A method for controlling the aspect ratio of Invar etching for ultra-precision metal mask
By forming an oxide film on the ultra-precision metal mask plate, developing and etching treatment, the problems of difficult and poor etching aspect ratio regulation in the prior art are solved, and higher etching precision and factor optimization are achieved.
Patent Information
- Application Number
- CN202410483035.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-22
AI Technical Summary
In the prior art, the Invar etching aspect ratio regulation method is inconvenient to control and has poor etching effect, making it difficult to meet the high-precision metal mask plate in the production of OLED display screens.
By forming an oxide film on the surface of the ultra-precision metal mask plate, film compression, exposure and development operations are performed, the oxide film in the dry film opening area is removed using the surface conditioning liquid, and etching is performed before etching, adjusting the etching depth and aspect ratio to improve the Etching factor.
It effectively increases the etching depth ratio, slows down the lateral erosion behavior, improves the precision and graphical accuracy of etching, and ensures the optimization of etching factors.
Smart Images

Figure CN118441278B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultra-precision metal mask plates, and more specifically, to a method for regulating the depth-to-width ratio of Invar etching for ultra-precision metal mask plates. Background Art
[0002] In the process of producing OLED display screens, multiple layers of metal materials, inorganic materials or organic materials need to be deposited layer by layer on the glass substrate by evaporation. In the evaporation process, the metal mask is used to cover the glass substrate to be evaporated to form a specific pattern. The metal mask can be divided into ordinary metal mask and high-precision fine metal mask, which are used for the deposition of different film layers.
[0003] The existing method of improving the Invar etching aspect ratio in the precision metal mask process is mainly to apply vertical spray pressure to make the longitudinal etching rate greater than the lateral etching rate, thereby obtaining a better etching aspect ratio. The etching aspect ratio = longitudinal etching rate / lateral single-side etching rate. However, the above method is not convenient for regulating the etching aspect ratio, and the etching effect is poor.
[0004] In order to solve the above problems, a technical solution is now provided. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a method for controlling the aspect ratio of Invar etching for an ultra-precision metal mask to solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for controlling the aspect ratio of Invar etching for an ultra-precision metal mask comprises the following steps:
[0008] Step S1: Selecting an ultra-precision metal mask;
[0009] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0010] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0011] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0012] Step S5: preparing surface conditioning solution;
[0013] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0014] Step S7: etching process.
[0015] In a preferred embodiment, in step S1, the thickness of the ultra-precision metal mask is 0.03-0.1 mm.
[0016] In a preferred embodiment, in step S2, the thickness of the oxide film is 60-100 nm.
[0017] In a preferred embodiment, in step S3, a photoresist is applied to the oxide film on the ultra-precision metal mask, the photoresist in the non-pattern area is exposed, and then the photoresist in the unexposed area is dissolved.
[0018] In a preferred embodiment, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness of the developed photoresist are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2;
[0019] When X1<X2, a weak development signal is obtained;
[0020] When X1≥X2, a strong development signal is obtained;
[0021] After a weak development signal is obtained, steps S1 to S4 need to be repeated until a strong development signal is obtained.
[0022] In a preferred embodiment, in step S5, the preparation of the surface conditioning solution comprises the following steps:
[0023] Step S51, preparing 20-24 parts of glycerol, 6-10 parts of potassium oxalate, 7-11 parts of triethanolamine, 10-14 parts of saponin solution and 8-12 parts of triazole corrosion inhibitor;
[0024] Step S52, adding some deionized water into the stainless steel stirring kettle, and heating the stainless steel stirring kettle with steam, with the heating temperature set to 40-45° C.;
[0025] Step S53, adding glycerol, potassium oxalate and triethanolamine in sequence every 5-10 minutes, during which the solution is stirred at a stirring speed of 80-100 r / min;
[0026] Step S54, adding saponin solution and triazole corrosion inhibitor in sequence every 15-20 minutes, during which the solution is stirred, and the stirring speed is set to 120-140 r / min;
[0027] Step S55, after the solution is cooled, finally obtaining the surface adjustment solution.
[0028] In a preferred embodiment, in step S6, removing the oxide film exposed in the dry film opening area includes the following steps:
[0029] Step S61, calculating the area of the oxide film exposed in the dry film opening area;
[0030] Step S62, using a dropper to absorb an appropriate amount of the surface adjustment liquid according to the area of the oxide film exposed in the opening area of the dry film;
[0031] Step S63, dripping the surface conditioning liquid onto the oxide film exposed in the dry film opening area;
[0032] Step S64, erasing the cleaned oxide film and drying the cleaned area;
[0033] Step S65, drying the cleaned part by heat drying, and the drying temperature is set to 30-40°C.
[0034] In a preferred embodiment, in step S7, the etching process comprises the following steps:
[0035] S71, place the ultra-precision metal mask under the horizontal etching line, and etch with etching liquid at an etching speed of 0.6-1.0m / min, with an upper and lower spray pressure of 2-2.4Kg / cm 2 , until the precise etching of the graphics is completed;
[0036] S72, taking out the ultra-precision metal mask plate and performing a cleaning operation, and after the cleaning is completed, air-drying the ultra-precision metal mask plate.
[0037] The technical effects and advantages of the method for controlling the aspect ratio of Invar etching for ultra-precision metal mask of the present invention are as follows:
[0038] 1. Before etching, use the surface adjustment liquid to remove the exposed oxide film in the open area of the dry film, and then etch to increase the aspect ratio. By adjusting the thickness of the dense oxide film on the surface of the ultra-precision metal mask, the etching aspect ratio can be adjusted. There is no oxide film attached to the opening area, and the oxide film is attached to the non-opening area, that is, the area where the dry film remains. There is a certain repulsion to the etching liquid within a certain range, which slows down the lateral side etching behavior to a certain extent, so as to improve the etching factor.
[0039] 2. The present invention performs a developing operation on the exposed photoresist, marks the thickness of the photoresist and the thickness of the photoresist after development, obtains the photoresist thickness difference, marked as X1, and sets a photoresist thickness difference threshold, marked as X2, and then compares X1 and X2 to obtain a weak development signal and a strong development signal. After obtaining the weak development signal, it is necessary to repeat steps S1 to S4 until a strong development signal is obtained, so that the development effect can be well guaranteed.
[0040] 3. The present invention prepares the surface conditioning liquid, and the prepared surface conditioning liquid can effectively remove the oxide film exposed in the opening area of the dry film. When removing the oxide film exposed in the opening area of the dry film, firstly calculate the area of the oxide film exposed in the opening area of the dry film, and then use a dropper to absorb an appropriate amount of the surface conditioning liquid according to the area of the oxide film exposed in the opening area of the dry film, and then drop the surface conditioning liquid onto the oxide film exposed in the opening area of the dry film, so as to ensure the removal effect of the oxide film exposed in the opening area of the dry film. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The present invention is a schematic diagram of a method for regulating the aspect ratio of Invar etching for an ultra-precision metal mask. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] Figure 1 The present invention provides a method for controlling the aspect ratio of ultra-precision metal mask etching using Invar, which comprises the following steps:
[0045] Step S1: Selecting an ultra-precision metal mask;
[0046] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0047] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0048] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0049] Step S5: preparing surface conditioning solution;
[0050] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0051] Step S7: etching process.
[0052] In step S1, the thickness of the ultra-precision metal mask is 0.03 mm, in step S2, the thickness of the oxide film is 60 nm, in step S3, a photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-graphic area is exposed, and then the photoresist in the unexposed area is dissolved, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness after the photoresist is developed are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; when X1<X2, the weak development is obtained. When X1≥X2, a strong developing signal is obtained; after a weak developing signal is obtained, steps S1-S4 need to be repeated until a strong developing signal is obtained; in step S5, the preparation of the surface conditioning solution includes the following steps: step S51, preparing 20 parts of glycerol, 6 parts of potassium oxalate, 7 parts of triethanolamine, 10 parts of saponin solution and 8 parts of triazole corrosion inhibitor; step S52, adding part of deionized water to a stainless steel stirring kettle, heating the stainless steel stirring kettle with steam, and setting the heating temperature to 40°C; step S53, adding glycerol and potassium oxalate in turn every 5 minutes. and triethanolamine, during this process, the solution is stirred, and the stirring speed is set to 80r / min; step S54, saponin solution and triazole corrosion inhibitor are added in sequence every 15min, during this process, the solution is stirred, and the stirring speed is set to 120r / min; step S55, after the solution is cooled, the surface adjustment solution is finally obtained; in step S6, the removal of the oxide film exposed in the dry film opening area includes the following steps: step S61, calculating the area size of the oxide film exposed in the dry film opening area; step S62, according to the exposed area of the dry film opening area The surface conditioning liquid is sucked with a dropper according to the area of the oxide film; step S63, the surface conditioning liquid is dripped onto the oxide film exposed in the opening area of the dry film; step S64, the cleaned oxide film is wiped off and the cleaned part is dried; step S65, the cleaned part is dried by heat drying, and the drying temperature is set to 30°C; in step S7, the etching process includes the following steps: S71, the ultra-precision metal mask is placed under the horizontal etching line, and the etching liquid is used for etching, the etching speed is 0.6m / min, and the upper and lower spray pressures are 2Kg / cm 2 , until the pattern precision etching is completed; S72, taking out the ultra-precision metal mask plate for cleaning operation, and after cleaning, air-drying the ultra-precision metal mask plate.
[0053] Example 2
[0054] Figure 1 The present invention provides a method for controlling the aspect ratio of ultra-precision metal mask etching using Invar, which comprises the following steps:
[0055] Step S1: Selecting an ultra-precision metal mask;
[0056] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0057] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0058] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0059] Step S5: preparing surface conditioning solution;
[0060] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0061] Step S7: etching process.
[0062] In step S1, the thickness of the ultra-precision metal mask is 0.05 mm, in step S2, the thickness of the oxide film is 70 nm, in step S3, a photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-graphic area is exposed, and then the photoresist in the unexposed area is dissolved, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness after the photoresist is developed are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; when X1<X2, the weak development is obtained. When X1≥X2, a strong developing signal is obtained; after a weak developing signal is obtained, steps S1 to S4 need to be repeated until a strong developing signal is obtained; in step S5, the preparation of the surface conditioning solution includes the following steps: step S51, preparing 21 parts of glycerol, 7 parts of potassium oxalate, 8 parts of triethanolamine, 11 parts of saponin solution and 9 parts of triazole corrosion inhibitor; step S52, adding part of deionized water to a stainless steel stirring kettle, heating the stainless steel stirring kettle with steam, and setting the heating temperature to 41°C; step S53, adding glycerol, potassium oxalate and triethanolamine, during this process, the solution is stirred, and the stirring speed is set to 85r / min; step S54, saponin solution and triazole corrosion inhibitor are added in sequence every 16min, during this process, the solution is stirred, and the stirring speed is set to 125r / min; step S55, after the solution is cooled, the surface adjustment solution is finally obtained; in step S6, the removal of the oxide film exposed in the dry film opening area includes the following steps: step S61, calculating the area size of the oxide film exposed in the dry film opening area; step S62, according to the exposed area of the dry film opening area Use a dropper to absorb an appropriate amount of surface conditioning liquid according to the area of the oxide film; step S63, drip the surface conditioning liquid onto the oxide film exposed in the opening area of the dry film; step S64, wipe off the cleaned oxide film and dry the cleaned part; step S65, use a hot baking method to dry the cleaned part, and the drying temperature is set to 32°C; in step S7, the etching process includes the following steps: S71, place the ultra-precision metal mask under the horizontal etching line, and etch with the etching liquid, the etching speed is 0.7m / min, and the upper and lower spray pressures are 2.1Kg / cm 2 , until the pattern precision etching is completed; S72, taking out the ultra-precision metal mask plate for cleaning operation, and after cleaning, air-drying the ultra-precision metal mask plate.
[0063] Example 3
[0064] Figure 1 The present invention provides a method for controlling the aspect ratio of ultra-precision metal mask etching using Invar, which comprises the following steps:
[0065] Step S1: Selecting an ultra-precision metal mask;
[0066] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0067] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0068] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0069] Step S5: preparing surface conditioning solution;
[0070] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0071] Step S7: etching process.
[0072] In step S1, the thickness of the ultra-precision metal mask is 0.06 mm, in step S2, the thickness of the oxide film is 80 nm, in step S3, a photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-graphic area is exposed, and then the photoresist in the unexposed area is dissolved, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness after the photoresist is developed are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; when X1<X2, the weak development is obtained. When X1≥X2, a strong developing signal is obtained; after a weak developing signal is obtained, steps S1 to S4 need to be repeated until a strong developing signal is obtained; in step S5, the preparation of the surface conditioning solution includes the following steps: step S51, preparing 22 parts of glycerol, 8 parts of potassium oxalate, 9 parts of triethanolamine, 12 parts of saponin solution and 10 parts of triazole corrosion inhibitor; step S52, adding part of deionized water to a stainless steel stirring kettle, heating the stainless steel stirring kettle with steam, and setting the heating temperature to 43°C; step S53, adding glycerol and potassium oxalate in turn every 7 minutes; step S54, adding glycerol and potassium oxalate in turn; step S55, adding glycerol and potassium oxalate in turn; step S56, adding glycerol and potassium oxalate in turn; step S57, adding glycerol and potassium oxalate in turn; step S58, adding glycerol and potassium oxalate in turn; step S59, adding glycerol and potassium oxalate in turn; step S60, adding glycerol and potassium oxalate in turn; step S71, adding glycerol and potassium oxalate in turn; step S72, adding glycerol and potassium oxalate in turn; step S73, adding glycerol and potassium oxalate in turn; step S74, adding glycerol and potassium oxalate in turn; step S75, adding glycerol and potassium oxalate in turn; step S76, adding glycerol and potassium oxalate in turn; step S77, adding glycerol and potassium oxalate in turn; step S78, adding glycerol and potassium oxalate in turn; step S79, adding glycerol and potassium oxalate in turn; step S80, adding glycerol and potassium oxalate in turn; step S81, adding glycerol and potassium oxalate in turn; step S82, adding glycerol and potassium oxalate and triethanolamine, during which the solution is stirred at a speed of 90 r / min; step S54, soap solution and triazole corrosion inhibitor are added in sequence every 17 min, during which the solution is stirred at a speed of 130 r / min; step S55, after the solution is cooled, the surface conditioning solution is finally obtained; in step S6, the removal of the oxide film exposed in the dry film opening area includes the following steps: step S61, calculating the area of the oxide film exposed in the dry film opening area; step S62, according to the exposed area of the dry film opening area Use a dropper to absorb an appropriate amount of surface conditioning liquid according to the area of the oxide film; step S63, drip the surface conditioning liquid onto the oxide film exposed in the opening area of the dry film; step S64, wipe off the cleaned oxide film and dry the cleaned part; step S65, use a hot baking method to dry the cleaned part, and the drying temperature is set to 36°C; in step S7, the etching process includes the following steps: S71, place the ultra-precision metal mask under the horizontal etching line, and etch with the etching liquid, the etching speed is 0.8m / min, and the upper and lower spray pressures are 2.2Kg / cm 2 , until the pattern precision etching is completed; S72, taking out the ultra-precision metal mask plate for cleaning operation, and after cleaning, air-drying the ultra-precision metal mask plate.
[0073] Example 4
[0074] Figure 1 The present invention provides a method for controlling the aspect ratio of ultra-precision metal mask etching using Invar, which comprises the following steps:
[0075] Step S1: Selecting an ultra-precision metal mask;
[0076] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0077] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0078] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0079] Step S5: preparing surface conditioning solution;
[0080] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0081] Step S7: etching process.
[0082] In step S1, the thickness of the ultra-precision metal mask is 0.08 mm, in step S2, the thickness of the oxide film is 90 nm, in step S3, a photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-graphic area is exposed, and then the photoresist in the unexposed area is dissolved, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness after the photoresist is developed are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; when X1<X2, the weak development is obtained. signal; when X1≥X2, a strong development signal is obtained; after obtaining a weak development signal, steps S1-S4 need to be repeated until a strong development signal is obtained; in step S5, the preparation of the surface conditioning solution includes the following steps: step S51, preparing 23 parts of glycerol, 9 parts of potassium oxalate, 10 parts of triethanolamine, 13 parts of saponin solution and 11 parts of triazole corrosion inhibitor; step S52, adding part of deionized water to a stainless steel stirring kettle, heating the stainless steel stirring kettle with steam, and setting the heating temperature to 44°C; step S53, adding glycerol and potassium oxalate in turn every 9 minutes and triethanolamine, during which the solution is stirred at a speed of 95 r / min; step S54, soap solution and triazole corrosion inhibitor are added in sequence every 19 min, during which the solution is stirred at a speed of 135 r / min; step S55, after the solution is cooled, the surface conditioning solution is finally obtained; in step S6, the removal of the oxide film exposed in the dry film opening area includes the following steps: step S61, calculating the area of the oxide film exposed in the dry film opening area; step S62, according to the exposed area of the dry film opening area Use a dropper to absorb an appropriate amount of surface conditioning liquid according to the area of the oxide film; step S63, drip the surface conditioning liquid onto the oxide film exposed in the opening area of the dry film; step S64, wipe off the cleaned oxide film and dry the cleaned part; step S65, use a hot baking method to dry the cleaned part, and the drying temperature is set to 38°C; in step S7, the etching process includes the following steps: S71, place the ultra-precision metal mask under the horizontal etching line, and etch with the etching liquid, the etching speed is 0.9m / min, and the upper and lower spray pressures are 2.3Kg / cm 2 , until the pattern precision etching is completed; S72, taking out the ultra-precision metal mask plate for cleaning operation, and after cleaning, air-drying the ultra-precision metal mask plate.
[0083] Example 5
[0084] Figure 1 The present invention provides a method for controlling the aspect ratio of ultra-precision metal mask etching using Invar, which comprises the following steps:
[0085] Step S1: Selecting an ultra-precision metal mask;
[0086] Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface;
[0087] Step S3: performing lamination and exposure operations on the ultra-precision metal mask;
[0088] Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film;
[0089] Step S5: preparing surface conditioning solution;
[0090] Step S6: using a surface conditioning liquid to remove the oxide film exposed from the opening area of the dry film;
[0091] Step S7: etching process.
[0092] In step S1, the thickness of the ultra-precision metal mask is 0.1 mm, in step S2, the thickness of the oxide film is 100 nm, in step S3, a photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-graphic area is exposed, and then the photoresist in the unexposed area is dissolved, in step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness after the photoresist is developed are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; when X1<X2, the weak development is obtained. signal; when X1≥X2, a strong development signal is obtained; after a weak development signal is obtained, steps S1-S4 need to be repeated until a strong development signal is obtained; in step S5, the preparation of the surface conditioning solution includes the following steps: step S51, preparing 24 parts of glycerol, 10 parts of potassium oxalate, 11 parts of triethanolamine, 14 parts of saponin solution and 12 parts of triazole corrosion inhibitor; step S52, adding part of deionized water to a stainless steel stirring kettle, heating the stainless steel stirring kettle with steam, and setting the heating temperature to 45°C; step S53, adding glycerol, oxalic acid in turn every 10 minutes; Potassium and triethanolamine, during this process, the solution is stirred, and the stirring speed is set to 100r / min; step S54, saponin solution and triazole corrosion inhibitor are added in sequence every 20min, during this process, the solution is stirred, and the stirring speed is set to 140r / min; step S55, after the solution is cooled, the surface adjustment solution is finally obtained; in step S6, the removal of the oxide film exposed in the dry film opening area includes the following steps: step S61, calculating the area size of the oxide film exposed in the dry film opening area; step S62, according to the exposed area of the dry film opening area The surface conditioning liquid is sucked with a dropper according to the area of the oxide film; step S63, the surface conditioning liquid is dripped onto the oxide film exposed in the opening area of the dry film; step S64, the cleaned oxide film is wiped off and the cleaned part is dried; step S65, the cleaned part is dried by heat drying, and the drying temperature is set to 40°C; in step S7, the etching process includes the following steps: S71, the ultra-precision metal mask is placed under the horizontal etching line, and the etching is performed using the etching liquid, the etching speed is 1.0m / min, and the upper and lower spray pressures are 2.4Kg / cm 2 , until the pattern precision etching is completed; S72, taking out the ultra-precision metal mask plate for cleaning operation, and after cleaning, air-drying the ultra-precision metal mask plate.
[0093] The ultra-precision metal mask was etched using the Invar etching depth-to-width ratio control method in Examples 1 to 5, and the ultra-precision metal mask was etched using a common method, which was set as a comparative example. The graphic accuracy, etching factor, and edge condition of the ultra-precision metal mask were recorded, and the results are shown in the following table:
[0094] Example Graphics Precision Etching Factor Edge Cases Example 1 high 4.2 smooth Example 2 high 4.6 smooth Example 3 high 4.8 smooth Example 4 high 4.5 smooth Example 5 high 4.3 smooth Comparative Example Low 1.2 Sawtooth
[0095] It can be clearly seen from the above content that the method for controlling the aspect ratio of Invar etching for ultra-precision metal mask of the present invention can effectively improve the etching effect of ultra-precision metal mask, and embodiment 3 is the best embodiment.
[0096] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
[0097] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for controlling the aspect ratio of Invar etching for ultra-precision metal mask, characterized in that: The steps include: Step S1: Selecting an ultra-precision metal mask; Step S2: placing the ultra-precision metal mask into a chemical vapor deposition chamber to form an oxide film on its surface; Step S3: performing lamination and exposure operations on the ultra-precision metal mask; Step S4: placing the exposed ultra-precision metal mask into a developer for development to form a dry film; Step S5: Preparation of surface conditioning solution; In step S5, the preparation of surface conditioning solution includes the following steps: Step S51, preparing 20-24 parts of glycerol, 6-10 parts of potassium oxalate, 7-11 parts of triethanolamine, 10-14 parts of saponin solution and 8-12 parts of triazole corrosion inhibitor; Step S52, adding some deionized water into the stainless steel stirring kettle, and heating the stainless steel stirring kettle with steam, with the heating temperature set to 40-45° C.; Step S53, adding glycerol, potassium oxalate and triethanolamine in sequence every 5-10 minutes, during which the solution is stirred at a stirring speed of 80-100 r / min; Step S54, adding saponin solution and triazole corrosion inhibitor in sequence every 15-20 minutes, during which the solution is stirred, and the stirring speed is set to 120-140 r / min; Step S55, after the solution is cooled, finally obtaining the surface adjustment solution; Step S6: using a surface conditioning liquid to remove the oxide film exposed from the dry film opening area; in step S6, removing the oxide film exposed from the dry film opening area includes the following steps: Step S61, calculating the area of the oxide film exposed in the dry film opening area; Step S62, using a dropper to absorb an appropriate amount of the surface adjustment liquid according to the area of the oxide film exposed in the opening area of the dry film; Step S63, dripping the surface conditioning liquid onto the oxide film exposed in the dry film opening area; Step S64, erasing the cleaned oxide film and drying the cleaned area; Step S65, drying the cleaned part by heat drying, with the drying temperature set to 30-40°C; Step S7: etching process.
2. The method for controlling the aspect ratio of Invar etching for ultra-precision metal mask according to claim 1, characterized in that: In step S1 , the thickness of the ultra-precision metal mask is 0.03-0.1 mm.
3. The method for controlling the aspect ratio of Invar etching for ultra-precision metal mask according to claim 1, characterized in that: In step S2, the thickness of the oxide film is 60-100 nm.
4. The method for controlling the aspect ratio of Invar etching for ultra-precision metal mask according to claim 1, characterized in that: In step S3, photoresist is pasted on the oxide film on the ultra-precision metal mask, the photoresist in the non-pattern area is exposed, and then the photoresist in the unexposed area is dissolved.
5. The method for controlling the aspect ratio of Invar etching for ultra-precision metal mask according to claim 4, characterized in that: In step S4, the exposed photoresist is developed, the thickness of the photoresist and the thickness of the developed photoresist are marked, the photoresist thickness difference is obtained, marked as X1, and the photoresist thickness difference threshold is set, marked as X2; When X1<X2, a weak development signal is obtained; When X1≥X2, a strong development signal is obtained; After a weak development signal is obtained, steps S1 to S4 need to be repeated until a strong development signal is obtained.
6. The method for controlling the aspect ratio of Invar etching for ultra-precision metal mask according to claim 1, characterized in that: In step S7, the etching process includes the following steps: S71, place the ultra-precision metal mask under the horizontal etching line, and etch with etching liquid at an etching speed of 0.6-1.0m / min, with an upper and lower spray pressure of 2-2.4Kg / cm 2 , until the precise etching of the graphics is completed; S72, taking out the ultra-precision metal mask plate and performing a cleaning operation, and after the cleaning is completed, air-drying the ultra-precision metal mask plate.
Citation Information
Patent Citations
Bottom etching method preventing etching of side wall of through-silicon-via
CN104505366A
Preparation method of active region
CN106229288A
Manufacturing method of trench and manufacturing method of memory device
CN114005750A
Preparation method of deep trench isolation structure with high aspect ratio
CN116313779A
Etching method for solving shape problem of deep groove with high aspect ratio
CN117476450A