Method and device for producing hydrogen by methane-assisted high-temperature electrolysis

By introducing the reducing fuel of methane into the solid oxide electrolytic cell, reducing the potential difference between the cathode and the anode, and using methane cracking and reverse steam reforming reactions, the waste of power resources and hydrogen production in the solid oxide electrolytic cell during the electrolysis of water are solved. The problem of low efficiency is improved by improving the hydrogen production efficiency and the utilization efficiency of synthesis gas.

CN118441291BActive Publication Date: 2024-10-29GUANGZHOU POWER SUPPLY BUREAU GUANGDONG POWER GRID CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410904716.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Existing solid oxide electrolytic cells need to overcome high potential differences during the electrolysis of water to produce hydrogen, resulting in a waste of power resources and low hydrogen production efficiency, and the hydrogen consumed on the anode side offsets the hydrogen produced by electrolysis on the cathode side.

Method used

The reducing fuel that introduces methane is coupled with the solid oxide electrolytic cell, and methane of different concentrations is sequentially input through multiple stages to reduce the potential difference between the cathode and the anode, and the methane cracking and reverse water vapor reforming reactions are used to improve the utilization of resources to generate additional gas. efficacy.

Benefits of technology

It reduces the electrolysis energy consumption of solid oxide electrolytic cells, improves the production efficiency of hydrogen and the utilization efficiency of synthesis gas, and promotes the industrial development of high-temperature electrolysis technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118441291B_ABST
    Figure CN118441291B_ABST
Patent Text Reader

Abstract

The present invention provides a method and device for producing hydrogen by methane-assisted high-temperature electrolysis, which is applied to a solid oxide electrolytic cell, wherein the solid oxide electrolytic cell includes a nickel-based cathode, an electrolyte and an anode, and the method includes: introducing water and carbon dioxide as raw materials into the solid oxide electrolytic cell to obtain hydrogen and carbon monoxide at the nickel-based cathode; introducing methane gas in different proportions into the solid oxide electrolytic cell at the corresponding reaction stage to obtain an additional product synthesis gas at the anode; extracting hydrogen from the hydrogen and carbon monoxide obtained at the nickel-based cathode and the additional product synthesis gas obtained at the anode. The method reduces the potential difference between the cathode and cathode by introducing a reducing fuel of methane and coupling it with the solid oxide electrolytic cell, and uses methane of different concentrations in multiple stages to sequentially input and consume the impurity gas generated during the electrolysis process, output high-grade synthesis gas, and improve the resource utilization efficiency of generating additional gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen production, and in particular to a method and device for producing hydrogen by methane-assisted high-temperature electrolysis. Background Art

[0002] Hydrogen is an ideal energy carrier due to its high energy density, storability, cleanliness and pollution-free. It has received extensive attention at home and abroad in recent years. At present, the main constraint on the development of hydrogen energy comes from the efficiency of hydrogen production.

[0003] Hydrogen production by water electrolysis uses water as raw material and produces hydrogen by electrolyzing water under the action of electric energy. The entire hydrogen production process is pollution-free and is a very promising hydrogen production method. The current hydrogen production technologies by water electrolysis mainly include alkaline electrolysis cell (AEC), proton exchange membrane electrolysis cell (PEMEC) and solid oxide electrolysis cell (SOEC). Among them, the solid oxide electrolysis cell can convert raw water into hydrogen and oxygen through an electrochemical reaction process at high temperature, thereby realizing the efficient conversion of electrical energy and thermal energy into chemical energy. The high-temperature electrolysis technology based on the solid oxide electrolysis cell has the advantages of modularization, easy assembly and flexible application, and is an energy conversion and storage technology with great application prospects.

[0004] However, in the existing process of producing hydrogen by electrolysis of water, the solid oxide electrolytic cell generally uses hydrogen or carbon monoxide as a carrier gas during operation so that the cathode is always in a reducing atmosphere, while the anode, as the oxygen generation side, is placed in the air. The traditional solid oxide electrolytic cell needs to overcome a very high potential difference to achieve the reverse migration of oxygen ions from the cathode to the anode, resulting in a huge waste of electricity resources. In addition, the hydrogen consumed on the anode side offsets part of the hydrogen produced by electrolysis on the cathode side, resulting in low hydrogen preparation efficiency. The method of producing hydrogen by electrolysis cannot be applied industrially. Summary of the invention

[0005] Based on this, the present invention provides a method and device for producing hydrogen by methane-assisted high-temperature electrolysis, which reduces the potential difference between the anode and cathode by introducing a reducing fuel of methane and couples it with a solid oxide electrolysis cell, and utilizes multi-stage methane of different concentrations to sequentially input and consume the impurity gas generated during the electrolysis process, outputs high-grade synthesis gas, and improves the resource utilization efficiency of generating additional gas.

[0006] In a first aspect, the present invention provides a method for producing hydrogen by methane-assisted high-temperature electrolysis, the method being applied to a solid oxide electrolysis cell, the solid oxide electrolysis cell comprising a nickel-based cathode, an electrolyte and an anode, the method comprising:

[0007] Water and carbon dioxide are introduced as raw materials into a solid oxide electrolytic cell to obtain hydrogen and carbon monoxide at a nickel-based cathode;

[0008] Different proportions of methane gas are introduced into the solid oxide electrolysis cell at corresponding reaction stages to obtain an additional product, synthesis gas, at the anode;

[0009] Hydrogen is extracted from hydrogen and carbon monoxide obtained from the nickel-based cathode and the additional product synthesis gas obtained from the anode.

[0010] Furthermore, the method of introducing different proportions of methane gas into the solid oxide electrolysis cell at the corresponding reaction stage to obtain an additional product synthesis gas at the anode includes:

[0011] Passing a first proportion of methane gas into the solid oxide electrolysis cell in the second reaction stage to obtain a first additional product synthesis gas at the anode;

[0012] Passing a second proportion of methane gas into the solid oxide electrolysis cell in the third reaction stage to obtain a second additional product synthesis gas at the anode;

[0013] The first additional product synthesis gas and the second proportion of methane gas are reacted in the third reaction stage through methane cracking reaction and reverse steam reforming reaction to obtain part of the second additional product synthesis gas.

[0014] Furthermore, the first additional product synthesis gas includes carbon dioxide and water vapor; the second additional product synthesis gas includes carbon monoxide and hydrogen; the additional product synthesis gas includes carbon monoxide and hydrogen.

[0015] Preferably, during the switching process between the second reaction stage and the third reaction stage, nitrogen is introduced into the anode of the solid oxide electrolytic cell until the original gas is exhausted.

[0016] Furthermore, the first ratio is smaller than the second ratio.

[0017] Furthermore, the first proportion of methane gas is methane gas with a concentration of 30%, and the second proportion of methane gas is methane gas with a concentration of 100%.

[0018] Preferably, the operating temperature of the electrolytic hydrogen production method is set at 800°C-1000°C.

[0019] In a second aspect, the present invention further provides a device for producing hydrogen by methane-assisted high-temperature electrolysis, the device being applied to a solid oxide electrolysis cell, the solid oxide electrolysis cell comprising a nickel-based cathode, an electrolyte and an anode, characterized in that the device comprises:

[0020] A cathode product module, used for passing water and carbon dioxide as raw materials into a solid oxide electrolysis cell to obtain hydrogen and carbon monoxide at a nickel-based cathode;

[0021] The anode product module is used to pass different proportions of methane gas into the solid oxide electrolysis cell at the corresponding reaction stage to obtain an additional product synthesis gas at the anode;

[0022] The gas purification module is used to extract hydrogen from the hydrogen and carbon monoxide obtained from the nickel-based cathode and the additional product synthesis gas obtained from the anode.

[0023] Furthermore, the anode product module comprises:

[0024] A first-stage reaction unit is used to pass a first proportion of methane gas into the solid oxide electrolysis cell in a second reaction stage to obtain a first additional product synthesis gas at the anode;

[0025] A second stage reaction unit is used to pass a second proportion of methane gas into the solid oxide electrolysis cell in the third reaction stage to obtain a second additional product synthesis gas at the anode;

[0026] The first additional product synthesis gas and the second proportion of methane gas are reacted in the third reaction stage through methane cracking reaction and reverse steam reforming reaction to obtain part of the second additional product synthesis gas.

[0027] Specifically, the first additional product synthesis gas includes carbon dioxide and water vapor; the second additional product synthesis gas includes carbon monoxide and hydrogen; the additional product synthesis gas includes carbon monoxide and hydrogen.

[0028] The beneficial effects of adopting the above technical solution are as follows: the present application reduces the potential difference between the cathode and the anode of the solid oxide electrolysis cell by introducing methane reducing gas, and further prepares high-grade synthesis gas while reducing the electrolysis energy consumption of the solid oxide electrolysis cell through methane cracking and reverse steam reforming reaction, thereby improving the utilization efficiency of the additional gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0030] Figure 1 This is a schematic diagram of a method for producing hydrogen by methane-assisted high-temperature electrolysis in one embodiment of the present application;

[0031] Figure 2 This is a schematic diagram of the first reaction stage of a solid oxide electrolysis cell in one embodiment of the present application;

[0032] Figure 3This is a schematic diagram of the second reaction stage of a solid oxide electrolytic cell in one embodiment of the present application;

[0033] Figure 4 This is a schematic diagram of the third reaction stage of a solid oxide electrolysis cell in one embodiment of the present application;

[0034] Figure 5 This is a schematic diagram of a device for producing hydrogen by methane-assisted high-temperature electrolysis in one embodiment of the present application. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In order to explain the present invention in more detail, the method and device for producing hydrogen by methane-assisted high-temperature electrolysis provided by the present invention are specifically described below in combination with the drawings.

[0036] Unless otherwise defined, the technical terms or scientific terms used in the disclosure of this application should be understood by people with ordinary skills in the field to which the present invention belongs. The "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, similar words such as "one", "one" or "the" do not indicate a quantitative limit, but indicate that there is at least one. Similar words such as "include" or "include" mean that the elements or objects appearing in front of the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Similar words such as "connect" or "connected" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship can also change accordingly.

[0037] Hydrogen production by water electrolysis uses water as raw material and produces hydrogen by electrolyzing water under the action of electric energy. The entire hydrogen production process is pollution-free and is a very promising hydrogen production method. The current hydrogen production technologies by water electrolysis mainly include alkaline electrolysis cell (AEC), proton exchange membrane electrolysis cell (PEMEC) and solid oxide electrolysis cell (SOEC). Among them, the solid oxide electrolysis cell can convert raw water into hydrogen and oxygen through an electrochemical reaction process at high temperature, thereby realizing the efficient conversion of electrical energy and thermal energy into chemical energy. The high-temperature electrolysis technology based on the solid oxide electrolysis cell has the advantages of modularization, easy assembly and flexible application, and is an energy conversion and storage technology with great application prospects.

[0038] The traditional solid oxide electrolysis cell (hereinafter referred to as SOEC) is the reverse process of the solid oxide fuel cell (SOFC). Taking high-temperature water electrolysis as an example, the high-temperature water vapor obtains electrons at the nickel-based cathode and is reduced to hydrogen and oxygen ions. Driven by an external voltage, the oxygen ions overcome a certain oxygen partial pressure gradient and pass through the electrolyte. They are transferred from the cathode to the anode and release electrons to generate oxygen. The specific electrolysis reaction is (the following formula is only for the reactants in SOEC, and its reaction conditions are not marked):

[0039] Cathode reaction: ,

[0040] Anode reaction: ,

[0041] Overall response of SOEC: .

[0042] However, in order to prevent the nickel-based cathode from being oxidized and deactivated, and to facilitate the subsequent separation of electrolysis products, SOEC generally uses hydrogen or carbon monoxide as a carrier gas to keep the cathode in a reducing atmosphere, while the anode is placed in the air as the oxygen generation side. The traditional solid oxide electrolysis cell needs to overcome a very high potential difference to achieve the reverse migration of oxygen ions from the cathode to the anode, resulting in a huge waste of power resources. Taking 800°C as an example, the working conditions of 50% (volume fraction) hydrogen-50% water vapor or air, the open circuit voltage of SOEC is as high as 0.94V, that is, only when the external voltage is higher than the open circuit voltage of 0.94V can the water electrolysis reaction be started to become effective electrical energy, and most of the electrical energy is used to overcome the potential difference between hydrogen-water vapor or air, resulting in a waste of power resources.

[0043] In this regard, the present invention provides a method for producing hydrogen by methane-assisted high-temperature electrolysis, wherein methane of different concentrations is sequentially introduced into a solid oxide electrolytic cell at multiple stages, the reducibility of methane is used to reduce the potential difference between the cathode and the anode, and the carbon dioxide gas generated during the electrolysis process is converted into carbon monoxide by partial oxidation of methane, so that the output synthetic gas only includes hydrogen and carbon monoxide, and a high-value additional product carbon monoxide is obtained, thereby improving the utilization efficiency of the gas produced by the solid oxide electrolytic cell. This method is described by taking the application of the method to a terminal device as an example, and combined with the attached Figure 1 Schematic diagram of the method for producing hydrogen using methane-assisted high-temperature electrolysis.

[0044] An embodiment of the present application provides an application scenario of a method for producing hydrogen by methane-assisted high-temperature electrolysis. The application scenario is a solid oxide electrolysis cell, which includes a nickel-based cathode, an electrolyte, and an anode. By inputting methane gas into the solid oxide electrolysis cell, a synthetic gas consisting only of hydrogen and carbon monoxide is obtained, and hydrogen is extracted from the synthetic gas. For the specific process, please refer to the embodiment of the method for producing hydrogen by methane-assisted high-temperature electrolysis.

[0045] Step S101, water and carbon dioxide are introduced as raw materials into a solid oxide electrolysis cell to obtain hydrogen and carbon monoxide at a nickel-based cathode.

[0046] Step S102, introducing methane gas in different proportions into a solid oxide electrolysis cell at corresponding reaction stages, and obtaining an additional product synthesis gas at the anode.

[0047] Specifically, the additional product synthesis gas obtained at the anode includes carbon monoxide and hydrogen.

[0048] Step S103, extracting hydrogen from the hydrogen and carbon monoxide obtained from the nickel-based cathode and the additional product synthesis gas obtained from the anode.

[0049] Specifically, the above step S102 introduces methane gas in different proportions into the solid oxide electrolysis cell at the corresponding reaction stage to obtain the additional product synthesis gas at the anode, which is further described as follows:

[0050] Step S201, introducing a first proportion of methane gas into a solid oxide electrolysis cell in a second reaction stage, and obtaining a first additional product synthesis gas at the anode.

[0051] The first proportion of methane gas is low-concentration methane gas, preferably methane gas with a concentration of 30%. The first additional product synthesis gas is carbon dioxide and water vapor.

[0052] Step S202, introducing a second proportion of methane gas into the solid oxide electrolysis cell in the third reaction stage to obtain a second additional product synthesis gas at the anode.

[0053] The second proportion of methane gas is high-concentration methane gas, the first proportion is less than the second proportion, and preferably the concentration of methane gas is 100%. The second additional product synthesis gas is carbon monoxide and hydrogen.

[0054] The first additional product synthesis gas and the second proportion of methane gas are reacted in the third reaction stage through methane cracking reaction and reverse steam reforming reaction to obtain part of the second additional product synthesis gas.

[0055] In addition, during the switching process between the second reaction stage and the third reaction stage, nitrogen is introduced into the anode of the solid oxide electrolytic cell until the original gas is exhausted. Generally, nitrogen is used to purge the anode of the solid oxide electrolytic cell for 3 minutes to exhaust the original gas and introduce new gas. The role of the nitrogen is only as a carrier gas to keep the nickel-based cathode in a reducing atmosphere.

[0056] The above-mentioned introduction of methane into the solid oxide electrolysis cell (SOEC) can reduce the operating cost of water electrolysis hydrogen production, improve the efficiency of water electrolysis hydrogen production, and promote the industrialization and production development of high-temperature electrolysis technology. Figure 2-4 The reaction diagram of the solid oxide electrolysis cell gives a detailed description of the overall reaction process based on the three reaction stages of the solid oxide electrolysis cell (SOEC).

[0057] Combined with Figure 2 In the first reaction stage of the solid oxide electrolysis cell (SOEC), water and carbon dioxide are input as raw materials into the solid oxide electrolysis cell to prepare a synthesis gas including carbon monoxide and hydrogen, wherein and The electrons obtained at the cathode are dissociated into , and , It can be converted into , Driven by an external voltage, it passes through the dense electrolyte from the cathode to the anode and releases electrons at the anode to generate The specific electrode reaction is as follows:

[0058] Cathode reaction: ,

[0059] Anode reaction: .

[0060] In addition, in order to observe the difference between the solid oxide electrolysis cell (SOEC) without the introduction of methane gas to assist hydrolysis and the introduction of methane gas to assist hydrolysis in the subsequent reaction stage, nitrogen ( ) and oxygen for comparison.

[0061] Combined with Figure 3 In the second reaction stage of the solid oxide electrolytic cell (SOEC), a low concentration of methane, such as 30% methane gas, is introduced into the anode of the SOEC, so that the methane is deeply oxidized to generate the first additional product, synthesis gas, carbon dioxide and water vapor. The production of a large amount of carbon dioxide can reduce the carbon potential of the atmosphere and reduce the possibility of carbon deposition on the electrode. The specific electrode reaction is as follows:

[0062] Cathode reaction: ,

[0063] ,

[0064] Anode reaction: .

[0065] Combined with Figure 4 In the third reaction stage of the solid oxide electrolysis cell (SOEC), a high concentration of methane, such as 100% methane gas, is introduced into the anode of the SOEC to partially oxidize the methane to generate a second additional product, synthesis gas, carbon monoxide and hydrogen. When the methane concentration is high enough, the anode fuel , and electrolytic migration In addition to partial oxidation reactions, methane cracking reactions and reverse water gas reforming reactions may also occur. If methane cracking reactions mainly occur to generate solid carbon, excess solid carbon will cover the catalyst surface of the solid oxide electrolytic cell, occupying the active sites of the electrode reaction, causing the electrolytic cell performance to rapidly deteriorate. and Complete reaction occurs and The increase in oxygen partial pressure at the cathode end of the electrolytic cell leads to an increase in the potential difference of the SOEC system, and the potential barrier that the system needs to overcome increases, which not only causes an increase in electrolysis power consumption but also A huge waste of resources will also generate a lot of Gas, making The benefits of auxiliary high-temperature electrolysis are greatly reduced. In order to reduce the power consumption of high-temperature water electrolysis hydrogen production technology while maximizing the development The industrial value of fuel requires that the anode side According to the partial oxidation reaction mode, a high-grade second additional product synthesis gas is produced, that is, + A gas mixture of The molar ratio is about 2. The specific electrode reaction is as follows:

[0066] Cathode reaction: ,

[0067] ,

[0068] Anode reaction: .

[0069] Furthermore, in order to ensure partial oxidation of methane gas in the third reaction stage, the working temperature of the electrolytic hydrogen production method is set at 800°C-1000°C. The equilibrium composition of each component at 800°C, 900°C and 1000°C on the anode side can be obtained by thermodynamic software calculation. Completely derived from byproducts of cathode electrolysis reaction , and is proportional to the electrolysis current. And as the working temperature increases from 800°C to 1000°C, the content of solid carbon decreases significantly, and the corresponding carbon monoxide concentration increases rapidly. The carbon deposition of the solid oxide electrolytic cell can be reduced by increasing the working temperature, and the selectivity of carbon monoxide can be improved.

[0070] In this embodiment, methane of different concentrations is introduced into the solid oxide electrolysis cell in sequence at multiple stages, the reducing property of methane is used to reduce the potential difference between the cathode and the anode, and the carbon dioxide gas generated during the electrolysis process is converted into carbon monoxide by partial oxidation of methane, so that the output synthesis gas only includes hydrogen and carbon monoxide, and a high-value added product carbon monoxide is obtained, thereby improving the utilization efficiency of the gas output from the solid oxide electrolysis cell.

[0071] In addition, with regard to the limitation of high temperature working conditions for hydrogen production by solid oxide electrolysis, the following specific examples are given to illustrate the influence of high temperature on hydrogen production by electrolysis:

[0072] The partial oxidation reaction of methane will release a certain amount of heat energy. The hydrolysis reaction uses the energy released by the partial oxidation reaction to reduce the total energy consumption of the reaction, that is, ,in The heat released by the partial oxidation of methane.

[0073] At 298.15K and 101.325kPa, the energy consumption of water electrolysis to produce hydrogen (denoted as ) and free energy (denoted as ) are 285.8 kJ / mol and 237.2 kJ / mol respectively. The power consumption is the total energy required for water electrolysis, the free energy is the Gibbs free energy, i.e. the power required for water electrolysis, and Q is the high temperature heat energy. The thermodynamic model at different temperatures is as follows:

[0074] .

[0075] As the reaction temperature increases from 600°C to 1000°C, the power consumption ( ) decreases with increasing temperature, and the corresponding ratio of power consumption to total energy consumption ( ) will also decrease accordingly. At the same time, thermal energy can be replaced by low-grade heat sources such as industrial waste heat, which is expected to reduce the operating cost of hydrogen production by electrolysis of water and enhance the industrial competitiveness of hydrogen production technology by electrolysis of water.

[0076] In addition, the temperature and current density were further investigated to determine the methane auxiliary The influence of chemical properties of the co-electrolysis process, the electrode polarization resistance of the electrolytic cell gradually decreases as the reaction temperature increases from 600℃ to 1000℃ under open circuit conditions. Therefore, increasing the working temperature is beneficial to accelerate the methane-assisted high temperature However, as the current density increases, the electrode polarization resistance gradually increases. Therefore, the reaction rate of the methane-assisted electrolysis process is mainly controlled by the concentration polarization caused by insufficient reactants, which is particularly obvious under high current and high temperature conditions.

[0077] It should be understood that although the Figure 1 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily executed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and these steps can be executed in other orders. Figure 1 At least part of the steps may include multiple sub-steps or sub-stages. These sub-steps or stages are not necessarily executed at the same time, but can be executed at different times. The execution order of these sub-steps or stages is not necessarily sequential, but can be executed in turn or alternately with other steps or at least part of the sub-steps or stages of other steps.

[0078] The above embodiments of the present invention describe in detail the method for producing hydrogen by methane-assisted high-temperature electrolysis. The above method disclosed in the present invention can be implemented by various types of equipment. Therefore, the present invention also discloses a device for producing hydrogen by methane-assisted high-temperature electrolysis corresponding to the above method. Figure 5 , specific embodiments are given below to explain in detail.

[0079] The cathode product module 301 is used to pass water and carbon dioxide as raw materials into the solid oxide electrolysis cell to obtain hydrogen and carbon monoxide at the nickel-based cathode.

[0080] The anode product module 302 is used to pass methane gas in different proportions into the solid oxide electrolysis cell at the corresponding reaction stage to obtain an additional product synthesis gas at the anode.

[0081] The gas purification module 303 is used to extract hydrogen from the hydrogen and carbon monoxide obtained from the nickel-based cathode and the additional product synthesis gas obtained from the anode.

[0082] Furthermore, the anode product module comprises:

[0083] A first-stage reaction unit is used to pass a first proportion of methane gas into the solid oxide electrolysis cell in a second reaction stage to obtain a first additional product synthesis gas at the anode;

[0084] A second stage reaction unit is used to pass a second proportion of methane gas into the solid oxide electrolysis cell in the third reaction stage to obtain a second additional product synthesis gas at the anode;

[0085] The first additional product synthesis gas and the second proportion of methane gas are reacted in the third reaction stage through methane cracking reaction and reverse steam reforming reaction to obtain part of the second additional product synthesis gas.

[0086] Specifically, the first additional product synthesis gas includes carbon dioxide and water vapor; the second additional product synthesis gas includes carbon monoxide and hydrogen; the additional product synthesis gas includes carbon monoxide and hydrogen.

[0087] Preferably, during the switching process between the second reaction stage and the third reaction stage, nitrogen is introduced into the anode of the solid oxide electrolytic cell until the original gas is exhausted.

[0088] Furthermore, the first ratio is smaller than the second ratio.

[0089] Furthermore, the first proportion of methane gas is methane gas with a concentration of 30%, and the second proportion of methane gas is methane gas with a concentration of 100%.

[0090] Preferably, the operating temperature of the electrolytic hydrogen production method is set at 800°C-1000°C.

[0091] For the device for producing hydrogen by methane-assisted high-temperature electrolysis, all the above-mentioned methods can be referred to, and no further details will be given here. Each module in the above-mentioned device can be implemented in whole or in part by software, hardware, and a combination thereof. Each of the above-mentioned modules can be embedded in or independent of the processor of the terminal device in the form of hardware, or can be stored in the memory of the terminal device in the form of software, so that the processor can call and execute the operations corresponding to each of the above modules.

[0092] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing hydrogen by methane-assisted high-temperature electrolysis, the method being applied to a solid oxide electrolytic cell, the solid oxide electrolytic cell comprising a nickel-based cathode, an electrolyte and an anode, characterized in that: The method comprises: Water and carbon dioxide are introduced as raw materials into a solid oxide electrolytic cell to obtain hydrogen and carbon monoxide at a nickel-based cathode; Different proportions of methane gas are introduced into the solid oxide electrolysis cell at corresponding reaction stages to obtain an additional product, synthesis gas, at the anode; Hydrogen is extracted from hydrogen and carbon monoxide obtained from the nickel-based cathode and the additional product synthesis gas obtained from the anode; In the first reaction stage, oxygen and nitrogen are introduced into the anode; The method of introducing different proportions of methane gas into a solid oxide electrolysis cell at corresponding reaction stages to obtain an additional product synthesis gas at the anode comprises: Passing a first proportion of methane gas into the solid oxide electrolysis cell in the second reaction stage to obtain a first additional product synthesis gas at the anode; Passing a second proportion of methane gas into the solid oxide electrolysis cell in the third reaction stage to obtain a second additional product synthesis gas at the anode; The second proportion of methane gas is subjected to a methane cracking reaction and a reverse steam reforming reaction in the third reaction stage to obtain a portion of the second additional product synthesis gas; The first additional product synthesis gas includes carbon dioxide and water vapor; the second additional product synthesis gas includes carbon monoxide and hydrogen; The first ratio is smaller than the second ratio.

2. The method for producing hydrogen by methane-assisted high-temperature electrolysis according to claim 1, characterized in that: Also includes: During the switching process between the second reaction stage and the third reaction stage, nitrogen is introduced into the anode of the solid oxide electrolytic cell until the original gas is exhausted.

3. The method for producing hydrogen by methane-assisted high-temperature electrolysis according to claim 1, characterized in that: The first proportion of methane gas is methane gas with a concentration of 30%, and the second proportion of methane gas is methane gas with a concentration of 100%.

4. The method for producing hydrogen by methane-assisted high-temperature electrolysis as claimed in claim 3, characterized in that: The working temperature of the method is set at 800°C-1000°C.

Citation Information

Patent Citations

  • Method for preparing chemicals by electrochemical oxidation of methane

    CN111058053A

  • Partial oxidation of methane (POM) assisted solid oxide co-electrolysis

    US20150299871A1