Carbon nanotube aqueous phase dispersion method and preparation method of aqueous carbon nanotube composite film slurry
The dispersion process of carbon nanotubes is carried out through the combination of hydrogen peroxide and ammonia water. Ultrasonic and grinding technology, combined with the auxiliary dispersant, the problems of poor dispersion and high energy consumption of carbon nanotubes in the water system are solved, and high efficiency and environmental protection are achieved. Carbon nanotube dispersion and composite film slurry preparation.
Patent Information
- Application Number
- CN202410903149.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing carbon nanotube dispersion process has problems such as high energy consumption, poor generation of polluted wastewater and poor dispersion, especially in the water system, the dispersion effect is poor, and the commonly used organic solvents are highly toxic and not environmentally friendly.
The combination of hydrogen peroxide and ammonia water is used to perform predispersion, ultrasonic dispersion and grinding dispersion of carbon nanotubes. Through shear stirring and oxidation modification, the oxidation degree is regulated by the oxidation properties of hydrogen peroxide and ammonia water, combined with a co-dispersant such as ethanolamine acrylic acid, etc. , realize efficient dispersion of carbon nanotubes in water.
The high purity and conductive properties of carbon nanotubes are maintained, the process energy consumption and wastewater generation are reduced, the dispersion stability and production efficiency are improved, and the process is simple and environmentally friendly.
Smart Images

Figure CN118439597B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a carbon nanotube dispersion process, in particular to a carbon nanotube aqueous phase dispersion method and a method for preparing an aqueous carbon nanotube composite film slurry. Background Art
[0002] Carbon nanotubes are a new type of nanomaterial with many excellent mechanical, thermal and electrical properties. With the continuous deepening of research on carbon nanomaterials, the manufacturing technology of carbon nanotubes has become more mature and stable, and the price of ordinary multi-walled carbon nanotubes has been reduced year by year. Carbon nanotubes are increasingly involved in various advanced material manufacturing industries. However, due to the strong interaction between multiple carbon nanotubes, it is extremely easy to entangle with each other and difficult to untie them. When applied, their high performance advantages cannot be fully utilized. Therefore, how to improve the dispersion performance has become the research focus of carbon nanotubes.
[0003] CN114314566B provides a method for separating and purifying carbon nanotubes by liquid phase oxidation, wherein the carbon nanotubes are first evenly dispersed in a surfactant solution by ultrasonication, the carbon nanotube bundle is opened, and after centrifugal separation, hydrogen peroxide is added and heated to reflux to remove the carbon byproducts that wrap the metal catalyst. Then, after suction filtration and washing, a diluted concentrated acid solution is added, and the mixture is placed in an oil bath and heated to reflux and stirred to remove the residual metal catalyst; the mixture is naturally cooled to room temperature, the pH value is adjusted, and suction filtration is performed. The obtained carbon nanotubes are dried at 120°C for 12 hours to obtain purified carbon nanotubes. This method uses hydrogen peroxide heating and oxidizing acid for oxidation, and a large amount of cleaning wastewater will be generated during the purification process, and the process energy consumption is high.
[0004] CN116462187A provides a batch purification method, which uses one of hydrogen peroxide, ozone or hydroxyl free radicals as an oxidant, and then uses dilute hydrochloric acid to reflux and pickle in batches after oxidation. After the pickling is completed, it is washed in batches with clean water, and the filtrate produced by the M+1th washing of the previous batch is used as the washing liquid for the Mth washing, which further reduces the amount of washing wastewater generated. However, the oxidation time is long and a large amount of acid waste liquid caused by pickling still exists.
[0005] CN114516630B provides a method for improving the dispersibility of carbon nanotubes. Through a series of physical / chemical methods such as pre-oxidation treatment, air flow crushing, high-pressure infiltration, high-speed emulsification dispersion, coarse grinding, and fine grinding, carbon nanotubes are evenly dispersed in a carbon nanotube dispersion, solving the problems of carbon nanotubes being difficult to disperse, easy to agglomerate, and having a low dispersion concentration in the carbon nanotube dispersion. However, the reaction temperature of the pre-oxidation furnace is as high as 500°C, and the dispersion requires pressurized (20MPa) infiltration, which consumes a lot of energy. Moreover, a good dispersion effect can only be achieved in NMP, and it is difficult to disperse well in water.
[0006] In addition, the dispersibility of carbon nanotubes in organic solvents such as THF, NMP, and DMF is better than that in water-alcohol solvents, but these organic solvents are highly toxic and environmentally unfriendly, which is not in line with future development trends. Water-alcohol solvents have poor wettability and dispersibility for carbon nanotubes, so it is necessary to develop a carbon nanotube dispersion method with a simple process, short preparation cycle, high repeatability, and easy to carry out in water-alcohol solvents. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a method for dispersing carbon nanotubes in water, comprising the following steps:
[0008] S1. Pre-dispersion: slowly add carbon nanotubes into hydrogen peroxide solution for purification, and shear and stir for 5-30 minutes; the role of hydrogen peroxide is to remove surface impurities of carbon nanotubes through its own oxidation ability, reduce the effect of impurity adhesion on the dispersion of carbon nanotubes, and ensure the high purity and high conductivity of carbon nanotubes. Hydrogen peroxide can modify some active groups on the surface of carbon nanotubes while purifying, and then preliminarily disperse the carbon nanotubes through shear dispersion process, thereby enhancing the subsequent dispersion effect;
[0009] S2, ultrasonic dispersion: the pre-dispersed slurry is transferred into an ultrasonic container for ultrasonic dispersion, with a cycle time of 0.8-1.4h; ultrasonic dispersion can not only disperse the carbon nanotubes evenly throughout the solvent, reduce the aggregation of carbon nanotubes, and enhance the dispersion stability of carbon nanotubes; at the same time, the ultrasonic process can also make the surface of the carbon nanotubes fully contact with hydrogen peroxide, accelerating the purification of the surface of the carbon nanotubes by hydrogen peroxide;
[0010] S3. Prepare aqueous dispersion slurry: add dispersant and ammonia water to the mixed slurry after ultrasound and stir to disperse, then transfer to grinding equipment, repeatedly disperse for 1-2 hours, and finally obtain an aqueous carbon nanotube dispersion with stable dispersion ability; the role of ammonia water is to regulate the oxidation degree of hydrogen peroxide by reacting with hydrogen peroxide.
[0011] Other inorganic bases may also have the ability to regulate the degree of oxidation of hydrogen peroxide, but other components will inevitably be introduced during the reaction, affecting the conductivity and dispersion of carbon nanotubes.
[0012] Furthermore, the concentration of the hydrogen peroxide solution is 30%, the concentration of the ammonia solution is 25-30%, and the mass ratio of the carbon nanotubes, the hydrogen peroxide solution, and the ammonia solution is (1-5): (90-110): (0.1-3). The hydrogen peroxide solution of the present invention is generally set to be relatively excessive so as to fully exert the oxidation effect.
[0013] Furthermore, the diameter of the carbon nanotubes is 1-20 nm, the length is 5-100 um, and the mass of the added carbon nanotubes accounts for 1-5% of the total amount of the aqueous carbon nanotube dispersion.
[0014] Further, in step S2, the ultrasonic frequency is 20-25 KHz.
[0015] Furthermore, the dispersant is one or more of ethanolamine type acrylic acid, alkyl alcohol amide, and lauryl amide propyl amine oxide, and the mass of the added dispersant accounts for 0.1-1.5% of the total amount of the aqueous carbon nanotube dispersion. Ammonia water itself is suitable as a dispersant for dispersing carbon nanotubes after oxidation with hydrogen peroxide. The surface of the carbon nanotube wall after oxidation is negatively charged. Ammonia water is hydrolyzed and ionized to produce ammonium ions, which are combined with the negatively charged carbon nanotubes through electrostatic attraction, thereby producing a synergistic effect with the amide dispersant to promote the dispersion of carbon nanotubes.
[0016] Furthermore, the shear dispersion of S1, the ultrasonic dispersion of S2, and the stirring and grinding dispersion of S3 are all performed at room temperature. The oxidation of hydrogen peroxide and the reaction of hydrogen peroxide and ammonia water in the present invention require relatively low temperatures and can occur at room temperature without the need for an additional heating process.
[0017] The present invention also provides a method for preparing a carbon nanotube composite film slurry, wherein the aqueous carbon nanotube dispersion prepared by the above-mentioned dispersion process is mixed with an aqueous resin adhesive phase to obtain a carbon nanotube composite film slurry that can be cast and coated; wherein the mass ratio of solid carbon nanotubes to aqueous resin is 1: (0.5-5). The carbon nanotube composite film slurry is coated on a plastic film to obtain a carbon nanotube film with excellent conductive properties.
[0018] Further, the method comprises step S4, adding a defoamer and a thickener into the aqueous carbon nanotube dispersion, and stirring and dispersing the mixture for 10-12 minutes;
[0019] Step S5, adding water-based resin to the slurry treated in S4, and shearing and stirring for 1-1.5 hours to obtain the water-based carbon nanotube composite film slurry.
[0020] Furthermore, in step S4, the defoaming agent is one or more of a polyether defoaming agent, an acetylene alcohol defoaming agent and a polyether-modified silicon defoaming agent.
[0021] Furthermore, in step S4, the thickener is one or more of polyurethane, acrylic acid alkali swelling associative type, and sodium polyacrylate.
[0022] Furthermore, in step S4, the water-based resin material includes: one or more of water-based polyacrylic resin, water-based epoxy resin, water-based polyurethane, water-based polyester resin, and water-based PTFE emulsion.
[0023] The present invention is based on the development of carbon nanotube film and provides a method for dispersing carbon nanotubes without affecting the high performance of carbon nanotubes. The strong oxidizing property of hydrogen peroxide is used to remove the carbon byproducts wrapped with metal catalysts, oxidatively modify the carbon nanotubes, and then the oxidation degree of hydrogen peroxide is regulated by ammonia water. The oxidative modification method proposed by the present invention is simple, efficient, easy to operate, and has universal applicability.
[0024] The reaction requires a relatively low temperature and can be carried out at room temperature. At the same time, the purified suspension of the reaction does not produce any wastewater, and can enter the next dispersion process without subsequent treatment such as drying. The process is energy-saving and environmentally friendly, does not increase the filtering and cleaning process and wastewater discharge, and saves production costs. There is no need to use energy-consuming processes such as centrifugal cleaning, which greatly improves production efficiency and reduces power consumption.
[0025] The present invention adopts high-efficiency composite surfactant formulation technology, utilizes ethanolamine type acrylic acid, alkyl alcohol amide, lauryl amide propyl amine oxide and other small molecular weight nonionic surfactants to electrostatically adsorb on the surface of carbon tubes and play a role of physical barrier; at the same time, the amide functional group can promote the wetting of carbon tubes by water, produce synergistic effect with ammonia water, and promote the dispersion of carbon tubes. The carbon nanotube dispersion process provided by the present invention has little destructiveness to the carbon nanotubes themselves, and can further obtain an aqueous carbon nanotube slurry with uniformly dispersed carbon nanotubes and high aspect ratio. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a microscopic electron microscope scanning image of slurry CN1 prepared in Example 1;
[0027] Figure 2 is a microscopic electron microscope scanning image of slurry CN2 prepared in Example 2;
[0028] Figure 3 is a microscopic electron microscope scanning image of slurry CN3 prepared in Example 3;
[0029] Figure 4 is a microscopic electron microscope scanning image of slurry CN4 prepared in Example 4;
[0030] Figure 5 is a microscopic electron microscope scanning image of slurry CN5 prepared in Comparative Example 1;
[0031] Figure 6 This is an infrared temperature detection diagram of the carbon film material obtained by coating the slurry CNE1. DETAILED DESCRIPTION
[0032] Example 1: A water-based carbon nanotube composite film slurry is prepared according to the following process:
[0033] S1. Add 4.215kg of 30% hydrogen peroxide solution into the dispersion container, slowly add 200g of carbon nanotubes (Shenzhen Nanoport NTP3003) into the hydrogen peroxide solution at room temperature and perform shear dispersion; the diameter of the carbon nanotubes is 7-15nm and the length is 5-15μm. The shear dispersion speed is 3Kr / min, and it lasts for 5-30min, so that the carbon nanotubes are initially dispersed in the hydrogen peroxide solution by high-speed shearing.
[0034] S2. The sheared and dispersed slurry is transferred to an ultrasonic crushing device for ultrasonic dispersion treatment. The ultrasonic crushing power is 2000W and the cycle time is 0.8-1.4h to further improve the dispersion of the carbon nanotubes and catalyze the oxidation effect of hydrogen peroxide on the surface of the carbon nanotubes, thereby improving the purification efficiency of the carbon nanotubes.
[0035] S3. Add 120g of alkyl alcohol amide and 120g of 25-30% ammonia water to the mixed slurry after ultrasound at room temperature and stir and disperse, catalyzing the incompletely oxidized hydrogen peroxide to decompose into water; at the same time, similar to alkyl alcohol amide, ammonia water can also enhance the dispersion effect of carbon nanotubes in the solvent. Then transfer to the grinding equipment for repeated grinding and dispersion for 1-2h, and peel and shear the carbon nanotubes by sand milling to enhance the dispersion ability of the carbon nanotubes, and finally obtain 4kg of water-based carbon nanotube dispersion with good dispersion ability, in which the carbon nanotube content accounts for 5%. The dispersion is recorded as slurry CN1 and a carbon nanotube composite film slurry is prepared based on the dispersion.
[0036] S4. Add 5g of acetylene alcohol defoamer (Tuyile Foamic 021) and 10g of thickener water-based polyurethane (Guangzhou Tianhe District Hongtouchuan New Materials 8w) to 4kg of slurry CN1, mix thoroughly and stir to disperse for 10 minutes.
[0037] S5. Add 572 g of water-based epoxy resin (Shenzhen Jitian Chemical F0707) to the mixed slurry of S4, and perform shearing, stirring and dispersing treatment for 1 hour to obtain the target water-based carbon nanotube composite slurry, which is recorded as slurry CNE1.
[0038] Example 2: S1. Add 4.331 kg of 30% hydrogen peroxide solution into a dispersion container, slowly add 160 g of carbon nanotubes (TG-MAL264 from Wuxi Carbon Valley) into the hydrogen peroxide solution at room temperature and perform shear dispersion; the diameter of the carbon nanotubes is 8-11 nm and the length is 10-30 μm. The shear dispersion speed is 3 Kr / min and lasts for 5-30 min.
[0039] S2. The sheared and dispersed slurry is transferred to an ultrasonic crushing device for ultrasonic dispersion treatment. The ultrasonic crushing power is 2000 W and the cycle time is 0.8-1.4 h.
[0040] S3, add 54g ethanolamine type acrylic resin liquid (Hanhua SHD853), 6g lauramide propyl amine oxide (Xinquansheng LAO-30) and 60g 25-30% ammonia water to the mixed slurry after ultrasound at room temperature and stir and disperse; then transfer to the grinding equipment and grind and disperse repeatedly for 1-2h, and finally obtain 4kg of water-based carbon nanotube dispersion with good dispersibility, in which the carbon nanotube content accounts for 4%. The dispersion is recorded as slurry CN2 and the carbon nanotube composite film slurry is prepared based on the dispersion.
[0041] S4. Add 16g of polyether defoamer (Guangdong Defeng DF-8201) and 8g of acrylic acid alkali swelling thickener (ASE-60) to 4kg of slurry CN2, mix thoroughly and stir to disperse for 10 minutes.
[0042] S5. Add 457 g of water-based acrylic resin (Guangzhou Huigu Chemical WPA4413) to the mixed slurry of S4, and perform shearing, stirring and dispersing treatment for 1 hour to obtain the target water-based carbon nanotube composite slurry, which is recorded as slurry CNE2.
[0043] Example 3: S1. Add 4.556 kg of 30% hydrogen peroxide solution into a dispersion container, slowly add 40 g of carbon nanotubes (TNM0, Chengdu Zhongke Times Nano Energy) into the hydrogen peroxide solution at room temperature and perform shear dispersion; the diameter of the carbon nanotubes is 4-6 nm and the length is 10-20 μm. The shear dispersion speed is 3 Kr / min and lasts for 5-30 min.
[0044] S2. The sheared and dispersed slurry is transferred to an ultrasonic crushing device for ultrasonic dispersion treatment. The ultrasonic crushing power is 2000 W and the cycle time is 0.8-1.4 h.
[0045] S3, add 20g of ethanolamine type acrylic resin liquid (Hanhua SHD853) and 30g of 25-30% ammonia water to the mixed slurry after ultrasound at room temperature and stir and disperse; then transfer to the grinding equipment and grind and disperse repeatedly for 1-2h, and finally obtain 4kg of water-based carbon nanotube dispersion with good dispersibility, in which the carbon nanotube content accounts for 1%. This dispersion is recorded as slurry CN3 and is used as the basis for preparing carbon nanotube composite film slurry.
[0046] S4. Add 10g of acetylene alcohol defoamer (Guangdong Defeng DF-2684) and 8g of sodium polyacrylate (Tonglingda FMN-17) to 4kg of slurry CN3, mix thoroughly and stir to disperse for 10 minutes.
[0047] S5. Add 312 g of aqueous polytetrafluoroethylene dispersion (Kemu DISP30) to the mixed slurry of S4, and perform shearing, stirring and dispersing treatment for 1 hour to obtain the target aqueous carbon nanotube composite slurry, which is recorded as slurry CNE3.
[0048] Example 4: S1. Add 4.436 kg of 30% hydrogen peroxide solution into a dispersion container, slowly add 100 g of carbon nanotubes (Qingdao Haoxin HX-N1) into the hydrogen peroxide solution at room temperature and perform shear dispersion; the diameter of the carbon nanotubes is 8-10 nm and the length is 50-100 μm. The shear dispersion speed is 3 Kr / min and lasts for 5-30 min.
[0049] S2. The sheared and dispersed slurry is transferred to an ultrasonic crushing device for ultrasonic dispersion treatment. The ultrasonic crushing power is 2000 W and the cycle time is 0.8-1.4 h.
[0050] S3. Add 14g alkyl alcohol amide (Shandong Jinmei Chemical 6503), 20g ethanolamine type acrylic resin liquid (Hanhua SHD853), 6g lauramide propyl amine oxide (Xinquansheng LAO-30), 50g 25-30% ammonia water to the mixed slurry after ultrasound at room temperature and stir and disperse; then transfer to the grinding equipment and grind and disperse repeatedly for 1-2h, and finally obtain 4kg of water-based carbon nanotube dispersion with good dispersibility, in which the carbon nanotube content accounts for 2.5%. The dispersion is recorded as slurry CN4 and the carbon nanotube composite film slurry is prepared based on the dispersion.
[0051] S4. Add 10g of acetylene alcohol defoamer (Guangdong Defeng DF-2684) and 8g of sodium polyacrylate (Tonglingda FMN-17) to 4kg of slurry CN4, mix thoroughly and stir to disperse for 10 minutes.
[0052] S5. Add 112 g of waterborne polyurethane (Shenzhen Yoshida Chemical F0402) and 200 g of waterborne polyester (Nittoyobo water-dispersible polyester MD-2000) to the mixed slurry of S4, and perform shear stirring and dispersion treatment for 1 h to obtain the target waterborne carbon nanotube composite slurry, which is recorded as slurry CNE4.
[0053] Comparative Example 1: An aqueous carbon nanotube dispersion was prepared by the same steps S1-S3 as in Example 1, except that the solvent was replaced by deionized water instead of hydrogen peroxide solution. The obtained dispersion was recorded as slurry CN5 and a carbon nanotube composite thin film slurry was prepared based on the dispersion according to steps S4 and S5 of Example 1, recorded as CNE5.
[0054] Comparative Example 2: The aqueous carbon nanotube dispersion slurry uses the same raw material components as those in Example 1, except that after the pre-shearing dispersion process in step S1, the dispersant and ammonia water are first added to the hydrogen peroxide solution, mixed evenly and then transferred to the grinding equipment for grinding and dispersion in S3, and then subjected to the ultrasonic dispersion process in S2. The obtained dispersed slurry is recorded as slurry CN6, and a carbon nanotube composite thin film slurry is prepared based on the dispersion according to steps S4 and S5 of Example 1, recorded as CNE6.
[0055] First, the carbon nanoparticles obtained in the examples and comparative examples were characterized using transmission electron microscopy and scanning electron microscopy. Figures 1 to 4 Shown are electron microscope images of Examples CN1 to CN4, Figure 5 The transmission electron microscope image of CN5. It can be seen from the figure that in the embodiment provided by the present invention, after being oxidized and purified by hydrogen peroxide, the carbon nanotubes have less impurities on the tube wall, so the dispersion effect of the carbon nanotubes in water can be guaranteed, and the conductivity of the carbon nanotubes can be guaranteed. In CN5, the carbon nanotubes are entangled and there are more impurities on the tube wall.
[0056] At the same time, the prepared carbon nanotube composite film slurries CN1 to CN6 were coated with a 50μm square resistance test. According to the table below, the coating square resistance of CN1 to CN4 was maintained at 60Ω / □, which is judged to have good conductivity. For CN5 that was not purified by hydrogen peroxide oxidation, the coating square resistance was 420Ω / □. For Comparative Example 2, after the carbon nanotubes were dissolved in hydrogen peroxide, they did not first undergo an ultrasonic accelerated oxidation process, but were directly neutralized by adding ammonia water. The final test results show that the dispersibility of CN6 is improved compared to that of CN5, but it is still not ideal. The explanation for this result is that during the shear dispersion and sand milling dispersion process, the oxidation process of hydrogen peroxide is not sufficient. In the ultrasonic dispersion stage, only a small amount of residual hydrogen peroxide has an oxidizing effect on the carbon tubes.
[0057] Water-based carbon nanotube slurry sample Carbon nanotube solid content Coating 50μm square resistance Ω / □ Example 1 5% 40 Comparative Example 1 5% 420 Comparative Example 2 5% 310 Example 2 4% 50 Example 3 2.5% 45 Example 4 1% 60
[0058] Then the prepared carbon nanotube composite film slurries CN1 to CN6 were tested for Zeta potential. According to the table below, the absolute values of the Zeta potential of CN1 to CN4 are all above 61mV, and the stability is excellent. However, the Zeta potential of CN5 and CN6 is in the range of instability, and water precipitation begins to occur after being left at room temperature for seven days.
[0059] Water-based carbon nanotube slurry sample Carbon nanotube solid content Zeta potential (mV) Example 1 5% -61.84 Comparative Example 1 5% -26.13 Comparative Example 2 5% -28.52 Example 2 4% -62.46 Example 3 2.5% -61.23 Example 4 1% -62.74
[0060] Finally, the water-based carbon nanotube composite slurry CNE1 obtained in Example 1 was subjected to tape casting coating to prepare a carbon film material, and infrared temperature detection was performed on the carbon film material. The specific detection parameters are as follows:
[0061] CNE1 was coated on the substrate surface by using a tape coating machine, with a coating thickness of 300μm, a coating width of 24cm, and a controlled tape coating speed of 0.7m / min; the drying oven was preheated to 70°C, and finally the required carbon film material was obtained. 10mm copper foil tape was used to lead out on both sides of the carbon film material, and the heating was powered on. The total heating current was 4.5A, the voltage was 230V, and the power was 990W. The infrared temperature detection diagram of the carbon film material is shown in the figure below: Figure 6As shown in the figure, the heating temperature distribution of the carbon film is uniform, which also shows that the carbon nanotubes have excellent dispersion effect.
[0062] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for dispersing carbon nanotubes in water, characterized in that: The steps include: S1. Pre-dispersion: slowly add carbon nanotubes into a hydrogen peroxide solution for purification, and shear and stir for 5-30 minutes; S2, ultrasonic dispersion: the pre-dispersed slurry is transferred into an ultrasonic container for ultrasonic dispersion, with a cycle time of 0.8-1.4h; S3. Prepare aqueous dispersion slurry: add dispersant and ammonia water to the mixed slurry after ultrasound and stir to disperse, then transfer to grinding equipment, repeatedly disperse for 1-2 hours, and finally obtain an aqueous carbon nanotube dispersion with stable dispersibility, wherein the dispersant is one or more of ethanolamine type acrylic acid, alkyl alcohol amide, and lauryl amide propyl amine oxide.
2. The method for dispersing carbon nanotubes in water as claimed in claim 1, characterized in that: The concentration of the hydrogen peroxide solution is 30%, the concentration of the ammonia solution is 25-30%, and the mass ratio of the carbon nanotubes, the hydrogen peroxide solution and the ammonia solution is (1-5): (90-110): (0.1-3).
3. The method for dispersing carbon nanotubes in water as claimed in claim 1, characterized in that: The diameter of the carbon nanotubes is 1-20 nm, the length is 5-100 um, and the mass of the added carbon nanotubes accounts for 1-5% of the total amount of the aqueous carbon nanotube dispersion.
4. The method for dispersing carbon nanotubes in water as claimed in claim 1, characterized in that: In step S2, the ultrasonic frequency is 20-25 KHz.
5. The method for dispersing carbon nanotubes in water as claimed in claim 1, characterized in that: The mass of the added dispersant accounts for 0.1-1.5% of the total amount of the aqueous carbon nanotube dispersion.
6. The method for dispersing carbon nanotubes in water as claimed in claim 1, characterized in that: The shear dispersion of S1, the ultrasonic dispersion of S2, and the stirring and grinding dispersion of S3 are all carried out at room temperature.
7. A method for preparing an aqueous carbon nanotube composite film slurry, characterized in that: The aqueous carbon nanotube dispersion is prepared by mixing an aqueous carbon nanotube dispersion and an aqueous resin; wherein the aqueous carbon nanotube dispersion is obtained by the carbon nanotube aqueous phase dispersion method according to any one of claims 1 to 6, and the mass ratio of solid carbon nanotubes to aqueous resin is 1: (0.5-5).
8. The method for preparing an aqueous carbon nanotube composite film slurry according to claim 7, characterized in that: The method comprises step S4, adding a defoamer and a thickener into the aqueous carbon nanotube dispersion, and stirring and dispersing the mixture for 10-12 minutes; Step S5, adding water-based resin to the slurry treated in S4, and shearing and stirring for 1-1.5 hours to obtain the water-based carbon nanotube composite film slurry.
9. The method for preparing an aqueous carbon nanotube composite film slurry according to claim 8, characterized in that: In step S4, the defoaming agent is one or more of a polyether defoaming agent, an acetylene alcohol defoaming agent and a polyether-modified silicon defoaming agent.
10. The method for preparing an aqueous carbon nanotube composite film slurry according to claim 8, characterized in that: In step S4, the water-based resin material includes: one or more of water-based polyacrylic resin, water-based epoxy resin, water-based polyurethane, water-based polyester resin, and water-based PTFE emulsion.
Citation Information
Patent Citations
A method for separating and purifying carbon nanotubes
CN114314566B
A method to improve the dispersibility of carbon nanotubes
CN114516630B
Batch purification method of carbon nanotubes
CN116462187A
Method for manufacturing mono-layer carbon nano pipe
CN101164872A
Preparation method for dispersing carbon nanotubes and application
CN105731425A