improve construction efficiency and welding accuracy.

[0055] As a preferred embodiment of the present invention, the coating method of the anti-corrosion coating 2 and the outer anti-corrosion layer 7 comprises: referring to Figures 2 to 4 As shown, an inner casting mold 19 is installed on the inner circumference of the base tube 1 and an outer casting mold 20 is installed on the outer circumference of the base tube 1. The anti-corrosion coating 2 is cast on the inner circumference of the base tube 1 through the inner casting mold 19 to press the overlapped portion 4 of the corrosion-resistant alloy layer 3, and the outer anti-corrosion layer 7 is cast on the outer circumference of the base tube 1 through the outer casting mold 20; then, a 10°C to 20°C fluid is continuously introduced into the cavities of the inner casting mold 19 and the outer casting mold 20 respectively to cool and solidify the anti-corrosion coating 2 and the outer anti-corrosion layer 7. Molding, wherein, in this embodiment, water at 15°C is continuously introduced to uniformly cool the anti-corrosion coating 2 and the outer anti-corrosion layer 7. When the outflowing water temperature is close to 15°C, it indicates that the anti-corrosion coating 2 and the outer anti-corrosion layer 7 have been solidified and formed, and then the inner casting mold 19 and the outer casting mold 20 are removed to obtain an anti-corrosion pipeline; and the anti-corrosion coating 2 after casting has the same pore size as the inner wall of the corrosion-resistant alloy layer 3, which is used to reduce the impact damage of the fluid on the anti-corrosion coating 2 when the anti-corrosion pipeline is conveying the fluid.

[0056] In the above-mentioned embodiment, in order to accurately control the pouring amount of the anti-corrosion coating 2 and the outer anti-corrosion layer 7, pressure control valves are respectively installed at the pouring ports of the inner pouring mold 19 and the outer pouring mold 20. The standard pressure value of the pressure control valve is set to the pouring pressure value of the inner pouring mold 19 and the outer pouring mold 20 respectively using the conveying pump during the pouring construction process. At the same time, the pressure control valve is connected to a controller (a single-chip microcomputer is selected) and an alarm. When the standard pressure value of the pressure control valve is greater than the pouring pressure value, it means that the pouring construction is completed. The controller controls the pressure control valve and the conveying pump to close and sends an alarm through the alarm to remind the end of this pouring construction.

[0057] As another embodiment of the present invention, the coating method of the anti-corrosion coating 2 and the outer anti-corrosion layer 7 comprises: referring to Figure 5As shown, the substrate 1 is heat treated by a medium frequency heater, the inner surface temperature of the substrate 1 is heated to 170°C to 190°C, and then the epoxy phenolic powder coating is uniformly sprayed at a preset position on the inner circumference of the substrate 1 by carrying an inner spray gun on a spray trolley at a moving speed of 1.5m / min to 10m / min, wherein the amount of epoxy phenolic powder sprayed by the inner spray gun is 40g / min to 105g / min, thereby forming an anti-corrosion coating 2 on the inner circumference of the substrate 1 to crimp the connecting portion 4 of the corrosion-resistant alloy layer 3; the outer surface temperature of the substrate 1 is heated to 180°C to 195°C, and then the outer circumference of the substrate 1 is uniformly sprayed at a moving speed of 3m / min to 10m / min on the outer circumference of the substrate 1 by carrying an outer spray gun on a spray trolley. min at a moving speed of 300 g / min to spray the epoxy phenolic powder coating at a preset position at a uniform speed, wherein the epoxy phenolic powder sprayed by the external spray gun is in an amount of 300 g / min to 600 g / min, thereby forming an outer anti-corrosion layer 7 on the outer periphery of the base pipe 1; when the anti-corrosion coating 2 and the outer anti-corrosion layer 7 are all sprayed, the anti-corrosion coating 2 and the outer anti-corrosion layer 7 on the surface of the base pipe 1 are cooled and solidified by a water-cooling solidification system. Specifically, the water flow in the spray pipe is automatically adjusted to cool the base pipe 1 with the epoxy phenolic powder coating, and the outer surface temperature of the base pipe 1 is cooled to 40°C to 45°C, thereby prefabricating an anti-corrosion pipeline, which is convenient for subsequent on-site butt welding of two adjacent groups of anti-corrosion pipelines at the construction site. In the above embodiment, in order to ensure that the anti-corrosion coating 2 and the outer anti-corrosion layer 7 do not interfere with each other during spraying construction, the inner surface temperature and the outer surface temperature of the base pipe 1 are controlled within 180°C ~ 190°C, and the inner spray gun and the outer spray gun are installed on the same spraying carriage, or the moving speeds of the two spraying carriages are controlled to be the same, so that their moving speeds are controlled within 3m / min ~ 10m / min, and the anti-corrosion coating 2 and the outer anti-corrosion layer 7 are sprayed on the surface of the base pipe 1 at the same time. At the same time, the anti-corrosion coating 2 has the same inner wall pore size as the corrosion-resistant alloy layer 3 after spraying, which is used to reduce the impact damage of the fluid on the anti-corrosion coating 2 when the anti-corrosion pipeline is transporting the fluid.

[0058] In the above, when cladding welding is performed at the annular welding point or the area to be filled, and epoxy phenolic powder is sprayed between the opposite surfaces of the outer anti-corrosion layers 7 of the two anti-corrosion pipes for leveling, the rotating drive mechanism on the welding bracket is controlled to drive the fixed plate 9 to drive the anti-corrosion pipe to rotate, thereby achieving uniform speed cladding welding of the anti-corrosion pipe and uniform spraying of the epoxy phenolic powder.

[0059] Specifically, the present invention provides a welding bracket with rotation and clamping functions in order to butt-weld a plurality of anti-corrosion pipes into the connection pipes required at the construction site through the steel anti-corrosion pipe connection process. Figure 6 and Figure 7As shown, the welding bracket includes a support frame 8, a rotary drive mechanism is installed on the top of the support frame 8, and at least two groups of fixed disks 9 are installed on the rotary drive mechanism. The center lines of the two groups of fixed disks 9 coincide with each other, and each group of fixed disks 9 is used to clamp and fix the anti-corrosion pipe, wherein three installation cavities are evenly arranged along the ring inside the fixed disk 9, and an electric telescopic rod 10 is installed in each installation cavity. The angle between the center lines of two adjacent electric telescopic rods 10 is 120°, and the output end of the electric telescopic rod 10 passes through the inner circumference of the fixed disk 9 and is installed with an arc-shaped clamping plate 11, and the inner concave surface of the arc-shaped clamping plate 11 faces the side close to the center of the fixed disk 9, which is used for when the anti-corrosion pipe penetrates into the fixed disk 9 and is located between the three arc-shaped clamping plates 11, the three electric telescopic rods 10 are controlled to extend synchronously and drive the arc-shaped clamping plates 11 to clamp the outer circumference of the anti-corrosion pipe, thereby realizing the positioning and clamping of the anti-corrosion pipe. Specifically, the rotary drive mechanism includes a base 12 arranged at the bottom of each fixed plate 9, the base 12 is fixedly mounted on the top of the support frame 8, a C-shaped mounting groove 13 is provided on the top of the base 12, the opening of the C-shaped mounting groove 13 is arranged upward, a mounting through groove 14 is provided on one side of the opening of the C-shaped mounting groove 13, and the mounting through groove 14 runs through the outer periphery of the base 12 away from the side of the C-shaped mounting groove 13, the bottom of the fixed plate 9 is rotatably mounted in the C-shaped mounting groove 13, and the outer periphery of the fixed plate 9 is provided with an external tooth profile; each mounting through groove 14 is provided with a gear 15, the gear 15 is meshed with the outer tooth profile of the fixed disk 9; a rotating shaft 16 is arranged on the outer periphery of one of the bases 12 located on one side of the support frame 8, one end of the rotating shaft 16 passes through all the mounting grooves 14 and is rotatably connected to the base 12, the inner periphery of the gear 15 is fixedly mounted on the outer periphery of the rotating shaft 16, and the other end of the rotating shaft 16 is fixedly connected to the output shaft of the driving motor 17 through a coupling, and the driving motor 17 is fixedly mounted on the base 12 through a frame; wherein, the electric telescopic rod 10 and the driving motor 17 are respectively connected to the control unit and the external power supply.

[0060] In the above, after the two anti-corrosion pipes are clamped and fixed in the fixed plate 9, the control unit controls the driving motor 17 to drive the rotating shaft 16 to rotate, so that the rotating shaft 16 drives several gears 15 to rotate synchronously, and then drives the fixed plate 9 to drive the anti-corrosion pipes to rotate through the gear 15. Then, the operator performs butt welding on the two anti-corrosion pipes on one side of the welding bracket, and spraying and leveling construction of the outer anti-corrosion layer 7, so that there is no need to turn over the two anti-corrosion pipes during the operation, thereby avoiding secondary clamping errors in the anti-corrosion pipes during the turning process, which can improve construction accuracy and efficiency, and reduce the labor intensity of operators.

[0061] It should be noted that the working state of the fixed disk 9 is reciprocating rotation, that is, it rotates forward for one circle and then rotates reversely to reset before performing the next forward rotation, so as to prevent the fixed disk 9 from continuously rotating and tearing off the external power cord of the electric telescopic rod 10; at the same time, in order to prevent the external power cord from scratching the external anti-corrosion layer during movement, a circle of U-shaped wire clamping groove can be arranged in a ring at one end of the fixed disk 9, and the opening of the U-shaped wire clamping groove faces the outer circumference of the fixed disk 9, so that the fixed disk 9 can wrap the external power cord in the U-shaped wire clamping groove during rotation.

[0062] Embodiment 2:

[0063] Reference Figure 4 and Figure 5 As shown, the present invention provides an anti-corrosion pipeline with an inner coating of a corrosion-resistant alloy layer and modified epoxy powder, the anti-corrosion pipeline is butt-welded using the above-mentioned anti-corrosion pipeline connection process, the anti-corrosion pipeline comprises a base pipe 1, an inner anti-corrosion layer is arranged on the inner periphery of the base pipe 1, an outer anti-corrosion layer 7 is arranged on the outer periphery of the base pipe 1, the inner anti-corrosion layer comprises an anti-corrosion coating 2 and a corrosion-resistant alloy layer 3, the anti-corrosion coating 2 is installed in the middle of the inner periphery of the base pipe 1, and the two ends of the anti-corrosion coating 2 are respectively aligned with the adjacent ends of the outer anti-corrosion layer 7; the corrosion-resistant alloy layer 3 is close to the base pipe 1, and the outer anti-corrosion layer 7 is arranged on the outer periphery of the base pipe 1. One end of the anti-corrosion coating 2 is protruding outward and is provided with a lap joint 4, which is embedded in the anti-corrosion coating 2. The corrosion-resistant alloy layer 3 is extended away from the end of the anti-corrosion coating 2 to the outside of the base pipe 1 and is provided with a welding portion 5 with a tubular structure. The outer periphery of the welding portion 5 is recessed inward and is provided with a circle of welding grooves 6, and the cross section of the welding grooves 6 is an arc-shaped structure, which is used to butt the adjacent ends of the welding portions 5 of two anti-corrosion pipes together to form an annular welding point with a semicircular cross section, so as to locate and align the welding point of the welding rod. Specifically, the corrosion-resistant alloy layer 3 is a nickel alloy layer or a titanium alloy layer, and the anti-corrosion coating 2 and the outer anti-corrosion layer 7 are both made of epoxy phenolic powder coating; the epoxy phenolic powder coating is made of phenolic epoxy resin, phenolic curing agent, mica powder, filler, degassing agent, leveling agent, first auxiliary agent, second auxiliary agent, 2-methylimidazole and pigment, and the weight percentage of each component is:

[0064] Phenolic epoxy resin 45~55%

[0065] Phenolic curing agent 18~22%

[0066] Mica powder 6~10%

[0067] Filler 18~25%

[0068] Degassing agent 0.2~0.3%

[0069] Leveling agent 0.8~1.2%

[0070] The first auxiliary agent 0.4~0.6%

[0071] Second additive 0.3~0.5%

[0072] The remaining components are 2-methylimidazole and pigment.

[0073] In the above, the performance indicators of the modified epoxy phenolic powder fusion-bonded epoxy powder coating used in this application are shown in Table 1 according to the Petroleum and Natural Gas Industry Standard SY / T 0442-2010 "Technical Standard for Internal Anticorrosion Layer of Steel Pipeline Fusion-bonded Epoxy Powder".

[0074] Table 1

[0075]

[0076] Furthermore, the overlapping portion 4 is an annular structure, and the center line of the overlapping portion 4 coincides with the center line of the corrosion-resistant alloy layer 3, which is used to cast the anti-corrosion coating 2 between the overlapping portions 4 of two groups of corrosion-resistant alloy layers 3, thereby enhancing the connection structural strength between the corrosion-resistant alloy layer 3 and the anti-corrosion coating 2.

[0077] Furthermore, the length of the welding portion 5 is greater than the radius of the welding rod, which facilitates extending the welding point of the welding rod from between the opposite surfaces of the two base pipes 1 to the annular welding point for cladding welding processing. The length of the welding portion 5 is less than the diameter of the welding rod, which facilitates cladding welding processing between the opposite surfaces of the two base pipes 1.

[0078] In the above-mentioned embodiment, the length of the corrosion-resistant alloy layer 3 along the axial direction is greater than the heat conduction distance of the welding groove 6 during cladding welding, thereby preventing the base pipe 1 from transferring heat to the anti-corrosion coating 2 and the outer anti-corrosion layer 7 during the welding process, thereby ensuring the integrity of the anti-corrosion coating 2 and the outer anti-corrosion layer 7 during the welding process.

[0079] In the above, by using modified epoxy phenolic powder coating to prepare the anti-corrosion coating 2 and the outer anti-corrosion layer 7, it can be ensured that the glass transition temperature of the inner anti-corrosion layer reaches above 140°C, and the inner anti-corrosion layer does not soften below 130°C, thereby ensuring the anti-corrosion effect; while the glass transition temperature of ordinary epoxy powder coating is basically between 95 and 105°C, which can meet the anti-corrosion requirements of the inner wall of ordinary pipelines, but when used as the inner anti-corrosion layer of deep wells or pipelines transporting high-pressure and high-temperature media, ordinary anti-corrosion epoxy powder coatings are difficult to meet the anti-corrosion requirements, resulting in the anti-corrosion coating being easily softened and falling off, causing corrosion of the pipeline. Among them, the performance indicators of the anti-corrosion coating of the present application are shown in Table 2.

[0080] Table 2

[0081]

[0082] The above are only several embodiments of the present invention and are not intended to limit the present invention in any form. Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, using the above disclosed technical content to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. Anti-corrosion pipeline connection process with inner coating of corrosion-resistant alloy layer and modified epoxy powder, characterized in that: The following steps are involved: S1. Derusting the surface of the base tube (1), wherein the thickness of the derusting on the surface of the base tube (1) is 0.05 to 0.3 mm; then spraying an anticorrosive primer with a thickness of 0.3 to 0.4 mm on the surface of the base tube (1) and performing a drying and curing treatment; after the primer is cured, spraying a layer of epoxy resin adhesive on the surface of the primer and at the location where the corrosion-resistant alloy layer (3) is to be installed, for bonding and positioning the corrosion-resistant alloy layer (3); S2, metallurgically coating the inner circumference of the base tube (1) and at both ends of the opening with a corrosion-resistant alloy layer (3), wherein: One end of the corrosion-resistant alloy layer (3) extends to the outside of the base tube (1) and has a welding portion (5) with a tubular structure, and a circle of welding grooves (6) with an arc-shaped cross section are provided inwardly on the outer periphery of the welding portion (5), and the other end of the corrosion-resistant alloy layer (3) protrudes outwardly and is provided with an overlap portion (4); S3, coating an anti-corrosion coating (2) on the inner periphery of the base pipe (1) and between the two groups of the corrosion-resistant alloy layers (3), crimping the overlapped portion (4) with the anti-corrosion coating (2), and coating an outer anti-corrosion layer (7) on the outer periphery of the base pipe (1) to obtain an anti-corrosion pipeline, wherein; An inner casting mold (19) is installed on the inner circumference of the base tube (1), and an outer casting mold (20) is installed on the outer circumference of the base tube (1). The inner casting mold (19) is used to cast an anti-corrosion coating (2) on the inner circumference of the base tube (1) to crimp the overlapping portion (4) of the corrosion-resistant alloy layer (3), and the outer casting mold (20) is used to cast an outer anti-corrosion layer (7) on the outer circumference of the base tube (1). The casting ports of the inner casting mold (19) and the outer casting mold (20) are A pressure control valve is installed at each of the two locations, the standard pressure value of the pressure control valve is set to the pouring pressure value of the inner pouring mold (19) and the outer pouring mold (20) respectively using the delivery pump during the pouring construction process, the pressure control valve is connected to a controller and an alarm, when the standard pressure value of the pressure control valve is greater than the pouring pressure value, it means that the pouring construction is completed, the controller controls the pressure control valve and the delivery pump to close and sends an alarm through the alarm to remind the pouring construction to be completed; Then, a fluid at 10°C to 20°C is continuously introduced into the cavities of the inner casting mold (19) and the outer casting mold (20) to cool and solidify the anti-corrosion coating (2) and the outer anti-corrosion layer (7). After solidification, the inner casting mold (19) and the outer casting mold (20) are removed to obtain an anti-corrosion pipeline; after casting, the anti-corrosion coating (2) has the same pore size as the inner wall of the corrosion-resistant alloy layer (3); S4, respectively clamping the outer anti-corrosion layers (7) of the two anti-corrosion pipes on the fixing plate (9) of the welding bracket, and butting the adjacent ends of the welding parts (5) of the two anti-corrosion pipes together to form an annular welding point with a semicircular cross section, and then performing cladding welding along the annular welding point by clamping the welding rod with a welding machine, welding the welding parts (5) of the two anti-corrosion pipes together, and forming a to-be-filled area between the opposite surfaces of the base pipes (1) of the two anti-corrosion pipes; S5, clamping the welding rod with the welding machine again to perform cladding welding on the area to be filled to form a reinforcement layer (18); S6. Spray epoxy phenolic powder between the opposite surfaces of the outer anti-corrosion layers (7) of the two anti-corrosion pipes for leveling to obtain a complete connected pipe.

2. The anti-corrosion pipeline connection process with an inner coating of a corrosion-resistant alloy layer and modified epoxy powder according to claim 1 is characterized in that: When cladding welding is performed at the annular welding point or the area to be filled, and epoxy phenolic powder is sprayed between the opposite surfaces of the outer anti-corrosion layers (7) of the two anti-corrosion pipes for leveling, the rotary drive mechanism on the welding bracket is controlled to drive the fixed plate (9) to drive the anti-corrosion pipe to rotate, thereby achieving uniform cladding welding of the anti-corrosion pipe and uniform spraying of epoxy phenolic powder. 3.Anti-corrosion pipeline covered with corrosion-resistant alloy layer and modified epoxy powder, characterized in that: The anti-corrosion pipeline is butt-welded using the anti-corrosion pipeline connection process according to any one of claims 1 to 2, the anti-corrosion pipeline comprising a base pipe (1), an inner anti-corrosion layer is arranged on the inner periphery of the base pipe (1), an outer anti-corrosion layer (7) is arranged on the outer periphery of the base pipe (1), the inner anti-corrosion layer comprising: An anti-corrosion coating (2), the anti-corrosion coating (2) being installed at the middle of the inner circumference of the base pipe (1), and the two ends of the anti-corrosion coating (2) being aligned with the adjacent ends of the outer anti-corrosion layer (7); A corrosion-resistant alloy layer (3), wherein one end of the corrosion-resistant alloy layer (3) close to the anti-corrosion coating (2) is provided with an overlap portion (4) protruding outward, and the overlap portion (4) is embedded in the anti-corrosion coating (2); one end of the corrosion-resistant alloy layer (3) away from the anti-corrosion coating (2) extends to the outside of the base pipe (1) and is provided with a welding portion (5) with a tubular structure, and a circle of welding grooves (6) is provided inwardly on the outer periphery of the welding portion (5), and the cross section of the welding groove (6) is an arc-shaped structure, which is used for butting the adjacent ends of the welding portions (5) of two anti-corrosion pipes together to form an annular welding point with a semicircular cross section, so as to position and align the welding point of the welding rod; The anti-corrosion coating (2) and the outer anti-corrosion layer (7) are both made of epoxy phenolic powder coating; The epoxy phenolic powder coating is made of phenolic epoxy resin, phenolic curing agent, mica powder, filler, degassing agent, leveling agent, first auxiliary agent, second auxiliary agent, 2-methylimidazole and pigment, and the weight percentage of each component is: Phenolic epoxy resin 45~55% Phenolic curing agent 18~22% Mica powder 6~10% Filler 18~25% Degassing agent 0.2~0.3% Leveling agent 0.8~1.2% The first auxiliary agent 0.4~0.6% Second additive 0.3~0.5% The remaining components are 2-methylimidazole and pigment.

4. The anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder according to claim 3, characterized in that: The overlapping portion (4) is an annular structure, and the center line of the overlapping portion (4) coincides with the center line of the corrosion-resistant alloy layer (3).

5. The anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder according to claim 3, characterized in that: The length of the welding portion (5) is greater than the radius of the welding rod, and the length of the welding portion (5) is less than the diameter of the welding rod.

6. The anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder according to claim 3, characterized in that: The corrosion-resistant alloy layer (3) is a nickel alloy layer or a titanium alloy layer.

7. The anti-corrosion pipeline coated with a corrosion-resistant alloy layer and modified epoxy powder according to claim 3, characterized in that: The length of the corrosion-resistant alloy layer (3) along the axial direction is greater than the heat conduction distance of the welding groove (6) during cladding welding.