Antistatic polycaprolactam composite material and preparation method thereof

By in-situ polymerizing nano-zinc oxide, carbon nanotubes, modified graphene oxide and other materials into polycaprolactam fiber, the problem of static electricity accumulation in polycaprolactam fiber is solved, achieving both permanent antistatic properties and mechanical properties of the material, improving improve textile performance and market efficiency.

CN118459987BActive Publication Date: 2024-10-01JIANGSU WENFENG CHEM FIBER GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410910822.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The accumulation of static electricity in polycaprolactam fibers in dry environments results in low comfort and poor safety. Existing antistatic improvement methods affect mechanical properties or are costly and unsustainable.

Method used

Nano-zinc oxide, carbon nanotubes, modified graphene oxide, modified fiber powder and other materials are compounded into the polycaprolactam polymer structure through in-situ polymerization to prepare antistatic polycaprolactam composite materials, which are combined with modified fiber powder. Explosion and microwave treatment ensure the permanent antistatic effect and mechanical properties of the material.

Benefits of technology

It achieves permanent antistatic properties of polycaprolactam fiber, maintains good mechanical properties and textile properties, and improves the market economic benefits of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides an antistatic polycaprolactam composite material and a preparation method thereof, and relates to the field of textile chemical fiber technology. The antistatic polycaprolactam composite material is obtained by in-situ polymerization of caprolactam, nano zinc oxide, carbon nanotubes, modified graphene oxide, modified fiber powder, phosphoric acid, acetic acid and other materials, and the modified fiber powder is obtained by steam explosion treatment of plant fiber powder, microwave shaping and then mixing with nano titanium dioxide for modification. The present invention overcomes the shortcomings of the prior art, achieves a permanent antistatic effect of the material by an in-situ polymerization method, ensures good mechanical properties and textile properties of the material, and increases the market economic benefits of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile chemical fibers, and in particular to an antistatic polycaprolactam composite material and a preparation method thereof. Background Art

[0002] Polycaprolactam (PA6) fiber has excellent strength, abrasion resistance, moisture absorption and elastic recovery rate. It has been widely used in clothing, home decoration and industrial industries. Polycaprolactam polymer is bonded by covalent bonds, and there are fewer polar groups in the main chain structure. Therefore, polycaprolactam has a large surface resistance of up to 10 13 ~10 14 Ω, which will generate static electricity accumulation when it rubs against other objects or itself. In the textile field, this type of chemical fiber product is less comfortable to use, especially in dry winter, and has poor safety for high-tech industries such as electronics, which greatly limits the application of polycaprolactam.

[0003] The existing methods to improve the antistatic ability of polycaprolactam are mainly divided into physical blending, surface treatment and copolymerization modification. Among them, physical blending is to mix various antistatic agents / conductive agents into PA6 slices through screw blending and other methods. Its antistatic effect is mainly related to the amount and type of antistatic agent added. However, after overall physical blending, the antistatic agent will cause the material's anti-corrosion performance to deteriorate, affecting the material's durability and mechanical properties;

[0004] Surface treatment is generally used in the field of prevention and control. For polycaprolactam spinning or fabric, the surface is impregnated, brushed, sprayed, etc. to form an antistatic layer, but this type of antistatic layer is not resistant to friction. The textile will cause the coating to fall off after machine or manual washing, thereby reducing the antistatic property of the material. In addition, for the textile field, the cost of surface treatment antistatic is high and the effect is poor in sustainability;

[0005] Copolymer modification mainly introduces materials with antistatic or conductive properties into the polymer structure by in-situ polymerization to achieve a permanent antistatic effect. However, changes in the polymer structure will also cause changes in the mechanical properties of the final product and may even affect the spinnability of polycaprolactam fibers, making it difficult to be well used in the textile field. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides an antistatic polycaprolactam composite material and a preparation method thereof, which achieves a permanent antistatic effect of the material through an in-situ polymerization method, ensures good mechanical properties and textile properties of the material, and increases the market economic benefits of the material.

[0007] To achieve the above objectives, the technical solution of the present invention is implemented through the following solutions:

[0008] An antistatic polycaprolactam composite material comprises the following raw materials in parts by weight: 100-120 parts of caprolactam, 0.1-0.4 parts of nano zinc oxide, 0.5-1.0 parts of carbon nanotubes, 0.8-1.2 parts of modified graphene oxide, 1.5-2.5 parts of modified fiber powder, 0.2-0.6 parts of phosphoric acid, and 0.2-0.4 parts of acetic acid; wherein the modified graphene oxide is obtained by treating graphene oxide with 4-amino-N-methylbenzamide as a modifier; and the modified fiber powder is obtained by treating plant fiber powder with steam explosion, microwave shaping, and then mixing with nano titanium dioxide for modification.

[0009] Preferably, the carbon nanotubes have a length of 100 nm-500 nm and a tube diameter of 5 nm-15 nm.

[0010] Preferably, the particle size of the nano zinc oxide is 30nm-80nm.

[0011] Preferably, the preparation method of the modified graphene oxide comprises the following steps:

[0012] S1-1, adding graphene oxide to 4-amino-N-methylbenzamide and stirring evenly to obtain a mixed solution for later use;

[0013] S1-2, the mixed solution is pressurized to 2Mpa-4Mpa, allowed to stand for treatment, and then centrifuged to obtain the precipitate to obtain modified graphene oxide.

[0014] Preferably, in step S1-2, the standing treatment time is 2h-4h, the centrifugal speed is 3200r / min-4500r / min, and the centrifugal time is 8min-12min.

[0015] Preferably, the preparation method of the modified fiber powder comprises the following steps:

[0016] S2-1, grinding the plant fiber through a 200-mesh sieve, and then performing a steam explosion treatment to obtain pretreated plant fiber for later use;

[0017] S2-2, after controlling the moisture content of the pretreated plant fiber to ≤ 20%, subjecting the pretreated plant fiber to microwave drying at 100°C-110°C to obtain a shaped powder for later use;

[0018] S2-3. Add the above-mentioned shaped powder into deionized water for ultrasonic vibration, then add nano titanium dioxide, place in a high-pressure reactor and increase the pressure to 0.4Mpa-0.6Mpa, stir for 20min-30min, centrifuge and dry to obtain modified fiber powder.

[0019] Preferably, in step S2-1, the steam explosion treatment temperature is 119°C-121°C, the treatment pressure is 0.4Mpa-0.6Mpa, and the treatment time is 30s-40s.

[0020] Preferably, the microwave drying and shaping time in step S2-2 is 30s-40s.

[0021] Preferably, in step S2-3, the ultrasonic oscillation power is 400W-600W, and the ultrasonic oscillation time is 10min-15min, and the subsequent centrifugal speed is 5000r / min-8000r / min, and the centrifugal time is 5min-10min.

[0022] Preferably, the amount of nano-titanium dioxide added in step S2-3 is 20%-40% of the total mass of the shaped powder.

[0023] The method for preparing the antistatic polycaprolactam composite material comprises the following steps:

[0024] (1) Add caprolactam, deionized water, phosphoric acid and acetic acid into a reaction kettle, replace the air in the reaction kettle with nitrogen, and then continue to increase the pressure to 0.4Mpa-0.6Mpa and stir to obtain a first mixed solution for standby use;

[0025] (2) Mixing nano zinc oxide, carbon nanotubes, modified graphene oxide, and modified fiber powder, adding them to deionized water and ultrasonically dispersing them uniformly to obtain a second mixed solution for later use;

[0026] (3) adding the second mixed liquid into the first mixed liquid, maintaining the pressure at 0.4Mpa-0.6Mpa and stirring evenly, then heating to 160°C-180°C for prepolymerization for 40min-60min to obtain the first prepolymer for standby use;

[0027] (4) Continue stirring to control the water content of the first prepolymer to be 2%-5%, then restore the pressure to normal and cool to 50°C-80°C, let stand for 20min-40min, and obtain the pretreated mixture for use;

[0028] (5) Rapidly heating the pretreated mixture to 240°C-260°C, stirring and polymerizing at normal pressure for 120min-160min, and obtaining a second prepolymer for standby use;

[0029] (6) The second prepolymer is subjected to a pressure-raising and standing treatment, and is allowed to continue to react at pressures of 0.2 MPa-0.4 MPa, 0.8 MPa-1.2 MPa, and 2 MPa-4 MPa, respectively, to obtain an antistatic polycaprolactam composite material.

[0030] Preferably, the amount of deionized water added in step (1) is 5%-10% of the total mass of caprolactam, and the subsequent stirring speed is 400r / min-800r / min, and the stirring time is 10min-20min.

[0031] Preferably, the amount of deionized water added in step (2) is 3-5 times the volume of the total substance after mixing the nano zinc oxide, carbon nanotubes, modified graphene oxide and modified fiber powder.

[0032] Preferably, in step (3), the pressure-maintaining stirring speed is 1200 r / min-1600 r / min, and the stirring time is 5 min-10 min.

[0033] Preferably, in step (5), the rapid heating rate is 20°C / min-30°C / min, and the stirring speed at normal pressure is 80r / min-120r / min.

[0034] Preferably, in step (6), the standing time at a pressure of 0.2 MPa-0.4 MPa is 20 min-30 min, the standing time at a pressure of 0.8 MPa-1.2 MPa is 40 min-60 min, and the standing time at a pressure of 2 MPa-4 MPa is 10 min-20 min.

[0035] The application method of the antistatic polycaprolactam composite material in preparing textile fibers is to extract the antistatic polycaprolactam composite material with boiling water for 40 minutes to 60 minutes, dry it to make slices, and then spin it into fibers and shape it.

[0036] The present invention provides an antistatic polycaprolactam composite material and a preparation method thereof, which has the advantages over the prior art in that:

[0037] (1) The present invention adopts an in-situ polymerization method to compound materials such as nano zinc oxide, carbon nanotubes, modified graphene oxide, and modified fiber powder into the polycaprolactam polymer structure, which can achieve permanent antistatic properties of the material, and the overall amount of auxiliary materials added is small, which has little interference on the color of the subsequent polycaprolactam fiber, and achieves a better dyeing effect after subsequent weaving.

[0038] (2) The present invention uses modified graphene oxide and modified fiber powder for in-situ polymerization, which effectively improves the antistatic effect of the material while further ensuring the mechanical properties of the material. The modified fiber powder is composited with nano-titanium dioxide after steam explosion modification and microwave shaping, which effectively improves the antistatic property while ensuring the mechanical stability and chemical control property of subsequent spinning. DETAILED DESCRIPTION

[0039] In order to make the purpose, advantages and technical solutions of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1:

[0040] Preparation of antistatic polycaprolactam composite materials:

[0041] 1. Preparation of modified graphene oxide:

[0042] (1) adding graphene oxide to 3 times the volume of 4-amino-N-methylbenzamide and stirring evenly to obtain a mixed solution;

[0043] (2) The mixed solution was pressurized to 3 MPa, allowed to stand for 3 h, and then centrifuged at 4000 r / min for 10 min to obtain the precipitate to obtain modified graphene oxide.

[0044] 2. Preparation of modified fiber powder:

[0045] (1) Ramie fiber was taken as the experimental plant fiber, ground through a 200-mesh sieve, then pressurized to 0.5 MPa, and steam-exploded at 120°C for 40 seconds to obtain steam-exploded plant fiber powder;

[0046] (2) drying the steam-exploded plant fiber powder at 45° C. to a moisture content of ≤20%, and then subjecting the powder to microwave drying at 110° C. for 30 seconds to obtain a plant fiber shaped powder;

[0047] (3) The above-mentioned shaping powder was added into deionized water at a material-liquid ratio of 1:8, and ultrasonically vibrated at 400 W for 15 minutes, and then 30% of the total mass of the shaping powder was added with nano-titanium dioxide (30nm-80nm), and the mixture was placed in a high-pressure reactor and the pressure was increased to 0.4Mpa-0.6Mpa and stirred for 20min-30min, and then centrifuged at a speed of 6000r / min for 10min, and then dried at a constant temperature of 65°C to constant weight to obtain a modified fiber powder;

[0048] 3. Preparation of antistatic polycaprolactam composite materials:

[0049] (1) caprolactam, deionized water (8% by mass of caprolactam), phosphoric acid and acetic acid are injected into a reactor together, and the air in the reactor is replaced with nitrogen gas with a purity of ≥99.9%, and then the pressure is increased to 0.5 MPa and stirred at 500 r / min for 15 min to obtain a first mixed solution;

[0050] (2) Add nano zinc oxide (30nm-80nm), carbon nanotubes (length 100nm-500nm, tube diameter 5nm-15nm), modified graphene oxide, and fiber powder to 4 times the total volume of deionized water, and disperse them under 400W ultrasonic dispersion for 15 minutes to obtain a second mixed solution;

[0051] (3) adding the second mixed liquid into the first mixed liquid and maintaining the pressure at 0.5 MPa, stirring at a speed of 1500 r / min for 5 min, and then heating to 170° C. for prepolymerization for 50 min to obtain a first prepolymer for standby use;

[0052] (4) Continue stirring to control the water content of the first prepolymer to 4%, then restore the pressure to normal and cool to 60°C, let stand for 30 minutes, and obtain the pretreated mixture for use;

[0053] (5) The pretreated mixture was rapidly heated to 250°C at a heating rate of 25°C / min, and the mixture was stirred at a speed of 100 r / min for polymerization for 140 min to obtain a second prepolymer for standby use;

[0054] (6) The second prepolymer is pressurized to 0.3 MPa and allowed to stand for 20 min, then to 1 MPa and allowed to stand for 50 min, and finally to 3 MPa and allowed to stand for 15 min to obtain an antistatic polycaprolactam composite material.

[0055] Referring to the above preparation method, different experimental groups were set according to the selection of fiber powder and the weight of each component in Table 1 below:

[0056] Table 1

[0057]

[0058] Comparative Example 1:

[0059] Preparation of antistatic polycaprolactam composite materials:

[0060] (1) Prepare the following materials in parts by weight: 100 parts of caprolactam, 0.1 parts of nano zinc oxide, 0.5 parts of carbon nanotubes, 0.8 parts of modified graphene oxide, 1.15 parts of plant fiber shaping powder, 0.35 parts of nano titanium dioxide (30nm-80nm), 0.2-0.6 parts of phosphoric acid, and 0.2 parts of acetic acid;

[0061] (2) caprolactam, deionized water (8% by mass of caprolactam), phosphoric acid and acetic acid are injected into a reactor together, and the air in the reactor is replaced with nitrogen gas with a purity of ≥99.9%, and then the pressure is increased to 0.5 MPa and stirred at 500 r / min for 15 min to obtain a first mixed solution;

[0062] (3) Add nano zinc oxide, carbon nanotubes, modified graphene oxide, plant fiber shaping powder, and nano titanium dioxide to deionized water 4 times the total volume, and disperse them under 400W ultrasonic dispersion for 15 minutes to obtain a second mixed solution;

[0063] (4) adding the second mixed liquid into the first mixed liquid and maintaining the pressure at 0.5 MPa, stirring at a speed of 1500 r / min for 5 min, and then heating to 170° C. for prepolymerization for 50 min to obtain a first prepolymer for standby use;

[0064] (5) Continue stirring to control the water content of the first prepolymer to 4%, then restore the pressure to normal and cool to 60°C, let stand for 30 minutes, and obtain the pretreated mixture for use;

[0065] (6) The pretreated mixture was rapidly heated to 250°C at a heating rate of 25°C / min, and the mixture was stirred at a speed of 100 r / min for polymerization for 140 min to obtain a second prepolymer for standby use;

[0066] (7) The second prepolymer is pressurized to 0.3 MPa and allowed to stand for 20 min, then to 1 MPa and allowed to stand for 50 min, and finally to 3 MPa and allowed to stand for 15 min to obtain an antistatic polycaprolactam composite material.

[0067] Comparative Example 2:

[0068] Referring to the raw material ratio of the experimental group 1 in the above embodiment 1, the antistatic polycaprolactam composite material was prepared by the following method. The specific preparation method is as follows:

[0069] (1) caprolactam, deionized water (8% by mass of caprolactam), phosphoric acid and acetic acid are injected into a reactor together, the air in the reactor is replaced with nitrogen with a purity of ≥99.9%, the pressure is continuously increased to 0.5 MPa, and then stirred at 500 r / min for 15 min to obtain a first mixed solution;

[0070] (2) Add nano zinc oxide (30nm-80nm), carbon nanotubes (length 100nm-500nm, tube diameter 5nm-15nm), modified graphene oxide, and modified fiber powder to deionized water 4 times the total volume, and disperse them at 400W ultrasonic for 15 minutes to obtain a second mixed solution;

[0071] (3) adding the second mixed liquid into the first mixed liquid and maintaining the pressure at 0.5 MPa, stirring at a speed of 1500 r / min for 5 min, and then heating to 170° C. for prepolymerization for 50 min to obtain a first prepolymer for standby use;

[0072] (4) Continue stirring to control the water content of the first prepolymer to 4%, then restore the pressure to normal and cool to 60°C, let stand for 30 minutes, and obtain the pretreated mixture for use;

[0073] (5) The pretreated mixture was rapidly heated to 250°C at a heating rate of 25°C / min, and the mixture was stirred at a speed of 100 r / min for polymerization for 140 min to obtain a second prepolymer for standby use;

[0074] (6) The second prepolymer was pressurized and allowed to stand according to Table 2 below to prepare different groups of antistatic polycaprolactam composite materials:

[0075] Table 2

[0076]

[0077] Comparative Example 3:

[0078] Referring to the raw material ratio of the experimental group 1 in the above embodiment 1, the antistatic polycaprolactam composite material was prepared by the following method. The specific preparation method is as follows:

[0079] (1) caprolactam, deionized water (8% by mass of caprolactam), phosphoric acid and acetic acid are injected into a reactor together, the air in the reactor is replaced with nitrogen with a purity of ≥99.9%, the pressure is continuously increased to 0.5 MPa, and then stirred at 500 r / min for 15 min to obtain a first mixed solution;

[0080] (2) Add nano zinc oxide (30nm-80nm), carbon nanotubes (length 100nm-500nm, tube diameter 5nm-15nm), modified graphene oxide, and modified fiber powder to deionized water 4 times the total volume, and disperse them at 400W ultrasonic for 15 minutes to obtain a second mixed solution;

[0081] (3) adding the second mixed solution into the first mixed solution and heating the mixture to 170° C. to carry out prepolymerization for 50 minutes to obtain a first prepolymer for later use;

[0082] (4) Continue stirring to control the water content of the first prepolymer to 4%, then raise the temperature to 250°C, stir at a speed of 100 r / min and perform polymerization reaction at normal pressure for 140 min to obtain a second prepolymer for standby use;

[0083] (5) The second prepolymer is pressurized to 0.3 MPa and allowed to stand for 20 min, then to 1 MPa and allowed to stand for 50 min, and finally to 3 MPa and allowed to stand for 15 min, to obtain an antistatic polycaprolactam composite material.

[0084] Detection:

[0085] The properties of the antistatic polycaprolactam composite materials prepared in the above experimental groups and comparative examples were tested:

[0086] 1. Test the antistatic properties of the above groups of materials:

[0087] After the preparation, each group of materials was placed in an environment with a humidity of 30% and a temperature of 22°C for 0 days, 10 days and 30 days. The surface resistance of the polycaprolactam composite materials prepared in each group was tested and the resistance value at each placement time was recorded (the resistance value was 10 6 -10 12 Belong to antistatic), the specific results are shown in Table 3 below:

[0088] Table 3

[0089]

[0090] It can be seen from the above table that experimental group 1, experimental group 2 and comparative example 3 have good antistatic effect and antistatic stability.

[0091] 2. Detect the relative viscosity and oligomer content of each group of antistatic polycaprolactam composite materials:

[0092] (1) Relative viscosity test: According to GB / T 38138 standard test, weigh each group of samples and dissolve them in concentrated sulfuric acid (96%) to make a 0.01 g / mL test solution. Use an Ubbelohde viscometer to test at 25°C, record the outflow time t, and calculate the viscosity of the sample: η=t / t0; where t0 is the outflow time of pure concentrated sulfuric acid;

[0093] (2) Oligomer content detection: According to GB / T 38138 standard, first dry each group of samples in a vacuum drying oven at 120±2℃ for 8h, then weigh 20g of each group and extract in hot water above 97℃ for 8h, then take out and dry in a vacuum drying oven at 120±2℃ to constant weight, record the weight as m1, and calculate the oligomer content based on the mass before and after extraction: oligomer content% = (20-m1) / 20×100%.

[0094] The specific test results are shown in Table 4 below:

[0095] Table 4

[0096]

[0097] It can be seen from the above table that experimental group 1 and experimental group 2 have better viscosity and lower oligomer content.

[0098] 3. Mechanical properties test of the spinning prepared by the above groups of antistatic polycaprolactam composite materials:

[0099] Preparation for spinning: Each group of antistatic polycaprolactam composite materials was extracted in boiling water for 50 minutes, dried and sliced, and then spun using a spinning machine (VC406B), and the spinneret specifications used were: 0.3mm×36f, the spinning speed was 800m / min, and the primary fibers obtained after spinning were stretched using a drawing machine (VC443A), and the drawing speed was 1000m / min. The specific spinning parameters are shown in Table 5 below:

[0100] Table 5

[0101]

[0102] The obtained groups of spun fibers were subjected to the following tests:

[0103] (1) The single yarn strength tester YG020B was used for testing according to GB / T 14344 standard, with a tensile speed of 350 mm / min, a clamping distance of 500 mm, and a pre-tension of 5 cN. Five groups of valid data were obtained for each group of samples, and the average value was taken. The specific results are shown in Table 6 below.

[0104] Table 6

[0105]

[0106] It can be seen from the above table that experimental group 1 and experimental group 2 have higher mechanical properties.

[0107] 4. Detect the dye uptake (D) of the fibers prepared from the antistatic polycaprolactam composite materials of each group: soak the fibers prepared from each group in acid scarlet GR dye with a pH value of 4, dye them for 100 min at constant temperatures of 75°C, 85°C, and 95°C, then take them out and use a UV-2006 ultraviolet-visible spectrophotometer to measure the absorbance of the dye solution before and after dyeing, and calculate D according to the following formula:

[0108] D = (1-mA1 / nA0)×100%;

[0109] Wherein: n and m are the dilution multiples of the dye solution before and after dyeing; A0 and A1 are the absorbances of the dye solution before and after dyeing, respectively. The specific results are shown in Table 7 below:

[0110] Table 7

[0111]

[0112] As can be seen from the above table, adding fiber powder can effectively improve the dyeing rate of the material, and experimental group 1, experimental group 2 and comparative example 1 all have high dyeing rates.

[0113] Through all the above tests, it can be seen that the antistatic polycaprolactam composite materials prepared by the preparation process and raw material ratio of experimental group 1 and experimental group 2 have the highest comprehensive performance and are suitable for batch and large-scale production.

[0114] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An antistatic polycaprolactam composite material, characterized in that: The antistatic polycaprolactam composite material comprises the following raw materials in parts by weight: 100-120 parts of caprolactam, 0.1-0.4 parts of nano zinc oxide, 0.5-1.0 parts of carbon nanotubes, 0.8-1.2 parts of modified graphene oxide, 1.5-2.5 parts of modified fiber powder, 0.2-0.6 parts of phosphoric acid, and 0.2-0.4 parts of acetic acid; The modified graphene oxide is obtained by treating graphene oxide with 4-amino-N-methylbenzamide as a modifier; The modified fiber powder is prepared by steam explosion treatment of plant fiber powder, microwave shaping, and then mixing with nano-titanium dioxide for modification. The preparation method of the modified fiber powder includes the following steps: S2-1, grinding the plant fiber through a 200-mesh sieve, and then performing a steam explosion treatment to obtain pretreated plant fiber for later use; S2-2, after controlling the moisture content of the pretreated plant fiber to ≤ 20%, subjecting the pretreated plant fiber to microwave drying at 100°C-110°C to obtain a shaped powder for later use; S2-3. Add the above-mentioned shaped powder into deionized water for ultrasonic vibration, then add nano titanium dioxide, place in a high-pressure reactor, increase the pressure to 0.4Mpa-0.6Mpa, stir for 20min-30min, centrifuge and dry to obtain modified fiber powder.

2. The antistatic polycaprolactam composite material according to claim 1, characterized in that: The length of the carbon nanotube is 100nm-500nm, and the diameter of the carbon nanotube is 5nm-15nm.

3. The antistatic polycaprolactam composite material according to claim 1, characterized in that: The particle size of the nano zinc oxide is 30nm-80nm.

4. The antistatic polycaprolactam composite material according to claim 1, characterized in that: The preparation method of the modified graphene oxide comprises the following steps: S1-1, adding graphene oxide to 4-amino-N-methylbenzamide and stirring evenly to obtain a mixed solution for later use; S1-2, the mixed solution is pressurized to 2Mpa-4Mpa, allowed to stand for treatment, and then centrifuged to obtain the precipitate to obtain modified graphene oxide.

5. The antistatic polycaprolactam composite material according to claim 4, characterized in that: The standing time in step S1-2 is 2h-4h, the centrifugal speed is 3200r / min-4500r / min, and the centrifugal time is 8min-12min.

6. The antistatic polycaprolactam composite material according to claim 1, characterized in that: In the step S2-1, the steam explosion treatment temperature is 119°C-121°C, the treatment pressure is 0.4Mpa-0.6Mpa, and the treatment time is 30s-40s.

7. The antistatic polycaprolactam composite material according to claim 1, characterized in that: The microwave drying and shaping time in step S2-2 is 30s-40s.

8. The antistatic polycaprolactam composite material according to claim 1, characterized in that: In step S2-3, the ultrasonic oscillation power is 400W-600W, and the ultrasonic oscillation time is 10min-15min, and the subsequent centrifugal speed is 5000r / min-8000r / min, and the centrifugal time is 5min-10min.

9. The antistatic polycaprolactam composite material according to claim 1, characterized in that: In step S2-3, the amount of nano titanium dioxide added is 20%-40% of the total mass of the shaped powder.

10. A method for preparing the antistatic polycaprolactam composite material according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: (1) Add caprolactam, deionized water, phosphoric acid and acetic acid into a reactor together, replace the air in the reactor with nitrogen, and then continue to increase the pressure to 0.4Mpa-0.6Mpa and stir to obtain a first mixed solution for standby use; (2) Mixing nano zinc oxide, carbon nanotubes, modified graphene oxide, and modified fiber powder, adding them to deionized water and ultrasonically dispersing them uniformly to obtain a second mixed solution for later use; (3) adding the second mixed liquid into the first mixed liquid, maintaining the pressure at 0.4Mpa-0.6Mpa and stirring evenly, then heating to 160°C-180°C for prepolymerization for 40min-60min to obtain the first prepolymer for standby use; (4) Continue stirring to control the water content of the first prepolymer to be 2%-5%, then restore the pressure to normal and cool to 50℃-80℃, let stand for 20min-40min, and obtain the pretreated mixture for use; (5) Rapidly heating the pretreated mixture to 240°C-260°C, stirring and polymerizing at normal pressure for 120min-160min, and obtaining a second prepolymer for standby use; (6) The second prepolymer is subjected to a pressure-raising and standing treatment, and is allowed to continue to react at pressures of 0.2 MPa-0.4 MPa, 0.8 MPa-1.2 MPa, and 2 MPa-4 MPa, respectively, to obtain an antistatic polycaprolactam composite material, wherein the standing time at a pressure of 0.2 MPa-0.4 MPa is 20 min-30 min, the standing time at a pressure of 0.8 MPa-1.2 MPa is 40 min-60 min, and the standing time at a pressure of 2 MPa-4 MPa is 10 min-20 min.

11. The preparation method according to claim 10, characterized in that: In the step (1), the amount of deionized water added is 5%-10% of the total mass of caprolactam, and the subsequent stirring speed is 400r / min-800r / min, and the stirring time is 10min-20min.

12. The preparation method according to claim 10, characterized in that: In the step (2), the amount of deionized water added is 3 to 5 times the volume of the total substance after the nano zinc oxide, carbon nanotubes, modified graphene oxide and modified fiber powder are mixed.

13. The preparation method according to claim 10, characterized in that: In the step (3), the pressure-maintaining stirring speed is 1200 r / min-1600 r / min, and the stirring time is 5 min-10 min.

14. The preparation method according to claim 10, characterized in that: In the step (5), the rapid heating rate is 20°C / min-30°C / min, and the stirring speed at normal pressure is 80r / min-120r / min.

15. Use of the antistatic polycaprolactam composite material according to any one of claims 1 to 9 in preparing textile fibers.

16. The use according to claim 15, characterized in that: The application method comprises the following steps: extracting the antistatic polycaprolactam composite material with boiling water for 40 minutes to 60 minutes, drying and slicing the composite material, and then spinning and shaping the composite material.

Citation Information

Cited By

  • A low-addition-amount synergistically reinforced multifunctional PA6 composite material and its preparation method

    CN123107346A