Silicon-based heterojunction solar cell and preparation method thereof

By introducing a carbon-doped amorphous silicon layer into the first passivation layer of silicon-based heterojunction solar cells, the conductivity and passivation effect are optimized, the problems of insufficient conductivity and current loss are solved, and the short-circuit current and Fill factor improves device performance.

CN118431309BActive Publication Date: 2024-10-18TRINA SOLAR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410896155.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-18
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

When existing silicon-based heterojunction solar cells improve conductivity and passivation effects, they face problems of insufficient conductivity and increased parasitic absorption, resulting in current loss and reduced fill factor.

Method used

The carbon-doped amorphous silicon layer is introduced into the first passivation layer, and the defect density of the carbon-doped amorphous silicon is used to perform energy band jumping, optimizing the conductivity of the film layer, reducing the thickness of the passivation layer, and improving the short-circuit current and filling factor of the battery. .

Benefits of technology

It increases the short-circuit current and fill factor of silicon-based heterojunction solar cells, improves device performance, and avoids the problems of increased resistance and reduced fill factor caused by excessively thick intrinsic amorphous silicon layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118431309B_ABST
    Figure CN118431309B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of solar cells, and provides a silicon-based heterojunction solar cell and a method for preparing the same. The silicon-based heterojunction solar cell comprises: a silicon substrate, and a first passivation layer, an N-type doping layer, a first transparent conductive oxide layer, and a first electrode stacked in sequence on the front side of the silicon substrate and along a first direction; wherein the first passivation layer comprises: a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer stacked in sequence along the first direction. The technical solution provided by the present application introduces a carbon-doped amorphous silicon layer into the first passivation layer, which is conducive to optimizing the conductivity of the film layer, thereby improving the short-circuit current and fill factor of the battery, and improving the device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a silicon-based heterojunction solar cell and a preparation method thereof. Background Art

[0002] Silicon-based heterojunction cell (Heterojunction with Intrinsic Thin Layer, referred to as "HJT") is a high-efficiency solar cell with technical advantages such as good weak light response, high cell efficiency, fewer production processes, and high bifaciality.

[0003] In existing battery structure solutions, intrinsic amorphous silicon is usually used as a passivation material for the surface of crystalline silicon. However, since the conductivity of intrinsic amorphous silicon is too poor and a certain thickness is required to maintain good passivation, certain trade-offs need to be made in the process. In addition, in order to achieve good ohmic contact between the N-doped layer and the transparent conductive oxide (TCO) layer, the doping concentration of the contact layer needs to be increased to enhance the carrier transmission performance. However, increasing the doping concentration will increase parasitic absorption accordingly, which will lead to current loss in solar cells. Summary of the invention

[0004] The embodiment of the present application provides a silicon-based heterojunction solar cell and a method for preparing the same to solve or alleviate the technical problems mentioned above. The silicon-based heterojunction solar cell of the embodiment of the present application introduces a carbon-doped amorphous silicon layer into the first passivation layer (i.e., the N-type passivation layer), which is beneficial to optimize the conductivity of the film layer, thereby increasing the short-circuit current and fill factor of the battery, and improving the device performance.

[0005] In a first aspect, an embodiment of the present application provides a silicon-based heterojunction solar cell, comprising:

[0006] A silicon substrate, the silicon substrate comprising a front side and a back side arranged opposite to each other;

[0007] A first passivation layer, an N-type doping layer, a first transparent conductive oxide layer, and a first electrode are sequentially stacked on the front side of the silicon substrate and along a first direction;

[0008] Wherein, the first passivation layer comprises: a first sub-passivation layer, a carbon-doped amorphous silicon layer and a second sub-passivation layer which are sequentially stacked along the first direction;

[0009] The carbon-doped amorphous silicon layer is disposed between the first sub-passivation layer and the second sub-passivation layer, which is beneficial for electrons to utilize the defect density of the carbon-doped amorphous silicon to perform energy band hopping, thereby improving the conductivity of the first passivation layer.

[0010] In a second aspect, an embodiment of the present application provides a method for preparing a silicon-based heterojunction solar cell, comprising:

[0011] Providing a silicon substrate, wherein the silicon substrate comprises a front side and a back side that are oppositely arranged;

[0012] Forming a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer in sequence on the front surface of the silicon substrate; wherein the first sub-passivation layer, the carbon-doped amorphous silicon layer, and the second sub-passivation layer together constitute a first passivation layer;

[0013] forming an N-type doped layer on the second sub-passivation layer;

[0014] forming a first transparent conductive oxide layer on the N-type doped layer;

[0015] A first electrode is formed on the first transparent conductive oxide layer.

[0016] The above technical solution adopted in the embodiment of the present application may have the following advantages:

[0017] The first passivation layer located on the front side of the silicon substrate includes a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer stacked in sequence. The first sub-passivation layer close to the silicon substrate has a good passivation effect, and the second sub-passivation layer far from the silicon substrate is conducive to the formation of subsequent doped layers. The carbon-doped amorphous silicon layer located between the first sub-passivation layer and the second sub-passivation layer is made of silicon carbide (Si x C y , x is not equal to y), which is conducive to optimizing the conductivity of the film layer, reducing the thickness of the first passivation layer, and avoiding problems such as increased resistance and reduced fill factor caused by an excessively thick intrinsic amorphous silicon layer. In addition, the gap between the valence band and the conduction band of silicon carbide is relatively wide, at 2.8-4.2eV, which can increase the short-circuit current and fill factor of silicon-based heterojunction solar cells, thereby improving device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0019] Figure 1 is a schematic structural diagram of a silicon-based heterojunction solar cell provided in Example 1 of the present application;

[0020] Figure 2 is a schematic structural diagram of a silicon-based heterojunction solar cell provided in Example 5 of the present application;

[0021] Figure 3 is a schematic structural diagram of a silicon-based heterojunction solar cell provided in Example 6 of the present application;

[0022] Figure 4 It is a schematic diagram of the structure of a silicon-based heterojunction solar cell provided in Example 10 of the present application.

[0023] Description of reference numerals:

[0024] 100. Silicon substrate;

[0025] 210, first passivation layer; 211, first sub-passivation layer; 212, carbon-doped amorphous silicon layer; 213, second sub-passivation layer; 220, N-type doping layer; 221, first oxygen-containing seed layer; 222, second oxygen-containing seed layer; 223, N-type doped main layer; 224, N-type doped contact layer; 230, first transparent conductive oxide layer; 240, first electrode; 250, pre-passivation layer;

[0026] 310, second passivation layer; 311, third intrinsic amorphous silicon layer; 312, fourth intrinsic amorphous silicon layer; 313, fifth intrinsic amorphous silicon layer; 320, P-type doping layer; 321, P-type doping seed layer; 322, P-type doping main layer; 323, P-type doping contact layer; 330, second transparent conductive oxide layer; 340, second electrode;

[0027] D1, first direction; D2, second direction. DETAILED DESCRIPTION

[0028] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.

[0029] like Figures 1 to 4 As shown, the embodiment of the present application provides a silicon-based heterojunction solar cell, comprising:

[0030] A silicon substrate 100, wherein the silicon substrate 100 includes a front side and a back side that are oppositely arranged;

[0031] A first passivation layer 210, an N-type doping layer 220, a first transparent conductive oxide layer 230, and a first electrode 240 are sequentially stacked on the front side of the silicon substrate 100 and along a first direction D1;

[0032] The first passivation layer 210 includes: a first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212, and a second sub-passivation layer 213 which are sequentially stacked along the first direction D1;

[0033] The carbon-doped amorphous silicon layer is arranged between the first sub-passivation layer and the second sub-passivation layer, which is beneficial for electrons to utilize the defect density of the carbon-doped amorphous silicon to perform energy band hopping, thereby improving the conductivity of the first passivation layer.

[0034] In the embodiment of the present application, the first passivation layer 210 located on the front side of the silicon substrate 100 includes a first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212, and a second sub-passivation layer 213 which are stacked in sequence. The first sub-passivation layer 211 close to the silicon substrate 100 has a good passivation effect, and the second sub-passivation layer 213 far from the silicon substrate 100 is conducive to the formation of subsequent doped layers. The carbon-doped amorphous silicon layer 212 located between the first sub-passivation layer 211 and the second sub-passivation layer 213 is made of silicon carbide (Si x C y , x is not equal to y), has a high defect density, which is conducive to electrons using the high defect density of carbon-doped amorphous silicon to perform energy band hopping, which is conducive to optimizing the conductivity of the film layer, and can reduce the thickness of the first passivation layer 210, and try to avoid problems such as increased resistance and reduced fill factor caused by an excessively thick intrinsic amorphous silicon layer. In addition, the gap between the valence band and the conduction band of silicon carbide is relatively wide, at 2.8-4.2eV, which can increase the short-circuit current and fill factor of silicon-based heterojunction solar cells, thereby improving device performance.

[0035] The silicon substrate 100 may be an N-type silicon substrate or a P-type silicon substrate. The N-type silicon substrate is an N-type single crystal silicon substrate (for example, a crystal phase of <100> or <111> ), the P-type silicon substrate is a P-type single crystal silicon substrate (for example, the crystal phase is <100> or <111> ).

[0036] The structure of each layer of a silicon-based heterojunction solar cell and its coordination relationship with other layers will be further introduced below by way of example.

[0037] In an optional embodiment, the structure factor of the first sub-passivation layer is greater than the structure factor of the carbon-doped amorphous silicon layer, and the structure factor of the carbon-doped amorphous silicon layer is greater than the structure factor of the second sub-passivation layer.

[0038] It should be noted that the density of each layer structure of a silicon-based heterojunction solar cell can be characterized by a structure factor. The higher the density, the lower the structure factor, and vice versa. In this application, the structure factor ( R* ) is calculated as: R* = I (SiH 2 ) / ( I(SiH) + I(SiH 2 ) ),in I(SiH) and I(SiH 2 )Respectively expressed at 2000cm -1 SiH at 2090cm -1 The integrated intensity of the Gaussian peak of the stretching vibration mode of SiH2 at , and the structure factor are related to the microvoids in the film and are used to characterize the density of the film.

[0039] In some embodiments, in the first passivation layer, the structure factors of the sublayers stacked in sequence along the first direction decrease in sequence, that is, the density increases in sequence. The structure factor of the first sub-passivation layer close to the silicon substrate is higher, so the density is lower, the refractive index is higher, and the passivation performance is better; the structure factor of the second sub-passivation layer close to the N-type doped layer is lower, so the density is higher, the refractive index is lower, and the conductivity of the solar cell is improved; the structure factor of the carbon-doped amorphous silicon layer is in the middle, and the photoelectric conversion performance of the solar cell can be improved under the premise of ensuring passivation. Because if the structure factor of the carbon-doped amorphous silicon layer is too high, the density is too low, the defect degree in the carbon-doped amorphous silicon layer is high, and the conductivity is poor; if the structure factor of the carbon-doped amorphous silicon layer is too low, the density is too high, and it is easy to form Si x C y (x=y) structure is not conducive to conductivity.

[0040] In an optional embodiment, the structure factor of the first sub-passivation layer is 0.6-0.75, the structure factor of the carbon-doped amorphous silicon layer is 0.45-0.58, and the structure factor of the second sub-passivation layer is 0.3-0.43. Exemplarily, the structure factor of the first sub-passivation layer can be 0.6, 0.63, 0.65, 0.68, 0.7 or 0.75, the structure factor of the carbon-doped amorphous silicon layer can be 0.45, 0.47, 0.5, 0.52, 0.55 or 0.58, and the structure factor of the second sub-passivation layer can be 0.3, 0.35, 0.38, 0.4 or 0.43.

[0041] In an optional embodiment, in the carbon-doped amorphous silicon layer, the carbon content is 0.1-4.4 at %.

[0042] If the amorphous silicon layer does not contain carbon or the carbon content is less than 0.1at%, the conductivity of the amorphous silicon layer is low; if the carbon content in the amorphous silicon layer is greater than 4.4at%, the light transmittance of the film will decrease; when the carbon content is 0.1-4.4at%, the carbon-doped amorphous silicon layer not only has a high conductivity to reduce the resistance, but also has good light transmittance. In some embodiments, the carbon content in the carbon-doped amorphous silicon layer is 3-4.4at%. Exemplarily, the carbon content in the carbon-doped amorphous silicon layer can be 3at%, 3.2at%, 3.5at%, 3.6at%, 3.8at%, 4at%, 4.2at% or 4.4at%.

[0043] In an optional embodiment, the thickness ratio of the first sub-passivation layer, the carbon-doped amorphous silicon layer, and the second sub-passivation layer is 1:(1-4):(5-7). For example, the thickness ratio of the first sub-passivation layer, the carbon-doped amorphous silicon layer, and the second sub-passivation layer can be 1:1:5, 1:1:6, 1:1:7, 1:2:5, 1:2:6, or 1:2:7, 1:3:5, 1:3:6, 1:3:7, 1:4:5, 1:4:6, or 1:4:7.

[0044] In some embodiments, the first sub-passivation layer is a first oxygen-doped amorphous silicon layer or a first intrinsic amorphous silicon layer, and the silicon-oxygen ratio of the first oxygen-doped amorphous silicon layer is greater than 0.1 and less than 1. Exemplarily, the silicon-oxygen ratio of the first oxygen-doped amorphous silicon layer is 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 0.95.

[0045] In some embodiments, the second sub-passivation layer is a second oxygen-doped amorphous silicon layer or a second intrinsic amorphous silicon layer, and the silicon-oxygen ratio of the second oxygen-doped amorphous silicon layer is greater than 0.1 and less than 1. Exemplarily, the silicon-oxygen ratio of the second oxygen-doped amorphous silicon layer is 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 0.95.

[0046] In some embodiments, the thickness of the first sub-passivation layer is 0.5-2nm, the thickness of the carbon-doped amorphous silicon layer is 0.5-2nm, and the thickness of the second sub-passivation layer is 3-6nm. Exemplarily, the thickness of the first sub-passivation layer can be 0.5nm, 0.8nm or 1nm, the thickness of the carbon-doped amorphous silicon layer can be 0.5nm, 0.8nm or 1nm, and the thickness of the second sub-passivation layer can be 3nm, 4nm, 4.5nm, 5nm, 5.5nm or 6nm.

[0047] In some embodiments, the thickness of the first passivation layer is 5-8 nm. For example, the thickness of the first passivation layer may be 5 nm, 6 nm, 7 nm or 8 nm.

[0048] In an optional embodiment, if Figure 2 and Figure 4 As shown, the silicon-based heterojunction solar cell further includes: a pre-passivation layer 250 disposed between the silicon substrate 100 and the first passivation layer 210;

[0049] Wherein, the material of the pre-passivation layer 250 includes silicon oxide;

[0050] The pre-passivation layer 250 is formed by sequentially adopting a hot water slow pull process and a plasma etching process.

[0051] In the embodiment of the present application, the pre-passivation layer 250 is located on the surface of the silicon substrate 100, which can reduce the influence of the external environment (such as water vapor, etc.) on the silicon substrate 100. In addition, when the material of the pre-passivation layer 250 includes silicon oxide, the interface quality between the silicon substrate 100 and the first passivation layer 210 can be improved, the defects and stress at the interface can be reduced, and the passivation effect can be further improved. When the thickness of the first passivation layer 210 is reduced, it can ensure that the device has a good fill factor.

[0052] In some embodiments, the thickness of the pre-passivation layer is 0.01-0.03 nm (e.g., 0.01 nm, 0.02 nm, or 0.03 nm). The pre-passivation layer within this thickness range is sufficient to reduce defects and stress at the interface and improve the passivation effect, and the thinner pre-passivation layer has fewer voids, which can reduce the amount of adsorbed gas.

[0053] In an optional embodiment, if Figure 3 and Figure 4 As shown, the N-type doped layer 220 includes: a first oxygen-containing seed layer 221, a second oxygen-containing seed layer 222, an N-type doped main layer 223, and an N-type doped contact layer 224 which are sequentially stacked along a first direction D1;

[0054] The silicon-oxygen ratio of the first oxygen-containing seed layer is greater than or equal to 0.05 and less than 0.4, the silicon-oxygen ratio of the second oxygen-containing seed layer is greater than or equal to 0.4 and less than 0.7, and the silicon-oxygen ratio of the N-type doped main layer is greater than or equal to 0.6 and less than 1; and / or

[0055] The phosphorus-silicon ratio of the first oxygen-containing seed layer is greater than or equal to 0.01 and less than 0.05, the phosphorus-silicon ratio of the second oxygen-containing seed layer is greater than or equal to 0.05 and less than 0.3, the phosphorus-silicon ratio of the N-type doped main layer is greater than or equal to 0.06 and less than 1, and the phosphorus-silicon ratio of the N-type doped contact layer is greater than or equal to 0.06 and less than 1.

[0056] The doping element of the N-type doping layer is an N-type semiconductor material, which includes phosphorus and may also include other elements, such as arsenic and antimony. The N-type doping layer may be located on the light incident surface.

[0057] The first oxygen-containing seed layer needs to maintain the characteristics of high crystallization rate, but high crystallization rate will lead to band contraction, resulting in band discontinuity and affecting carrier transmission. The band gap and Fermi level position can be adjusted by low oxygen doping to ensure the continuity of the band; compared with the first oxygen-containing seed layer, the silicon-oxygen ratio and phosphorus-silicon ratio of the second oxygen-containing seed layer are both larger. The second oxygen-containing seed layer, as a supplementary layer of the first oxygen-containing seed layer, belongs to a buffer transition layer and is used to reduce the instability of the early preparation process of the N-type doped main layer. The first oxygen-containing seed layer and the second oxygen-containing seed layer are used to jointly improve the crystallization rate of the N-type doped main layer. The N-type doped main layer is the main structure of the N-type doped layer. By adopting high oxygen content and high phosphorus doping, the conductivity is improved while ensuring the transmittance, and the balance of electrical and optical properties is maintained. The N-type doped contact layer adopts oxygen-free and high phosphorus doping to form a good ohmic contact with the first transparent conductive oxide layer, which improves the fill factor and current density of the solar cell.

[0058] In some embodiments, the silicon-oxygen ratios of the first oxygen-containing seed layer, the second oxygen-containing seed layer, and the N-type doped body layer increase in sequence.

[0059] In some embodiments, the silicon-oxygen ratio of the first oxygen-containing seed layer is 0.1-0.35, the silicon-oxygen ratio of the second oxygen-containing seed layer is 0.4-0.58, and the silicon-oxygen ratio of the N-type doped body layer is 0.6-0.95. Exemplarily, the silicon-oxygen ratio of the first oxygen-containing seed layer can be 0.1, 0.15, 0.2, 0.25, 0.3 or 0.35, the silicon-oxygen ratio of the second oxygen-containing seed layer can be 0.4, 0.45, 0.5 or 0.55, 0.58, and the silicon-oxygen ratio of the N-type doped body layer is 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9 or 0.95.

[0060] In some embodiments, the phosphorus-silicon ratios of the first oxygen-containing seed layer, the second oxygen-containing seed layer, the N-type doped body layer, and the N-type doped contact layer increase in sequence.

[0061] In some embodiments, the phosphorus-silicon ratio of the first oxygen-containing seed layer is 0.01-0.045, the phosphorus-silicon ratio of the second oxygen-containing seed layer is 0.05-0.25, the phosphorus-silicon ratio of the N-type doped body layer is 0.06-0.98, and the phosphorus-silicon ratio of the N-type doped contact layer is 0.06-0.98. Exemplarily, the phosphorus-silicon ratio of the first oxygen-containing seed layer can be 0.01, 0.015, 0.018, 0.02, 0.03, 0.04, or 0.045, the phosphorus-silicon ratio of the second oxygen-containing seed layer can be 0.05, 0.06, 0.07, 0.08, 0.1, 0.15, 0.2, or 0.25, the phosphorus-silicon ratio of the N-type doped main layer can be 0.06, 0.1, 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 0.98, and the phosphorus-silicon ratio of the N-type doped contact layer can be 0.06, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 0.98.

[0062] In an optional embodiment, the crystallization rate of the first oxygen-containing seed layer is 52%-70%; the crystallization rate of the second oxygen-containing seed layer is 50.5%-68%; the crystallization rate of the N-type doped main layer is greater than 10% and less than 50%, and the crystallization rate of the N-type doped contact layer is greater than 0% and less than 50%; wherein, the crystallization rate of the second oxygen-containing seed layer is less than the crystallization rate of the first oxygen-containing seed layer.

[0063] If the crystallization rate of the N-type doped layer is too high, the degree of recombination between electrons and holes in the valence band is high, which will lead to additional loss of filling factor; if the crystallization rate of the N-type doped layer is too low, it may be unfavorable for carrier transport, which will also cause a decrease in the filling factor. Therefore, in order to make the battery have a higher filling factor, it is necessary to reasonably control the crystallization rate of the N-type doped layer. The N-type doped layer of the embodiment of the present application controls the crystallization rate by setting multiple sublayers. The first oxygen-containing seed layer belongs to a seed layer with a high crystallization rate and has a crystallization inducing effect; the second oxygen-containing seed layer also belongs to a seed layer with a high crystallization rate, and the crystallization rate of the second oxygen-containing seed layer is slightly lower than that of the first oxygen-containing seed layer, which has a transition buffering effect; the crystallization rate of the N-type doped main layer is low, and it has good photoelectric conversion performance; the N-type doped contact layer adopts a low crystallization rate to further reduce the contact resistance between the N-type doped layer and the first transparent oxide layer, thereby improving the filling factor of the solar cell and improving the optical performance.

[0064] In some embodiments, the crystallization rates of the first oxygen-containing seed layer, the second oxygen-containing seed layer, the N-type doped main layer, and the N-type doped contact layer decrease in sequence.

[0065] In some embodiments, the crystallization rate of the first oxygen-containing seed layer is 55-69% (for example, 55%, 60%, 65% or 69%); the crystallization rate of the second oxygen-containing seed layer is 51-65% (for example, 51%, 55%, 60% or 65%); the crystallization rate of the N-type doped main layer is 12-45% (for example, 12%, 20%, 25%, 30%, 35%, 40% or 45%), and the crystallization rate of the N-type doped contact layer is 5-45% (for example, 5%, 10%, 12%, 20%, 25%, 30%, 35%, 40% or 45%); and the crystallization rate of the second oxygen-containing seed layer is less than the crystallization rate of the first oxygen-containing seed layer.

[0066] In some embodiments, the carbon-to-silicon ratio of the N-type doped body layer is 0.01-0.04. Exemplarily, the carbon-to-silicon ratio of the N-type doped body layer is 0.01, 0.02, 0.03, or 0.04.

[0067] In some embodiments, the thickness of the first oxygen-containing seed layer and the thickness of the second oxygen-containing seed layer are respectively and independently 0.1-1nm (for example, 0.1nm, 0.3nm, 0.4nm, 0.5nm, 0.6nm, 0.8nm or 1nm); the thickness of the N-type doped main layer is 8-20nm (for example, 8nm, 10nm, 11nm, 12nm, 14nm or 15nm, 18nm or 20nm); the thickness of the N-type doped contact layer is 1-3nm (for example, 1nm, 1.5nm, 2nm, 2.5nm or 3nm).

[0068] In an optional embodiment, if Figure 3 and Figure 4 As shown, the silicon-based heterojunction solar cell further comprises:

[0069] A second passivation layer 310, a P-type doping layer 320, a second transparent conductive oxide layer 330, and a second electrode 340 are sequentially stacked on the back side of the silicon substrate 100 and along the second direction D2;

[0070] The P-type doped layer 320 includes: a P-type doped seed layer 321, a P-type doped main layer 322 and a P-type doped contact layer 323 which are sequentially stacked along the second direction D2;

[0071] The second direction D2 is opposite to the first direction D1;

[0072] wherein the boron-silicon ratio of the P-type doped seed layer is greater than 0.01 and less than 0.9, the boron-silicon ratio of the P-type doped main layer is greater than 0.04 and less than 0.95, the boron-silicon ratio of the P-type doped contact layer is greater than 0.06 and less than 1, and the boron-silicon ratio of the P-type doped seed layer is less than the boron-silicon ratio of the P-type doped main layer; and / or

[0073] The crystallization rate of the P-type doped seed layer is greater than 50% and less than 70%, the crystallization rate of the P-type doped main layer is greater than 25% and less than 60%, the crystallization rate of the P-type doped contact layer is greater than 20% and less than 50%, and the crystallization rate of the P-type doped seed layer is greater than the crystallization rate of the P-type doped main layer.

[0074] The doping element of the P-type doping layer is a P-type semiconductor material, and the P-type semiconductor material includes boron and may also include other elements, such as gallium. The P-type doping layer may be located on the backlight side.

[0075] The P-type doped layer includes a P-type doped seed layer, a P-type doped main layer and a P-type doped contact layer which are stacked in sequence. The P-type doped seed layer is an incubation layer, which is used to improve the crystallization rate of the P-type doped main layer. Since the diffusion rate of doping elements such as boron atoms is relatively fast, the boron silicon ratio of the P-type doped seed layer is relatively low and the crystallization rate is relatively high compared with the P-type doped main layer. The P-type doped main layer is mainly used for conduction. The electrical performance of the solar cell can be improved by adopting a high boron doping and low crystallization rate method. The P-type doped contact layer adopts a high boron doping method to form a good ohmic contact between the P-type doped contact layer and the second transparent conductive oxide layer, thereby improving the conductive performance.

[0076] In some embodiments, the boron-silicon ratio of the P-type doped seed layer, the P-type doped main layer, and the P-type doped contact layer increases in sequence. In some embodiments, the crystallization rate of the P-type doped seed layer, the P-type doped main layer, and the P-type doped contact layer decreases in sequence.

[0077] In some embodiments, the boron-silicon ratio of the P-type doped seed layer is 0.02-0.3 (for example, 0.02, 0.04, 0.05, 0.08, 0.1, 0.14, 0.2 or 0.3), the boron-silicon ratio of the P-type doped main layer is 0.05-0.5 (0.05, 0.07, 0.1, 0.15, 0.2, 0.3, 0.4 or 0.5), the boron-silicon ratio of the P-type doped contact layer is 0.08-0.98 (for example, 0.08, 0.1, 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.65, 0.6, 0.7, 0.8, 0.9 or 0.98), and the boron-silicon ratio of the P-type doped seed layer is less than the boron-silicon ratio of the P-type doped main layer.

[0078] In some embodiments, the crystallization rate of the P-type doped seed layer is 55-69% (for example, 55%, 60%, 65% or 69%); the crystallization rate of the P-type doped main layer is 30-55% (for example, 12%, 30%, 35%, 40%, 45%, 50% or 55%), the crystallization rate of the P-type doped contact layer is 21-45% (for example, 21%, 25%, 30%, 35%, 40% or 45%), and the crystallization rate of the P-type doped seed layer is greater than the crystallization rate of the P-type doped main layer.

[0079] In some embodiments, the thickness of the P-type doped seed layer is 1-2nm (e.g., 1nm, 1.3nm, 1.5nm, 1.7nm, or 2nm), the thickness of the P-type doped main layer is 20-30nm (e.g., 20nm, 22nm, 23nm, 25nm, 26nm, 27nm, 28nm, or 30nm), and the thickness of the P-type doped contact layer is 2-4nm (e.g., 2nm, 3nm, or 4nm).

[0080] In an optional embodiment, if Figure 3 and Figure 4 As shown, the second passivation layer 310 includes a third intrinsic amorphous silicon layer 311, a fourth intrinsic amorphous silicon layer 312, and a fifth intrinsic amorphous silicon layer 313 which are sequentially stacked along the second direction D2;

[0081] The structure factor of the third intrinsic amorphous silicon layer is greater than that of the fourth intrinsic amorphous silicon layer, and the structure factor of the fourth intrinsic amorphous silicon layer is greater than that of the fifth intrinsic amorphous silicon layer.

[0082] The second passivation layer includes three intrinsic amorphous silicon layers with different structure factors. The higher the structure factor of the intrinsic amorphous silicon layer, the lower the density, the better the passivation effect, but the worse the conductive effect. Therefore, the third intrinsic amorphous silicon layer close to the silicon substrate has a higher structure factor and a lower density, and has a good passivation effect. The fifth intrinsic amorphous silicon layer close to the P-type doped layer needs to take into account both passivation performance and conductive performance, and has a lower structure factor and a higher density.

[0083] In an optional embodiment, the structure factor of the third intrinsic amorphous silicon layer is 0.5-0.7; the structure factor of the fourth intrinsic amorphous silicon layer is 0.4-0.6; and the structure factor of the fifth intrinsic amorphous silicon layer is 0.2-0.4. Exemplarily, the structure factor of the third intrinsic amorphous silicon layer may be 0.5, 0.55, 0.6, 0.63, 0.65 or 0.7, the structure factor of the fourth intrinsic amorphous silicon layer may be 0.4, 0.45, 0.47, 0.5, 0.52, 0.55 or 0.6, and the structure factor of the fifth intrinsic amorphous silicon layer may be 0.2, 0.25, 0.3, 0.35, 0.38 or 0.4.

[0084] In some embodiments, the thickness of the third intrinsic amorphous silicon layer is 0.5-2 nm (e.g., 0.5 nm, 1 nm, 1.5 nm, or 2 nm), the thickness of the fourth intrinsic amorphous silicon layer is 1-2.5 nm (e.g., 1 nm, 1.5 nm, 2 nm, or 2.5 nm), and the thickness of the fifth intrinsic amorphous silicon layer is 4-8 nm (e.g., 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, or 8 nm).

[0085] In some embodiments, the material of the first transparent conductive oxide layer and the material of the second transparent conductive oxide layer respectively and independently include one or more of indium tin oxide (ITO), indium zinc oxide (IZO), tungsten-doped indium oxide (IWO), fluorine-doped tin oxide (FTO), cerium-doped indium oxide (ICO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), and VTTO. Among them, the composition of VTTO is In2O3:ZrO2:TiO2:Ga2O3 with a mass ratio of 98.5:0.5:0.5:0.5. The materials of these transparent conductive oxide layers have high light transmittance and high conductivity.

[0086] In some embodiments, the texture thickness of the first transparent conductive oxide layer is 65-70 nm (eg, 65 nm, 68 nm, 70 nm), and the refractive index of the first transparent conductive oxide layer is 1.8-2.1 (eg, 1.8, 1.9, 1.97, 2.0, or 2.1).

[0087] In some embodiments, the texture thickness of the second transparent conductive oxide layer is 75-80 nm (eg, 75 nm, 77 nm, 80 nm), and the refractive index of the second transparent conductive oxide layer is 1.8-2.1 (eg, 1.8, 1.9, 1.97, 2.0, or 2.1).

[0088] In some embodiments, the first electrode and the second electrode respectively and independently include one or more of Au, Ag, Al, and Cu. The thickness of the first electrode and the second electrode respectively and independently may be 100-200 nm (eg, 100 nm, 150 nm, or 200 nm).

[0089] In some embodiments, the P-side gate lines and the N-side gate lines are used to form the second electrode and the first electrode, respectively, and the density of the P-side gate lines is greater than that of the N-side gate lines.

[0090] It should be noted that the crystallinity in this application can be tested using a Raman spectrometer with an incident light wavelength of 632.8 nm. For a film with amorphous, crystalline and small grains, its Raman spectrum will be at 480 cm after Lorentzian decomposition. -1 、510cm -1 and 520cm -1 Characteristic peaks appear at the three peaks corresponding to amorphous, small grains and crystals. From this, we can deduce the crystallization rate ( X c ) is calculated as: X c =( I 510 + I 520 ) / (I 480 + I 510 + I 520 );in, I 480 , I 510 and I 520 They represent the Raman spectrum at 480cm -1 、510cm -1 and 520cm -1 The relative integrated intensity of the peak at .

[0091] The present application provides a method for preparing a silicon-based heterojunction solar cell, comprising:

[0092] Step S110: providing a silicon substrate 100, wherein the silicon substrate 100 comprises a front side and a back side which are opposite to each other.

[0093] In step S110, velvet pyramids may be formed on the surface of the silicon substrate 100. The specific steps of forming the velvet pyramids on the surface of the silicon substrate 100 may include: cleaning and removing damage and texturing the silicon substrate 100 to form a pyramid structure of uniform size on the surface of the silicon substrate 100, then removing organic matter and metal ions on the surface by an RCA (Radio CorPoration of America) cleaning process, then rounding the pyramid structure by a rounding process, and finally removing the oxide layer by a hydrofluoric acid solution to form the velvet pyramids.

[0094] The velvet pyramids formed on the surface of the silicon substrate 100 are uneven structures of uniform size, and are similar to pyramids in microscopic morphology. When incident light enters the surface of the silicon substrate 100 from different angles, the velvet pyramids can increase the absorption of light, thereby improving the short-circuit current and conversion efficiency of the battery.

[0095] Step S120 : sequentially forming a first sub-passivation layer 211 , a carbon-doped amorphous silicon layer 212 and a second sub-passivation layer 213 on the front surface of the silicon substrate 100 ; wherein the first sub-passivation layer 211 , the carbon-doped amorphous silicon layer 212 and the second sub-passivation layer 213 together constitute the first passivation layer 210 .

[0096] In step S120, a first sub-passivation layer 211 can be formed on the front side of the substrate by using a chemical vapor deposition method (e.g., plasma chemical vapor deposition (PECVD) method); a carbon-doped amorphous silicon layer 212 can be formed by introducing methane gas based on an amorphous silicon process; and a second sub-passivation layer 213 can be formed on the surface of the carbon-doped amorphous silicon layer 212 by using a low-pressure chemical vapor deposition method.

[0097] In some embodiments, a carbon-oxygen co-doping method is used to form a first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212, and a second sub-passivation layer 213 stacked in sequence, wherein the carbon-doped amorphous silicon layer 212 is beneficial for optimizing the conductivity of the film layer, and can make the N-type doped layer 220 take into account both optical and electrical properties.

[0098] Step S130 : forming an N-type doping layer 220 on the second sub-passivation layer 213 .

[0099] In step S130, a chemical vapor deposition method (such as plasma chemical vapor deposition (PECVD) method) can be used to form an N-type doped layer 220 on the second sub-passivation layer 213 using hydrogen, silane, phosphine and carbon dioxide gases, wherein the doping material is an N-type semiconductor material, and the N-type semiconductor material includes phosphorus and may also include other elements (such as arsenic and antimony).

[0100] In some embodiments, the specific steps of forming the N-type doped layer 220 on the second sub-passivation layer 213 in step S130 include: by adjusting the amount of hydrogen, silane, phosphine and carbon dioxide gas, a first oxygen-containing seed layer 221, a second oxygen-containing seed layer 222, an N-type doped main layer 223, and an N-type doped contact layer 224 are sequentially formed on the second sub-passivation layer 213; wherein the first oxygen-containing seed layer 221, the second oxygen-containing seed layer 222, the N-type doped main layer 223, and the N-type doped contact layer 224 together constitute the N-type doped layer 220.

[0101] Step S140 : forming a first transparent conductive oxide layer 230 on the N-type doping layer 220 .

[0102] In step S140 , VTTO may be deposited on the N-type doping layer 220 by vacuum evaporation deposition (PVD) or vacuum ion deposition (RPD) to form the first transparent conductive oxide layer 230 .

[0103] Step S150 : forming a first electrode 240 on the first transparent conductive oxide layer 230 .

[0104] In step S150 , the first electrode 240 may be formed on the first transparent conductive oxide layer 230 by screen printing or electroplating.

[0105] In an optional embodiment, after providing the silicon substrate 100 and before forming the first sub-passivation layer 211, the method for preparing a silicon-based heterojunction solar cell further includes:

[0106] Step S160: firstly adopting a hot water slow pulling process and then adopting a plasma etching process to form a pre-passivation layer 250 on the front surface of the silicon substrate 100;

[0107] The material of the pre-passivation layer 250 includes silicon oxide.

[0108] In step S160, the specific steps of first using a hot water slow pull process and then using a plasma etching process to form a pre-passivation layer 250 on the front surface of the silicon substrate 100 include:

[0109] Step S161: using a hot water slow pull process to form a silicon oxide protective layer on the front and back sides of the silicon substrate 100;

[0110] Step S162: using a first plasma etching process to remove the silicon oxide protective layer on the back side of the silicon substrate 100;

[0111] Step S163 : using a second plasma etching process to process the silicon oxide protection layer on the front side of the silicon substrate 100 , remove physically adsorbed impurities, and form the silicon oxide protection layer on the front side of the silicon substrate 100 into a pre-passivation layer 250 .

[0112] The hot water slow pulling process can make the silicon oxide material uniformly deposited on the surface of the silicon substrate 100, which is conducive to forming a silicon oxide protective layer with uniform thickness and good performance, and can make the silicon oxide protective layer completely cover the silicon substrate 100 when it has a lower thickness, thereby optimizing the passivation performance. Since the silicon oxide protective layer will not affect the transmission of electrons, but will block the transmission of holes, the first plasma etching process is used to remove the silicon oxide protective layer on the back of the silicon substrate 100, and only the silicon oxide protective layer on the front of the silicon substrate 100 is retained, which can avoid affecting the transmission of holes on the back of the substrate. The second plasma etching process is used to remove the physically adsorbed impurities on the surface of the silicon oxide protective layer on the front of the substrate, and at the same time remove the weak bonds in the silicon oxide layer, so that the impurity content in the final pre-passivation layer 250 is less, thereby further improving the passivation effect.

[0113] In step S162, the first plasma etching process may be a hydrogen plasma etching process, the RF power may be 380-430 W, and the etching time may be 8-12 s. For example, the RF power may be 380 W, 400 W, 420 W, or 430 W, and the etching time may be 8 s, 10 s, or 12 s.

[0114] In step S163, the second plasma etching process may be a hydrogen plasma etching process, the RF power may be 320-380 W, and the etching time may be 3-7 s. The RF power may be 320 W, 350 W, 360 W, or 380 W, and the etching time may be 3 s, 5 s, or 7 s.

[0115] In an optional embodiment, the method for preparing a silicon-based heterojunction solar cell further includes:

[0116] Step S210 : forming a second passivation layer 310 on the back side of the silicon substrate 100 .

[0117] In step S210, a third intrinsic amorphous silicon layer 311, a fourth intrinsic amorphous silicon layer 312, and a fifth intrinsic amorphous silicon layer 313 can be formed in sequence on the back side of the silicon substrate 100 by chemical vapor deposition; wherein the density of the third intrinsic amorphous silicon layer 311 is less than the density of the fourth intrinsic amorphous silicon layer 312, and the density of the fourth intrinsic amorphous silicon layer 312 is less than the density of the fifth intrinsic amorphous silicon layer 313.

[0118] Step S220: forming a P-type doped seed layer 321 , a P-type doped main layer 322 and a P-type doped contact layer 323 in sequence on the second passivation layer 310 ; wherein the P-type doped seed layer 321 , the P-type doped main layer 322 and the P-type doped contact layer 323 together constitute the P-type doped layer 320 .

[0119] Step S230 : forming a second transparent conductive oxide layer 330 on the P-type doped contact layer 323 .

[0120] Step S240 : forming a second electrode 340 on the second transparent conductive oxide layer 330 .

[0121] In an optional embodiment, a method for preparing a silicon-based heterojunction solar cell comprises:

[0122] Step S310: providing a silicon substrate 100, wherein the silicon substrate 100 includes a front side and a back side that are oppositely arranged;

[0123] Step S320: forming a pre-passivation layer 250 on the front side of the silicon substrate 100; wherein the material of the pre-passivation layer 250 includes silicon oxide; the pre-passivation layer 250 is formed by successively adopting a hot water slow pull process and a plasma etching process;

[0124] Step S330: sequentially forming a first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212 and a second sub-passivation layer 213 on the pre-passivation layer 250; wherein the first sub-passivation layer 211, the carbon-doped amorphous silicon layer 212 and the second sub-passivation layer 213 together constitute the first passivation layer 210;

[0125] Step S340: forming a third intrinsic amorphous silicon layer 311, a fourth intrinsic amorphous silicon layer 312, and a fifth intrinsic amorphous silicon layer 313 in sequence on the back side of the silicon substrate 100; wherein the third intrinsic amorphous silicon layer 311, the fourth intrinsic amorphous silicon layer 312, and the fifth intrinsic amorphous silicon layer 313 together constitute a second passivation layer 310;

[0126] Step S350: forming a first oxygen-containing seed layer 221, a second oxygen-containing seed layer 222, an N-type doped main layer 223, and an N-type doped contact layer 224 in sequence on the second sub-passivation layer 213; wherein the first oxygen-containing seed layer 221, the second oxygen-containing seed layer 222, the N-type doped main layer 223, and the N-type doped contact layer 224 together constitute an N-type doped layer 220;

[0127] Step S360: forming a P-type doped seed layer 321, a P-type doped main layer 322 and a P-type doped contact layer 323 in sequence on the second passivation layer 310; wherein the P-type doped seed layer 321, the P-type doped main layer 322 and the P-type doped contact layer 323 together constitute the P-type doped layer 320;

[0128] Step S370: forming a first transparent conductive oxide layer 230 on the N-type doped layer 220 , and forming a second transparent conductive oxide layer 330 on the P-type doped contact layer 323 ;

[0129] Step S380 : forming the first electrode 240 on the first transparent conductive oxide layer 230 , and forming the second electrode 340 on the second transparent conductive oxide layer 330 .

[0130] The following specific examples further illustrate the present application, but should not be construed as limiting the present application. Without departing from the spirit and substance of the present application, modifications or replacements made to the methods, steps or conditions of the present application are within the scope of the present application.

[0131] Example 1

[0132] like Figure 1 As shown, a specific structure of a silicon-based heterojunction solar cell includes:

[0133] A silicon substrate 100, the silicon substrate 100 comprises a front side and a back side which are arranged opposite to each other; the silicon substrate 100 is an N-type single crystal silicon substrate;

[0134] A first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212, a second sub-passivation layer 213, an N-type doped layer 220, a first transparent conductive oxide layer 230, and a first electrode 240 are sequentially stacked on the front side of the silicon substrate 100 and along the first direction D1; wherein the first sub-passivation layer 211, the carbon-doped amorphous silicon layer 212, and the second sub-passivation layer 213 together constitute the first passivation layer 210; wherein the first sub-passivation layer 211 is a first intrinsic amorphous silicon layer, and the second sub-passivation layer 213 is a second intrinsic amorphous silicon layer;

[0135] A second passivation layer 310, a P-type doping layer 320, a second transparent conductive oxide layer 330, and a second electrode 340 are sequentially stacked on the back side of the silicon substrate 100 and along the second direction D2;

[0136] The second direction D2 is opposite to the first direction D1.

[0137] A method for preparing a silicon-based heterojunction solar cell is as follows:

[0138] Step S410: providing a silicon substrate 100, wherein the silicon substrate 100 includes a front side and a back side that are oppositely arranged;

[0139] The silicon substrate 100 is cleaned, damaged and textured to form a pyramid structure of uniform size on the surface of the silicon substrate 100, and then the organic matter and metal ions on the surface are removed by the RCA cleaning process, and then the pyramid structure is rounded by the rounding process (spherical process), and finally the oxidation layer is removed by a hydrofluoric acid solution to form a velvet pyramid on the surface of the silicon substrate 100;

[0140] Step S420: using PECVD equipment to form a first sub-passivation layer 211 on the front side of the silicon substrate 100 with hydrogen and silane; continuing to use the PECVD equipment, and increasing the hydrogen / silane ratio, while introducing methane gas, to form a carbon-doped amorphous silicon layer 212 on the first sub-passivation layer 211; continuing to use the PECVD equipment, further increasing the hydrogen / silane ratio, while stopping the introduction of methane gas, to form a second sub-passivation layer 213 on the carbon-doped amorphous silicon layer 212; wherein the first sub-passivation layer 211, the carbon-doped amorphous silicon layer 212 and the second sub-passivation layer 213 together constitute the first passivation layer 210;

[0141] The first sub-passivation layer 211 has a structure factor of 0.6 and a thickness of 0.8 nm.

[0142] The carbon-doped amorphous silicon layer 212 has a structure factor of 0.45, a carbon content of 4.4 at%, and a thickness of 0.8 nm;

[0143] The second sub-passivation layer 213 has a structure factor of 0.3 and a thickness of 5 nm;

[0144] Step S430: using PECVD method to form a second passivation layer 310 with a thickness of 12 nm on the back side of the silicon substrate 100 using hydrogen and silane;

[0145] Step S440: using PECVD equipment to form an N-type doping layer 220 on the first sub-passivation layer 211 with hydrogen, silane, phosphine and carbon dioxide gases;

[0146] The N-type doping layer 220 has a silicon-oxygen ratio of 0.8, a phosphorus-silicon ratio of 0.7, a crystallinity of 40%, and a thickness of 28 nm.

[0147] Step S450 : using PECVD equipment to form a P-type doping layer 320 with a thickness of 32 nm on the second passivation layer 310 using hydrogen, silane and borane.

[0148] Step S460: using a PVD method to deposit VTTO on the N-type doped layer 220 to form a first transparent conductive oxide layer 230;

[0149] Using a PVD method, VTTO is deposited on the P-type doped layer 320 to form a second transparent conductive oxide layer 330;

[0150] The first transparent conductive oxide layer 230 has a suede thickness of 68 nm and a refractive index of 1.97.

[0151] The second transparent conductive oxide layer 330 has a suede thickness of 75 nm and a refractive index of 1.97;

[0152] Step S470: using screen printing to form main fine grid lines on the first transparent conductive oxide layer 230, and performing curing and light injection on the grid lines to form the first electrode 240;

[0153] A screen printing method is used to form a main fine grid line on the second transparent conductive oxide layer 330 , and the grid line is cured and light is injected to form the second electrode 340 .

[0154] Example 2

[0155] The silicon-based heterojunction solar cell of Example 2 was prepared by referring to the preparation method of Example 1, except that, in Example 2,

[0156] The structure factor of the first subpassivation layer is 0.65 and the thickness is 1 nm;

[0157] The structure factor of the carbon-doped amorphous silicon layer is 0.58, the carbon content is 4at%, and the thickness is 1nm;

[0158] The second sub-passivation layer has a structure factor of 0.43 and a thickness of 5 nm.

[0159] Example 3

[0160] The silicon-based heterojunction solar cell of Example 3 was prepared by referring to the preparation method of Example 1, except that, in Example 3,

[0161] The first sub-passivation layer has a structure factor of 0.75 and a thickness of 0.8 nm, and is a first oxygen-doped amorphous silicon layer with a silicon-oxygen ratio of 0.6;

[0162] The carbon-doped amorphous silicon layer has a structure factor of 0.5, a carbon content of 4.2 at%, and a thickness of 0.8 nm;

[0163] The second sub-passivation layer has a structural factor of 0.3 and a thickness of 4.8 nm. The second sub-passivation layer is a second intrinsic amorphous silicon layer.

[0164] Step S420 in Example 3 is: using PECVD equipment to form a first sub-passivation layer on the front side of the silicon substrate using hydrogen, silane and carbon dioxide; continuing to use the PECVD equipment, and increasing the hydrogen / silane ratio, introducing methane gas, and stopping the introduction of carbon dioxide gas, to form a carbon-doped amorphous silicon layer on the first sub-passivation layer; continuing to use the PECVD equipment, further increasing the hydrogen / silane ratio, and stopping the introduction of methane gas, to form a second sub-passivation layer on the carbon-doped amorphous silicon layer; wherein the first sub-passivation layer, the carbon-doped amorphous silicon layer and the second sub-passivation layer together constitute the first passivation layer.

[0165] Example 4

[0166] The silicon-based heterojunction solar cell of Example 4 was prepared by referring to the preparation method of Example 1, except that, in Example 4,

[0167] The structure factor of the first sub-passivation layer is 0.7, the thickness is 1 nm, and the first sub-passivation layer is a first intrinsic amorphous silicon layer;

[0168] The structure factor of the carbon-doped amorphous silicon layer is 0.55, the carbon content is 3at%, and the thickness is 1nm;

[0169] The second sub-passivation layer has a structural factor of 0.35 and a thickness of 6 nm. The second sub-passivation layer is a second oxygen-doped amorphous silicon layer with a silicon-oxygen ratio of 0.8.

[0170] Step S420 in Example 4 is: using PECVD equipment to form a first sub-passivation layer on the front side of the silicon substrate with hydrogen and silane; continuing to use the PECVD equipment and increasing the hydrogen / silane ratio, while introducing methane gas to form a carbon-doped amorphous silicon layer on the first sub-passivation layer; continuing to use the PECVD equipment, further increasing the hydrogen / silane ratio, introducing carbon dioxide gas, while stopping the introduction of methane gas, to form a second sub-passivation layer on the carbon-doped amorphous silicon layer; wherein the first sub-passivation layer, the carbon-doped amorphous silicon layer and the second sub-passivation layer together constitute the first passivation layer.

[0171] Example 5

[0172] The silicon-based heterojunction solar cell of Example 5 is similar to the silicon-based heterojunction solar cell of Example 1, except that, in Example 5, a pre-passivation layer 250 is provided between the silicon substrate 100 and the first sub-passivation layer 211. Figure 2 shown.

[0173] The silicon-based heterojunction solar cell of Example 5 is prepared by referring to the preparation method of Example 1, except that, in Example 5, between step S410 and step S420, the following steps are included: step S480: forming a pre-passivation layer 250 on the front surface of the silicon substrate 100;

[0174] In step S420 of embodiment 5: using PECVD equipment, hydrogen and silane are used to form a first sub-passivation layer 211 on the pre-passivation layer 250;

[0175] Wherein, step S480: forming a pre-passivation layer 250 on the front surface of the silicon substrate 100 comprises:

[0176] Step S481: using a hot water slow pull process to form a silicon oxide protective layer on the front and back sides of the silicon substrate 100;

[0177] Step S482: using a first plasma etching process to remove the silicon oxide protective layer on the back side of the silicon substrate 100; the first plasma etching process is a hydrogen plasma etching process, the radio frequency power is 400 W, and the etching time is 10 s;

[0178] Step S483: Use a second plasma etching process to process the silicon oxide protective layer on the front side of the silicon substrate 100 to remove physically adsorbed impurities, so that the silicon oxide protective layer on the front side of the silicon substrate 100 is formed into a pre-passivation layer 250; the second plasma etching process is a hydrogen plasma etching process, the RF power is 350W, and the etching time is 5s.

[0179] Example 6

[0180] like Figure 3 As shown, a specific structure of a silicon-based heterojunction solar cell includes:

[0181] A silicon substrate 100, the silicon substrate 100 comprises a front side and a back side which are arranged opposite to each other; the silicon substrate 100 is an N-type single crystal silicon substrate;

[0182] A first sub-passivation layer 211, a carbon-doped amorphous silicon layer 212, a second sub-passivation layer 213, a first oxygen-containing seed layer 221, a second oxygen-containing seed layer 222, an N-type doped main layer 223, an N-type doped contact layer 224, a first transparent conductive oxide layer 230, and a first electrode 240 are sequentially stacked on the front side of the silicon substrate 100 and along the first direction D1; wherein the first sub-passivation layer 211, the carbon-doped amorphous silicon layer 212 and the second sub-passivation layer 213 together constitute the first passivation layer 210; the first oxygen-containing seed layer 221, the second oxygen-containing seed layer 222, the N-type doped main layer 223 and the N-type doped contact layer 224 together constitute the N-type doped layer 220; wherein the first sub-passivation layer 211 is a first intrinsic amorphous silicon layer, and the second sub-passivation layer 213 is a second intrinsic amorphous silicon layer;

[0183] A third intrinsic amorphous silicon layer 311, a fourth intrinsic amorphous silicon layer 312, a fifth intrinsic amorphous silicon layer 313, a P-type doped seed layer 321, a P-type doped main layer 322, a P-type doped contact layer 323, a second transparent conductive oxide layer 330, and a second electrode 340 are sequentially stacked on the back side of the silicon substrate 100 and along the second direction D2; wherein the third intrinsic amorphous silicon layer 311, the fourth intrinsic amorphous silicon layer 312, and the fifth intrinsic amorphous silicon layer 313 together constitute the second passivation layer 310; the P-type doped seed layer 321, the P-type doped main layer 322, and the P-type doped contact layer 323 together constitute the P-type doped layer 320;

[0184] The second direction D2 is opposite to the first direction D1.

[0185] A method for preparing a silicon-based heterojunction solar cell is as follows:

[0186] Step S510: providing a silicon substrate 100, wherein the silicon substrate 100 includes a front side and a back side that are oppositely arranged;

[0187] The silicon substrate 100 is cleaned, damaged and textured to form a pyramid structure of uniform size on the surface of the silicon substrate 100, and then the organic matter and metal ions on the surface are removed by the RCA cleaning process, and then the pyramid structure is rounded by the rounding process (spherical process), and finally the oxidation layer is removed by a hydrofluoric acid solution to form a velvet pyramid on the surface of the silicon substrate 100;

[0188] Step S520: using PECVD to form a first sub-passivation layer 211 on the front side of the silicon substrate 100 with hydrogen and silane; continuing to use PECVD and increasing the hydrogen / silane ratio, while introducing methane gas, to form a carbon-doped amorphous silicon layer 212 on the first sub-passivation layer 211; continuing to use PECVD to further increase the hydrogen / silane ratio, while stopping the introduction of methane gas, to form a second sub-passivation layer 213 on the carbon-doped amorphous silicon layer 212; wherein the first sub-passivation layer 211, the carbon-doped amorphous silicon layer 212 and the second sub-passivation layer 213 together constitute the first passivation layer 210;

[0189] The first sub-passivation layer 211 has a structure factor of 0.6 and a thickness of 0.8 nm.

[0190] The carbon-doped amorphous silicon layer 212 has a structure factor of 0.5, a carbon content of 4.4 at %, and a thickness of 0.8 nm;

[0191] The second sub-passivation layer 213 has a structure factor of 0.3 and a thickness of 5 nm;

[0192] Step S530: using a PECVD method, continuously adjusting the ratio of hydrogen to silane, so that hydrogen and silane sequentially form a third intrinsic amorphous silicon layer 311, a fourth intrinsic amorphous silicon layer 312, and a fifth intrinsic amorphous silicon layer 313 on the back side of the silicon substrate 100; wherein the third intrinsic amorphous silicon layer 311, the fourth intrinsic amorphous silicon layer 312, and the fifth intrinsic amorphous silicon layer 313 together constitute a second passivation layer 310;

[0193] The third intrinsic amorphous silicon layer 311 has a structure factor of 0.6 and a thickness of 1 nm.

[0194] The fourth intrinsic amorphous silicon layer 312 has a structure factor of 0.5 and a thickness of 1.5 nm;

[0195] The fifth intrinsic amorphous silicon layer 313 has a structure factor of 0.3 and a thickness of 6 nm;

[0196] Step S540: using PECVD equipment, by adjusting the amount of hydrogen, silane, phosphine and carbon dioxide gas, hydrogen, silane, phosphine and carbon dioxide gas are used to sequentially form a first oxygen-containing seed layer 221, a second oxygen-containing seed layer 222, an N-type doped main layer 223, and an N-type doped contact layer 224 on the second sub-passivation layer 213; wherein the first oxygen-containing seed layer 221, the second oxygen-containing seed layer 222, the N-type doped main layer 223, and the N-type doped contact layer 224 together constitute the N-type doped layer 220;

[0197] The first oxygen-containing seed layer 221 has a silicon-oxygen ratio of 0.1, a phosphorus-silicon ratio of 0.015, a crystallization rate of 65%, and a thickness of 0.8 nm.

[0198] The second oxygen-containing seed layer 222 has a silicon-oxygen ratio of 0.5, a phosphorus-silicon ratio of 0.2, a crystallization rate of 60%, and a thickness of 0.8 nm;

[0199] The N-type doped main layer 223 has a silicon-oxygen ratio of 0.8, a phosphorus-silicon ratio of 0.7, a crystallinity of 40%, and a thickness of 18 nm;

[0200] The N-type doped contact layer 224 has a phosphorus-to-silicon ratio of 0.8, a crystallinity of 40%, and a thickness of 2 nm;

[0201] Step S550: using a PECVD device, by adjusting the amount of hydrogen, silane and borane gases, the hydrogen, silane and borane gases sequentially form a P-type doped seed layer 321, a P-type doped main layer 322 and a P-type doped contact layer 323 on the second passivation layer 310; wherein the P-type doped seed layer 321, the P-type doped main layer 322 and the P-type doped contact layer 323 together constitute the P-type doped layer 320;

[0202] The boron-silicon ratio of the P-type doped seed layer 321 is 0.02, the crystallization rate is 65%, and the thickness is 1.5 nm;

[0203] The boron-silicon ratio of the P-type doped body layer 322 is 0.06, the crystallinity is 55%, and the thickness is 25 nm;

[0204] The boron-silicon ratio of the P-type doped contact layer 323 is 0.15, the crystallinity is 35%, and the thickness is 3 nm;

[0205] Step S560: using a PVD method to deposit VTTO on the N-type doped layer 220 to form a first transparent conductive oxide layer 230;

[0206] Using a PVD method, VTTO is deposited on the P-type doped layer 320 to form a second transparent conductive oxide layer 330;

[0207] The first transparent conductive oxide layer 230 has a suede thickness of 68 nm and a refractive index of 1.97.

[0208] The second transparent conductive oxide layer 330 has a suede thickness of 77 nm and a refractive index of 1.97;

[0209] Step S570: using screen printing to form main fine gate lines on the first transparent conductive oxide layer 230, and performing curing and light injection on the gate lines to form the first electrode 240;

[0210] A screen printing method is used to form a main fine grid line on the second transparent conductive oxide layer 330 , and the grid line is cured and light is injected to form the second electrode 340 .

[0211] Example 7

[0212] The silicon-based heterojunction solar cell of Example 7 was prepared by referring to the preparation method of Example 6, except that, in Example 7,

[0213] The structure factor of the first subpassivation layer is 0.65 and the thickness is 1 nm;

[0214] The structure factor of the carbon-doped amorphous silicon layer is 0.55, the carbon content is 4.2at%, and the thickness is 1nm;

[0215] The structure factor of the second sub-passivation layer is 0.38 and the thickness is 7 nm.

[0216] The third intrinsic amorphous silicon layer has a structure factor of 0.55 and a thickness of 1 nm;

[0217] The fourth intrinsic amorphous silicon layer has a structure factor of 0.45 and a thickness of 2 nm;

[0218] The fifth intrinsic amorphous silicon layer has a structure factor of 0.3 and a thickness of 6.5 nm;

[0219] The first oxygen-containing seed layer has a silicon-oxygen ratio of 0.2, a phosphorus-silicon ratio of 0.02, a crystallinity of 65%, and a thickness of 0.6 nm;

[0220] The second oxygen-containing seed layer has a silicon-oxygen ratio of 0.5, a phosphorus-silicon ratio of 0.15, a crystallization rate of 55%, and a thickness of 0.8 nm;

[0221] The N-type doped main layer has a silicon-oxygen ratio of 0.85, a phosphorus-silicon ratio of 0.75, a crystallinity of 35%, and a thickness of 15 nm;

[0222] The N-type doped contact layer has a phosphorus-to-silicon ratio of 0.8, a crystallinity of 30%, and a thickness of 2.5 nm;

[0223] The boron-silicon ratio of the P-type doped seed layer is 0.02, the crystallization rate is 65%, and the thickness is 1.5nm;

[0224] The boron-silicon ratio of the P-type doped main layer is 0.08, the crystallization rate is 55%, and the thickness is 26nm;

[0225] The boron-silicon ratio of the P-type doped contact layer is 0.15, the crystallization rate is 40%, and the thickness is 2nm.

[0226] Example 8

[0227] The silicon-based heterojunction solar cell of Example 8 was prepared by referring to the preparation method of Example 6, except that, in Example 8,

[0228] The first subpassivation layer has a structure factor of 0.6 and a thickness of 1 nm;

[0229] The carbon-doped amorphous silicon layer has a structure factor of 0.45, a carbon content of 4 at%, and a thickness of 1 nm;

[0230] The second sub-passivation layer has a structure factor of 0.35 and a thickness of 6 nm.

[0231] The third intrinsic amorphous silicon layer has a structure factor of 0.5 and a thickness of 1.5 nm;

[0232] The fourth intrinsic amorphous silicon layer has a structure factor of 0.4 and a thickness of 1.5 nm;

[0233] The fifth intrinsic amorphous silicon layer has a structure factor of 0.25 and a thickness of 7 nm;

[0234] The first oxygen-containing seed layer has a silicon-oxygen ratio of 0.2, a phosphorus-silicon ratio of 0.025, a crystallization rate of 60%, and a thickness of 1 nm;

[0235] The second oxygen-containing seed layer has a silicon-oxygen ratio of 0.45, a phosphorus-silicon ratio of 0.25, a crystallization rate of 51%, and a thickness of 1 nm;

[0236] The N-type doped main layer has a silicon-oxygen ratio of 0.7, a phosphorus-silicon ratio of 0.65, a crystallinity of 40%, and a thickness of 12nm;

[0237] The N-type doped contact layer has a phosphorus-silicon ratio of 0.75, a crystallinity of 35%, and a thickness of 3nm;

[0238] The boron-silicon ratio of the P-type doped seed layer is 0.03, the crystallization rate is 60%, and the thickness is 2nm;

[0239] The boron-silicon ratio of the P-type doped main layer is 0.10, the crystallization rate is 50%, and the thickness is 23nm;

[0240] The boron-silicon ratio of the P-type doped contact layer is 0.2, the crystallization rate is 40%, and the thickness is 2nm.

[0241] Example 9

[0242] The silicon-based heterojunction solar cell of Example 9 was prepared by referring to the preparation method of Example 6, except that, in Example 9,

[0243] The first sub-passivation layer has a structure factor of 0.7 and a thickness of 0.8 nm, and is a first oxygen-doped amorphous silicon layer with a silicon-oxygen ratio of 0.85;

[0244] The carbon-doped amorphous silicon layer has a structure factor of 0.5, a carbon content of 4.3 at%, and a thickness of 0.8 nm;

[0245] The second sub-passivation layer has a structural factor of 0.4 and a thickness of 5 nm. The second sub-passivation layer is a second intrinsic amorphous silicon layer.

[0246] The third intrinsic amorphous silicon layer has a structure factor of 0.65 and a thickness of 1.5 nm;

[0247] The fourth intrinsic amorphous silicon layer has a structure factor of 0.5 and a thickness of 1.5 nm;

[0248] The fifth intrinsic amorphous silicon layer has a structure factor of 0.35 and a thickness of 5.5 nm;

[0249] The first oxygen-containing seed layer has a silicon-oxygen ratio of 0.15, a phosphorus-silicon ratio of 0.03, a crystallization rate of 60%, and a thickness of 1 nm;

[0250] The second oxygen-containing seed layer has a silicon-oxygen ratio of 0.45, a phosphorus-silicon ratio of 0.1, a crystallization rate of 55%, and a thickness of 1 nm;

[0251] The N-type doped main layer has a silicon-oxygen ratio of 0.75, a phosphorus-silicon ratio of 0.75, a crystallinity of 45%, and a thickness of 15 nm;

[0252] The N-type doped contact layer has a phosphorus-to-silicon ratio of 0.85, a crystallinity of 35%, and a thickness of 2nm;

[0253] The boron-silicon ratio of the P-type doped seed layer is 0.03, the crystallization rate is 60%, and the thickness is 2nm;

[0254] The boron-silicon ratio of the P-type doped main layer is 0.08, the crystallization rate is 55%, and the thickness is 26nm;

[0255] The boron-silicon ratio of the P-type doped contact layer is 0.2, the crystallization rate is 35%, and the thickness is 3nm.

[0256] In step S520 of Example 9: using PECVD equipment to form a first sub-passivation layer on the front side of the silicon substrate with hydrogen, silane and carbon dioxide; continuing to use the PECVD equipment, and increasing the hydrogen / silane ratio, introducing methane gas, and stopping the introduction of carbon dioxide gas, to form a carbon-doped amorphous silicon layer on the first sub-passivation layer; continuing to use the PECVD equipment, further increasing the hydrogen / silane ratio, and stopping the introduction of methane gas, to form a second sub-passivation layer on the carbon-doped amorphous silicon layer; wherein the first sub-passivation layer, the carbon-doped amorphous silicon layer and the second sub-passivation layer together constitute the first passivation layer.

[0257] Example 10

[0258] The silicon-based heterojunction solar cell of Example 10 is similar to the silicon-based heterojunction solar cell of Example 6, except that, in Example 10, a pre-passivation layer 250 is provided between the silicon substrate 100 and the first sub-passivation layer 211. Figure 4 shown.

[0259] The silicon-based heterojunction solar cell of Example 10 is prepared by referring to the preparation method of Example 6, except that, in Example 10, between step S510 and step S520, the following is further included: step S580: forming a pre-passivation layer 250 on the front surface of the silicon substrate 100;

[0260] In step S520 of embodiment 10: using PECVD equipment, hydrogen and silane are used to form a first sub-passivation layer 211 on the pre-passivation layer 250;

[0261] Wherein, step S580: forming a pre-passivation layer 250 on the front surface of the silicon substrate 100 comprises:

[0262] Step S581: using a hot water slow pull process to form a silicon oxide protective layer on the front and back sides of the silicon substrate 100;

[0263] Step S582: using a first plasma etching process to remove the silicon oxide protective layer on the back side of the silicon substrate 100; wherein the first plasma etching process is a hydrogen plasma etching process, the radio frequency power is 400 W, and the etching time is 10 s;

[0264] Step S583: Use a second plasma etching process to process the silicon oxide protective layer on the front side of the silicon substrate 100 to remove physically adsorbed impurities, so that the silicon oxide protective layer on the front side of the silicon substrate 100 is formed into a pre-passivation layer 250; wherein the second plasma etching process is a hydrogen plasma etching process, the RF power is 350 W, and the etching time is 5 s.

[0265] In order to more clearly illustrate the technical effects of the embodiments of the present application, the present application also points out the structure and preparation method of the silicon-based heterojunction solar cell of Comparative Example 1.

[0266] Comparative Example 1

[0267] The silicon-based heterojunction solar cell of Comparative Example 1 is prepared by referring to the preparation method of Example 1, except that step S420 of Comparative Example 1 is: using PECVD method to form an intrinsic amorphous silicon layer on the front surface of the silicon substrate with hydrogen and silane; wherein the intrinsic amorphous silicon layer is the first passivation layer;

[0268] Step S460 of Comparative Example 1 is: using the PVD method to deposit ITO on the N-type doped layer to form a first transparent conductive oxide layer; using the PVD method to deposit ITO on the P-type doped layer to form a second transparent conductive oxide layer.

[0269] Compared with Example 1, the structure of the silicon-based heterojunction solar cell of Comparative Example 1 is different in that an intrinsic amorphous silicon layer, an N-type doped layer, a first transparent conductive oxide layer, and a first electrode are stacked in sequence on the front side of the silicon substrate and along the first direction; wherein the intrinsic amorphous silicon layer is the first passivation layer, and the structure factor of the intrinsic amorphous silicon layer is 0.5 and the thickness is 10 nm.

[0270] In order to conduct stability testing, the above silicon-based heterojunction solar cells were all packaged. The device performance of the silicon-based heterojunction solar cells of Examples 1-10 of the present application and Comparative Example 1 was tested below to obtain the short-circuit current density Jsc, open-circuit voltage Voc, fill factor FF, and photoelectric conversion efficiency PCE of the corresponding battery devices, and the test results are shown in Table 1.

[0271] Table 1

[0272]

[0273] It can be seen from the data in Table 1 that, compared with Comparative Example 1, the open circuit voltage and short-circuit current density of the corresponding battery devices of the silicon-based heterojunction solar cells of Examples 1-10 of the present application are slightly improved, and the fill factor and photoelectric conversion efficiency are significantly improved; this indicates that the first passivation layer in Examples 1-10 of the present application includes a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer stacked in sequence, has a good passivation effect, can reduce the thickness of the first passivation layer, and has a wider energy band, which can improve the short-circuit current and fill factor of the silicon-based heterojunction solar cell, thereby improving the device performance.

[0274] In summary, the first passivation layer of the embodiment of the present application includes a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer stacked in sequence. Among them, the first sub-passivation layer close to the silicon substrate has a good passivation effect, and the second sub-passivation layer far from the silicon substrate is conducive to the formation of subsequent doped layers. The carbon-doped amorphous silicon layer located between the first sub-passivation layer and the second sub-passivation layer is made of silicon carbide (Si x C y , x is not equal to y), which is conducive to optimizing the conductivity of the film layer, reducing the thickness of the first passivation layer, and avoiding problems such as increased resistance and reduced fill factor caused by an excessively thick intrinsic amorphous silicon layer. In addition, the gap between the valence band and the conduction band of silicon carbide is relatively wide, at 2.8-4.2eV, which can increase the short-circuit current and fill factor of silicon-based heterojunction solar cells, thereby improving device performance.

[0275] It should be noted that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.

[0276] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0277] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0278] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0279] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A silicon-based heterojunction solar cell, characterized in that: include: A silicon substrate, the silicon substrate comprising a front side and a back side arranged opposite to each other; A first passivation layer, an N-type doping layer, a first transparent conductive oxide layer, and a first electrode are sequentially stacked on the front side of the silicon substrate and along a first direction; Wherein, the first passivation layer comprises: a first sub-passivation layer, a carbon-doped amorphous silicon layer and a second sub-passivation layer which are sequentially stacked along the first direction; The first sub-passivation layer is a first oxygen-doped amorphous silicon layer, and the silicon-oxygen ratio of the first oxygen-doped amorphous silicon layer is greater than 0.1 and less than 1; The second sub-passivation layer is a second oxygen-doped amorphous silicon layer, and the silicon-oxygen ratio of the second oxygen-doped amorphous silicon layer is greater than 0.1 and less than 1; In the carbon-doped amorphous silicon layer, the carbon content is 0.1-4.4 at %; The structure factor of the first sub-passivation layer is greater than the structure factor of the carbon-doped amorphous silicon layer, and the structure factor of the carbon-doped amorphous silicon layer is greater than the structure factor of the second sub-passivation layer; and the structure factor of the first sub-passivation layer is 0.6-0.75, the structure factor of the carbon-doped amorphous silicon layer is 0.45-0.58, and the structure factor of the second sub-passivation layer is 0.3-0.43; The N-type doped layer comprises: a first oxygen-containing seed layer, a second oxygen-containing seed layer, an N-type doped main layer, and an N-type doped contact layer sequentially stacked along the first direction; The silicon-oxygen ratios of the first oxygen-containing seed layer, the second oxygen-containing seed layer, and the N-type doped main layer increase in sequence; The phosphorus-silicon ratios of the first oxygen-containing seed layer, the second oxygen-containing seed layer, the N-type doped main layer, and the N-type doped contact layer are increased in sequence; The carbon-doped amorphous silicon layer is disposed between the first sub-passivation layer and the second sub-passivation layer, which is beneficial for electrons to utilize the defect density of the carbon-doped amorphous silicon to perform energy band hopping, thereby improving the conductivity of the first passivation layer.

2. The silicon-based heterojunction solar cell according to claim 1, characterized in that: The thickness ratio of the first sub-passivation layer, the carbon-doped amorphous silicon layer and the second sub-passivation layer is 1:(1-4):(5-7).

3. The silicon-based heterojunction solar cell according to any one of claims 1 to 2, characterized in that: Also includes: a pre-passivation layer disposed between the silicon substrate and the first passivation layer; Wherein, the material of the pre-passivation layer includes silicon oxide; The pre-passivation layer is formed by successively adopting a hot water slow pulling process and a plasma etching process.

4. The silicon-based heterojunction solar cell according to any one of claims 1 to 2, characterized in that: The silicon-oxygen ratio of the first oxygen-containing seed layer is greater than or equal to 0.05 and less than 0.4, the silicon-oxygen ratio of the second oxygen-containing seed layer is greater than or equal to 0.4 and less than 0.7, and the silicon-oxygen ratio of the N-type doped body layer is greater than or equal to 0.6 and less than 1; and / or The phosphorus-silicon ratio of the first oxygen-containing seed layer is greater than or equal to 0.01 and less than 0.05, the phosphorus-silicon ratio of the second oxygen-containing seed layer is greater than or equal to 0.05 and less than 0.3, the phosphorus-silicon ratio of the N-type doped main layer is greater than or equal to 0.06 and less than 1, and the phosphorus-silicon ratio of the N-type doped contact layer is greater than or equal to 0.06 and less than 1.

5. The silicon-based heterojunction solar cell according to claim 4, characterized in that: The crystallization rate of the first oxygen-containing seed layer is 52%-70%; the crystallization rate of the second oxygen-containing seed layer is 50.5%-68%; the crystallization rate of the N-type doped main layer is greater than 10% and less than 50%, and the crystallization rate of the N-type doped contact layer is greater than 0% and less than 50%; wherein the crystallization rate of the second oxygen-containing seed layer is less than the crystallization rate of the first oxygen-containing seed layer.

6. The silicon-based heterojunction solar cell according to any one of claims 1 to 2, characterized in that: Also includes: A second passivation layer, a P-type doping layer, a second transparent conductive oxide layer, and a second electrode are sequentially stacked on the back side of the silicon substrate and along a second direction; The P-type doped layer comprises: a P-type doped seed layer, a P-type doped main layer and a P-type doped contact layer which are sequentially stacked along the second direction; The second direction is opposite to the first direction; Wherein, the boron-silicon ratio of the P-type doped seed layer is greater than 0.01 and less than 0.9, the boron-silicon ratio of the P-type doped main layer is greater than 0.04 and less than 0.95, the boron-silicon ratio of the P-type doped contact layer is greater than 0.06 and less than 1, and the boron-silicon ratio of the P-type doped seed layer is less than the boron-silicon ratio of the P-type doped main layer; and / or The crystallization rate of the P-type doped seed layer is greater than 50% and less than 70%, the crystallization rate of the P-type doped main layer is greater than 25% and less than 60%, the crystallization rate of the P-type doped contact layer is greater than 20% and less than 50%, and the crystallization rate of the P-type doped seed layer is greater than the crystallization rate of the P-type doped main layer.

7. The silicon-based heterojunction solar cell according to claim 6, characterized in that: The second passivation layer includes a third intrinsic amorphous silicon layer, a fourth intrinsic amorphous silicon layer, and a fifth intrinsic amorphous silicon layer which are sequentially stacked along the second direction; The structure factor of the third intrinsic amorphous silicon layer is greater than the structure factor of the fourth intrinsic amorphous silicon layer, and the structure factor of the fourth intrinsic amorphous silicon layer is greater than the structure factor of the fifth intrinsic amorphous silicon layer.

8. The silicon-based heterojunction solar cell according to claim 7, characterized in that: The structure factor of the third intrinsic amorphous silicon layer is 0.5-0.7; the structure factor of the fourth intrinsic amorphous silicon layer is 0.4-0.6; and the structure factor of the fifth intrinsic amorphous silicon layer is 0.2-0.

4.

9. A method for preparing a silicon-based heterojunction solar cell according to any one of claims 1 to 8, characterized in that: include: Providing a silicon substrate, wherein the silicon substrate comprises a front side and a back side that are oppositely arranged; Forming a first sub-passivation layer, a carbon-doped amorphous silicon layer, and a second sub-passivation layer in sequence on the front surface of the silicon substrate; wherein the first sub-passivation layer, the carbon-doped amorphous silicon layer, and the second sub-passivation layer together constitute a first passivation layer; forming an N-type doped layer on the second sub-passivation layer; forming a first transparent conductive oxide layer on the N-type doped layer; A first electrode is formed on the first transparent conductive oxide layer.

10. The method for preparing a silicon-based heterojunction solar cell according to claim 9, characterized in that: Before forming the first sub-passivation layer, the method for preparing the silicon-based heterojunction solar cell further includes: Forming a pre-passivation layer on the front side of the silicon substrate by firstly adopting a hot water slow pulling process and then adopting a plasma etching process; Wherein, the material of the pre-passivation layer includes silicon oxide.

11. The method for preparing a silicon-based heterojunction solar cell according to claim 9, characterized in that: Also includes: forming a second passivation layer on the back side of the silicon substrate; forming a P-type doped seed layer, a P-type doped main layer and a P-type doped contact layer in sequence on the second passivation layer; wherein the P-type doped seed layer, the P-type doped main layer and the P-type doped contact layer together constitute a P-type doped layer; forming a second transparent conductive oxide layer on the P-type doped contact layer; A second electrode is formed on the second transparent conductive oxide layer.

Citation Information

Patent Citations

  • Structure of intrinsic passivation layer of silicon heterojunction solar cell and manufacturing method of structure

    CN111628032A

  • Silicon heterojunction solar cell and manufacturing method thereof

    CN112002778A

  • Heterojunction solar cell and preparation method thereof

    CN113113502A

  • Heterojunction solar cell and preparation method thereof

    CN116995111A

  • Silicon-based heterojunction solar cell, preparation method, electric equipment and application

    CN117525196A