Polyurethane rheology modifier for imparting water resistance to paint film, polyurethane coating and preparation method thereof

The polyurethane rheology modifier, combining modified hydroxypropyl methylcellulose and polymer with nano zinc oxide, addresses sagging and water resistance issues, enhancing adhesion and providing self-repair and antibacterial capabilities in polyurethane coatings.

CN118460034BActive Publication Date: 2024-12-03ANHUI BONA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410931510.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-12-03
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Existing polyurethane coatings face issues with sagging, water resistance, and weather resistance in harsh environments, and there is a need for improved antibacterial properties.

Method used

A polyurethane rheology modifier is developed using modified hydroxypropyl methylcellulose and a modified polymer, forming a semi-interpenetrating network structure with long-chain alkyl or alkenyl groups and loaded nano zinc oxide, enhancing adhesion and hydrophobicity, and incorporating active groups for self-repair and bactericidal properties.

Benefits of technology

The modified polyurethane coating exhibits improved sagging performance, hydrophobicity, water resistance, and antibacterial properties, with the ability to self-repair and maintain integrity under stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460034B_ABST
    Figure CN118460034B_ABST
Patent Text Reader

Abstract

The invention provides a polyurethane rheology modifier for imparting water resistance to a paint film, a polyurethane coating and a preparation method thereof. The polyurethane rheology modifier comprises modified hydroxypropyl methylcellulose and a modified polymer in a mass ratio of (1-1.5):1; the polyurethane coating comprises: 60-100 parts by weight of waterborne polyurethane, 5-10 parts by weight of the polyurethane rheology modifier and 1-3 parts by weight of a photoinitiator; the sag performance, hydrophobicity, viscosity and antibacterial performance of the sag modifier can be greatly improved by combining the modified hydroxypropyl methylcellulose and the modified polymer; the polyurethane rheology modifier is added to the polyurethane coating, and the coating is further cross-linked under the action of a photoinitiator, thereby further increasing the anti-sag performance and self-repairing performance to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings and relates to a polyurethane rheology modifier for imparting water resistance to a paint film, a polyurethane coating and a preparation method thereof. Background Art

[0002] Polyurethanes have excellent durability and can withstand daily use and environmental erosion. They can resist chemicals, UV radiation, humidity, abrasion and scratches, thus protecting the substrate from damage. Their excellent physical properties, including high hardness, high strength, high toughness and impact resistance, enable the coating film to withstand various stresses and deformations while maintaining its integrity and performance. Polyurethane coatings can adhere well to various substrates, including metal, plastic, wood and concrete. They can form a strong coating film structure, providing reliable waterproof protection and decorative effects.

[0003] The patent with publication number CN114644880A discloses a two-component polyurethane fire retardant coating, a preparation method and application thereof, wherein component A includes 30-50% polyether polyol, 2-10% nonlinear small molecule chain extender, 0.5-2% polyether amine, 10-20% expanded graphite, 5-15% ammonium polyphosphate, 5-15% melamine, 10-25% aluminum hydroxide, 0.2-2% water absorbent, 0.2-2% silane coupling agent, and 0.01-1% catalyst; component B is a polyisocyanate component; the fire retardant coating provided by the invention improves the anti-sagging performance and flexibility of the product to a certain extent, but its sagging performance still needs to be improved.

[0004] At present, some problems may occur in the use of coatings, such as sagging problems, water resistance and weather resistance in harsh environments, etc. Therefore, it is very necessary to develop a new type of polyurethane coating. Summary of the invention

[0005] The present invention aims to provide a polyurethane rheology modifier for imparting water resistance to a paint film, a polyurethane coating and a preparation method thereof. By modifying hydroxypropyl methylcellulose and a modified polymer combination, firstly, after modification, both have good compatibility and dispersibility, so that both can be well dispersed in a matrix material, and can be fully mixed, and promote each other to facilitate better performance; secondly, both are network structures, and after being fully mixed, it is easy to form a semi-interpenetrating network structure, and have long-chain alkyl or alkenyl groups, which interpenetrate and entangle with each other, so that the semi-interpenetrating network structure is more tightly aggregated, forming a lower porosity, which will limit the flow of fluid, and there are unfilled 3d orbitals in the loaded nano zinc oxide, which can interact with the fluid molecular orbitals to enhance the adhesion, thereby further increasing the sagging performance and hydrophobic performance; furthermore, after modification, the network structure surface has a large number of hydroxyl groups. , thiol, amino and other active groups, and the hydrogen bonds and van der Waals forces between the active groups are used to facilitate the further formation of the semi-interpenetrating network structure. On the premise of further increasing the sag performance and hydrophobic performance, it can also facilitate the subsequent application in the coating to form a self-repair of the paint film; in addition, nano zinc oxide can slowly release zinc ions in the water-based coating matrix. The bacterial surface is negatively charged due to the presence of free carboxyl groups, so that it can be adsorbed to the bacterial surface, causing damage to the cell wall. The hydroxyl groups on the surface of the network structure can react with the thiol and amino groups in the protein, so that the permeability of the cell membrane is further increased, so that the cells quickly lose their biological functions, resulting in the outflow of bacterial cytoplasm, and achieving better bactericidal performance; the rheology modifier is added to the water-based polyurethane, and under the action of the photoinitiator, on the basis of ensuring water resistance and antibacterial properties, it can further cross-link to improve the anti-sag performance and self-repairing performance of the coating.

[0006] One of the purposes of the present invention is to provide a polyurethane rheology modifier for imparting water resistance to a paint film, wherein the polyurethane rheology modifier comprises modified hydroxypropyl methylcellulose and a modified polymer in a mass ratio of (1-1.5):1;

[0007] The preparation method of the modified hydroxypropyl methylcellulose comprises:

[0008] A1, uniformly mixing olefinated hydroxyapatite, hydroxypropyl methylcellulose, undecene aldehyde and deionized water, and then adding sodium dodecylbenzene sulfonate and ammonium persulfate to react to obtain substituted hydroxypropyl methylcellulose;

[0009] A2, dispersing zinc oxide in anhydrous ethanol to form a zinc oxide dispersion, and then immersing the substituted hydroxypropyl methylcellulose obtained in A1 in the zinc oxide dispersion to obtain modified hydroxypropyl methylcellulose;

[0010] The preparation method of the modified polymer comprises:

[0011] S1. Add oleic acid and N,N-dimethylpropylenediamine in a molar ratio of 1:1.1 to a mixed solution of acetone and ethanol, and react at 120-150°C (e.g., 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc.) in a nitrogen environment for 12-24 h (e.g., 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, etc.) to obtain an oleic acid amidopropyl dimethyl tertiary amine mixed solution;

[0012] S2, cooling the oleic acid amide propyl dimethyl tertiary amine mixed solution obtained in S1 to 80-90°C (e.g., 80°C, 82°C, 85°C, 87°C, 90°C, etc.), adding allyl chloride to react for 8-10 h (e.g., 8 h, 8.5 h, 9 h, 9.5 h, 10 h, etc.) to obtain a hydrophobic monomer;

[0013] S3. Add the hydrophobic monomer obtained in S2 to an acrylamide solution with a concentration of 20-40% (for example, 20%, 25%, 30%, 35%, 40%, etc.), add cocamidopropyl betaine as a dispersant, adjust the pH to 6.5-7 (for example, 6.5, 6, 8, 7, etc.), lower the reaction temperature, introduce nitrogen to deoxygenate for 30 minutes at 0-5°C (for example, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, etc.), use sodium formate as a chain transfer agent, continue to pass nitrogen for 2 minutes and then stop passing nitrogen, and react adiabatically for 6-8 hours (for example, 6 h, 6.5 h, 7h, 7.5 h, 8 h, etc.) to obtain a transparent rubber block, dry and grind it, and then extract and purify it with acetone-ethanol for 12-16 hours (for example, 12 h, 13 h, 14 h, 15 h, 16 h, etc.) to obtain a modified polymer.

[0014] In the present invention, by modifying the polymer, the polymer has better stability and smaller critical association concentration, and the molecules are more tightly aggregated to form a higher density network structure in the aqueous solution, which has better viscoelasticity, temperature resistance and water resistance.

[0015] In the present invention, hydroxyapatite, long-chain alkyl and aldehyde groups are introduced into hydroxypropyl methylcellulose for modification, and nano zinc oxide is loaded on its surface, thereby improving the rheological properties and water retention of hydroxypropyl methylcellulose and improving the hydrophobicity and antibacterial properties.

[0016] In the present invention, the modified polymer is introduced into acrylamide by a hydrophobic surfactant, and under the action of the dispersant cocamidopropyl betaine, its structure and properties are well controlled, so that it has good sagging performance and hydrophobic performance; the modified hydroxy cellulose is introduced into cellulose by hydroxyapatite, long-chain alkyl and aldehyde groups, and nano zinc oxide is loaded on its surface, so that it has good thickening, water retention, hydrophobic performance and bactericidal performance; by combining the two, firstly, the two are modified to have good compatibility and dispersibility, so that the two can be well dispersed in the matrix material, and can be fully mixed, and promote each other to better play the performance; secondly, both are network structures, and after being fully mixed, it is easy to form a semi-interpenetrating network structure, and the long-chain alkyl or alkenyl groups are interlaced and entangled with each other, so that the semi-interpenetrating network structure is more tightly aggregated, forming a lower porosity, which will limit the flow of the fluid, and There are unfilled 3d orbitals in the loaded nano zinc oxide, which can interact with the fluid molecular orbitals to enhance adhesion, thereby further increasing the sagging performance and hydrophobicity; furthermore, after the two are modified, the network structure surface has a large number of active groups such as hydroxyl, thiol, and amino groups, and the hydrogen bonds and van der Waals forces between the active groups are used to facilitate the further formation of the semi-interpenetrating network structure. On the premise of further increasing the sagging performance and hydrophobicity, it can also facilitate the subsequent application in the coating to form a paint film for self-repair; in addition, nano zinc oxide can slowly release zinc ions in the water-based coating matrix, and the bacterial surface is negatively charged due to the presence of free carboxyl groups, so that it can be adsorbed to the bacterial surface, causing damage to the cell wall, and the hydroxyl groups on the surface of the network structure can react with the thiol and amino groups in the protein, so that the permeability of the cell membrane is further increased, so that the cells quickly lose their biological functions, resulting in the outflow of bacterial cytoplasm, achieving better bactericidal performance.

[0017] Preferably, the preparation method of the olefinic hydroxyapatite comprises: uniformly mixing nano-hydroxyapatite, γ-methacryloxypropyltrimethoxysilane and ethanol, reacting at 60-70°C (for example, 60°C, 62°C, 65°C, 68°C, 70°C, etc.) for 5-8 h (for example, 5 h, 6 h, 7 h, 8 h, etc.) to obtain olefinic hydroxyapatite.

[0018] Preferably, based on 100 g of hydroxypropyl methylcellulose, the amount of olefinated hydroxyapatite added is 7-15 g (e.g., 7 g, 8 g, 9 g, 10 g, 11 g, 12 g, 13 g, 14 g, 15 g, etc.), the amount of undecylenic aldehyde added is 18-25 g (e.g., 18 g, 19 g, 20 g, 21 g, 22 g, 23 g, 24 g, 25 g, etc.), the amount of sodium dodecylbenzene sulfonate added is 8-11 g (e.g., 8 g, 9 g, 10 g, 11 g, etc.), the amount of ammonium persulfate added is 1.5-2 g (e.g., 1.5 g, 1.6 g, 1.7 g, 1.8 g, 1.9 g, 2 g, etc.), and the amount of deionized water added is 3500-3800 g (e.g., 3500 g, 3550 g, 3600 g, 3650 g, 3700 g). g, 3750 g, 3800 g, etc.).

[0019] Preferably, in step A1, the reaction temperature is 60-70°C (e.g., 60°C, 62°C, 65°C, 68°C, 70°C, etc.), and the reaction time is 3-5 h (e.g., 3 h, 3.5 h, 4 h, 4.5 h, 5 h, etc.).

[0020] Preferably, in step A2, the concentration of the zinc oxide dispersion is 10-30%, for example, 10%, 15%, 20%, 25%, 30%, etc.

[0021] Preferably, step A2 further comprises drying the impregnated material, wherein the drying is vacuum drying, the drying temperature is 40-80°C (e.g. 40°C, 50°C, 60°C, 70°C, 80°C, etc.), and the drying time is 4-10 h (e.g. 4 h, 6 h, 8 h, 10 h, etc.).

[0022] A second object of the present invention is to provide a method for preparing a polyurethane rheology modifier, the preparation method comprising: mixing modified hydroxypropyl methylcellulose and a modified polymer in a mass ratio of (1-1.5):1 (e.g., 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, etc.) to obtain a polyurethane rheology modifier.

[0023] The third object of the present invention is to provide a polyurethane coating, which comprises, by weight:

[0024] 60-100 parts of waterborne polyurethane (for example, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, 95 parts, 100 parts, etc.), 5-10 parts of polyurethane rheology modifier (for example, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.) and 1-3 parts of photoinitiator (for example, 1 part, 2 parts, 3 parts, etc.).

[0025] Preferably, the photoinitiator includes photoinitiator 1173 or photoinitiator 184.

[0026] The fourth object of the present invention is to provide a method for preparing a polyurethane coating as described in the third object, the preparation method comprising: the preparation method comprising: stirring 60-100 parts by weight of aqueous polyurethane and 5-10 parts by weight of a polyurethane rheology modifier once, and then adding 1-3 parts by weight of a photoinitiator and stirring for a second time to obtain a polyurethane coating.

[0027] In the present invention, waterborne polyurethane is used as a base material of the coating and has good basic properties; the rheology modifier has good rheology, hydrophobicity and bactericidal properties; the photoinitiator has photoinitiating properties; the polyurethane rheology modifier is added to the waterborne polyurethane to make it uniformly dispersed in the waterborne polyurethane, and after the photoinitiator is added, under the action of the photoinitiator, the waterborne polyurethane and the polyurethane rheology modifier can be further cross-linked to achieve further cross-linking of the network structure, thereby further increasing the anti-sagging performance and self-repairing performance on the basis of ensuring water resistance and antibacterial properties.

[0028] Preferably, the stirring rate is 1500-2000 r / min (e.g., 1500 r / min, 1600 r / min, 1700 r / min, 1800 r / min, 1900 r / min, 2000 r / min, etc.), and the stirring time is 0.5-1h (e.g., 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, etc.).

[0029] The secondary stirring rate is 1500-2000 r / min (e.g., 1500 r / min, 1600 r / min, 1700 r / min, 1800 r / min, 1900 r / min, 2000 r / min, etc.), and the secondary stirring time is 1-4 h (e.g., 1 h, 2 h, 3 h, 4 h, etc.).

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] In the present invention, by combining the modified polymer and the modified hydroxypropyl methylcellulose, firstly, after modification, both have good compatibility and dispersibility, so that both can be well dispersed in the matrix material, and can be fully mixed, and promote each other to better exert the performance; secondly, both are network structures, and after being fully mixed, it is easy to form a semi-interpenetrating network structure, and the long-chain alkyl or alkenyl groups are interlaced and entangled with each other, so that the semi-interpenetrating network structure is more tightly aggregated, forming a lower porosity, which will limit the flow of the fluid, and the unfilled 3d orbital in the loaded nano zinc oxide can interact with the fluid molecular orbital to enhance the adhesion, thereby further increasing the sagging performance and hydrophobic performance; furthermore, the two are modified. After modification, the surface of the network structure has a large number of active groups such as hydroxyl, thiol, and amino groups. The hydrogen bonds and van der Waals forces between the active groups facilitate the further formation of the semi-interpenetrating network structure. On the premise of further increasing the sagging performance and hydrophobicity, it can also facilitate the subsequent application in the coating to form a self-repair of the paint film; in addition, nano zinc oxide can slowly release zinc ions in the water-based coating matrix. The surface of bacteria is negatively charged due to the presence of free carboxyl groups, so that it can be adsorbed on the surface of bacteria, causing damage to the cell wall. The hydroxyl groups on the surface of the network structure can react with the thiol and amino groups in the protein, so that the permeability of the cell membrane is further increased, so that the cells quickly lose their biological functions, resulting in the outflow of bacterial cytoplasm, and achieving better bactericidal performance. The rheology modifier is added to the waterborne polyurethane, and under the action of the photoinitiator, it can be further cross-linked, and on the basis of ensuring water resistance and antibacterial properties, the anti-rheological properties and self-repairing properties of the coating are further increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a scanning electron microscope image of the material prepared in Preparation Example 1, with a scale of 100 microns;

[0033] Figure 2 This is a contact angle measurement diagram of the hydrophobic performance test of the polyurethane coating prepared in Example 1;

[0034] Figure 3 Schematic diagram of the antibacterial performance test of the polyurethane coating prepared in Example 1. DETAILED DESCRIPTION

[0035] It should be noted that the following detailed descriptions are all exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those generally understood by those of ordinary skill in the art to which the present invention belongs. The technical scheme of the present invention is further illustrated below by specific embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0036] The brands, manufacturers and other information of the main chemical reagents used in the examples and comparative examples of the present invention are as follows:

[0037] Nanohydroxyapatite, Beijing Daojin Technology Co., Ltd.; γ-methacryloxypropyltrimethoxysilane, McLean; hydroxypropyl methylcellulose, McLean; undecenal, McLean; sodium dodecylbenzene sulfonate, Shanghai Shengzhong Fine Chemical Co., Ltd.; ammonium persulfate, Shanghai Aladdin Biochemical Technology Co., Ltd.; nano zinc oxide, Beijing Daojin Technology Co., Ltd.; waterborne polyurethane, McLean; photoinitiator 184, Shanghai Guangyi Chemical Co., Ltd.; the materials in Preparation Example 2 were provided by the original author after contacting him / her.

[0038] Preparation Example 1

[0039] This preparation example provides a method for preparing modified hydroxypropyl methylcellulose, comprising:

[0040] A1. Mix nano-hydroxyapatite, γ-methacryloxypropyltrimethoxysilane and 75% ethanol aqueous solution in a mass ratio of 100:85:3200, heat, react at 60°C for 8 hours, centrifuge at a speed of 6000 r / min for 8 minutes after the reaction, wash with anhydrous ethanol, and vacuum dry at 60°C for 6 hours to obtain olefinated hydroxyapatite;

[0041] A2, olefinated hydroxyapatite, hydroxypropyl methylcellulose, undecene aldehyde and deionized water are mixed evenly, and then sodium dodecylbenzene sulfonate and initiator ammonium persulfate are added, and stirred to mix, wherein the mass ratio of olefinated hydroxyapatite, hydroxypropyl methylcellulose, undecene aldehyde, deionized water, sodium dodecylbenzene sulfonate and initiator ammonium persulfate is 7:100:18:3500:8:1.5, react at 60°C for 3h, and after the reaction is completed, centrifuge at a speed of 5000r / min for 6min, and vacuum dry at 60°C for 6h to obtain unloaded modified hydroxypropyl methylcellulose;

[0042] A3. Disperse nano zinc oxide in anhydrous ethanol to form a zinc oxide dispersion with a mass fraction of 20%, immerse unloaded modified hydroxypropyl methylcellulose in the zinc oxide dispersion at a solid-liquid ratio of 1:20, immerse for 1 h, filter and dry to obtain modified hydroxypropyl methylcellulose.

[0043] Figure 1 The scanning electron microscope image of the modified hydroxypropyl methylcellulose shows that nano zinc oxide is loaded on the surface of the substituted hydroxypropyl methylcellulose.

[0044] Preparation Example 2

[0045] This preparation example provides a method for preparing a modified polymer, referring to the literature on the polymerization mechanism and rheological properties of micelle-modified hydrophobic associating polymers, and includes the following steps:

[0046] B1. Using acetone-ethanol as solvent, n(OA):n(DMAPA)=1:1.1, the amount of catalyst substance is 0.1 mmol, react at 120℃, N2 protection conditions for 12h, and obtain the intermediate oleic acid amidopropyl dimethyl tertiary amine (PKO). Cool the system to 80℃ for the next step of ammonium salt reaction, add allyl chloride (AC) to the system with a dropping funnel and continue to react for 8h, remove the solvent in the system with a rotary evaporator, and obtain the reactive functional surfactant monomer KS-3.

[0047] B2. Prepare a 30% mass fraction AM solution, add the reactive functional surfactant monomer KS-3, use cocamidopropyl betaine as the KS-3 dispersant, adjust the system pH to 6.5-7, lower the system temperature, deoxygenate with nitrogen at 0-5°C for 30 min, use sodium formate as the chain transfer agent, adopt a redox initiation system, m(HCOONa): m(APS): m(Vc): m(AIBN)=3:4:6:3, continue to pass nitrogen for 2 min and then stop passing nitrogen, react adiabatically for 6 h to obtain a transparent rubber block, dry and crush it, extract and purify it with acetone-ethanol for 12 h, and dry it at 75°C to obtain a modified polymer.

[0048] Example 1

[0049] The present embodiment provides a polyurethane coating, including 90 parts by weight of water-based polyurethane, 7.5 parts by weight of a polyurethane rheological agent, and 2.5 parts by weight of a photoinitiator 184. The mass ratio of modified hydroxypropyl methylcellulose to modified polymer in the polyurethane rheological agent is 1.5:1, and the modified hydroxypropyl methylcellulose and modified polymer are prepared by Preparation Example 1-2.

[0050] This embodiment also provides a method for preparing a polyurethane coating, comprising:

[0051] 90 parts by weight of aqueous polyurethane, 5 parts by weight of modified hydroxypropyl methylcellulose, and 2.5 parts by weight of modified polymer were stirred at a stirring rate of 2000 r / min for 1 h, and then 2.5 parts by weight of photoinitiator 184 were added and stirred for 2 h to obtain a polyurethane coating.

[0052] The polyurethane coating obtained in this example was subjected to the following performance tests:

[0053] (1) Sagging performance test: GB / T9264-1988 "Evaluation of anti-sagging properties of paints and varnishes"; the test was carried out using a sag meter and it was found that the coating did not sag when applied thickly with a thickness of 2000 microns.

[0054] (2) Viscosity test: GB / T19250-2013 Polyurethane waterproof coating; viscosity is 19700 mPa·s.

[0055] (3) Hydrophobic performance test: The polyurethane coating was sprayed on the wall, and a drop of 5 μl of deionized water was dropped on the surface of the formed paint film. The contact angle of the coating was measured using a contact angle meter. Figure 2 As shown, the contact angle was found to be 168°.

[0056] (4) Antibacterial performance test: GB / T1741-2020 "Test method for resistance of paint film to enzyme bacteria", see Figure 3 Escherichia coli was cultured in a 96-well plate and then tested according to the national standard method. The cultured Escherichia coli was evenly inoculated onto the surface of the paint film to detect cell activity, and it was found that the antibacterial rate could reach 99.9%.

[0057] (5) Self-healing performance: GB / T19250-2013 "Polyurethane Waterproof Coating", the paint film was subjected to a tensile strength test, and then the broken sections were butt-jointed and cured at 60°C for 2 hours. The tensile strength was tested again and it was found that the tensile strength could be restored to 70.3% of the original value.

[0058] Example 2

[0059] The present embodiment provides a polyurethane coating, comprising 100 parts by weight of an aqueous polyurethane, 10 parts by weight of a polyurethane rheological agent, and 5 parts by weight of a photoinitiator 184, wherein the mass ratio of modified hydroxypropyl methylcellulose to modified polymer in the polyurethane rheological agent is 1.5:1, and the modified hydroxypropyl methylcellulose and modified polymer are prepared by Preparation Example 1-2.

[0060] This embodiment also provides a method for preparing a polyurethane coating, comprising:

[0061] 100 parts by weight of aqueous polyurethane, 6 parts by weight of modified hydroxypropyl methylcellulose, and 4 parts by weight of modified polymer were stirred at a stirring rate of 1500 r / min for 1 h, and then 5 parts by weight of photoinitiator 184 were added and stirred for 4 hours to obtain a polyurethane coating.

[0062] The polyurethane coating obtained in this example was subjected to the same performance test as in Example 1:

[0063] (1) Sagging performance test: It was found that the coating did not sag when applied thickly at 1900 μm.

[0064] (2) Viscosity test: The viscosity is 20300 mPa·s.

[0065] (3) Hydrophobic performance test: contact angle is 171°.

[0066] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 99.9%.

[0067] (5) Self-repair performance: The tensile strength can be restored to 72.3% of the original.

[0068] Example 3

[0069] The present embodiment provides a polyurethane coating, including 60 parts by weight of aqueous polyurethane, 5 parts by weight of a polyurethane rheological agent, and 1 part by weight of a photoinitiator 184. The mass ratio of modified hydroxypropyl methylcellulose to modified polymer in the polyurethane rheological agent is 1:1, and the modified hydroxypropyl methylcellulose and modified polymer are prepared by Preparation Example 1-2.

[0070] This embodiment also provides a method for preparing a polyurethane coating, comprising:

[0071] 60 parts by weight of aqueous polyurethane, 2.5 parts by weight of modified hydroxypropyl methylcellulose, and 2.5 parts by weight of modified polymer were stirred at a stirring rate of 1800 r / min for 0.8 h, and then 1 part by weight of photoinitiator 184 was added and stirred for 0.5 h to obtain a polyurethane coating.

[0072] The polyurethane coating obtained in this example was subjected to the same performance test as in Example 1:

[0073] (1) Sagging performance test: It was found that it did not sag when applied thickly with a thickness of 2000 microns.

[0074] (2) Viscosity test: The viscosity is 19300 mPa·s.

[0075] (3) Hydrophobic performance test: contact angle is 165°.

[0076] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 99.7%.

[0077] (5) Self-repair performance: The tensile strength can be restored to 66.6% of the original value.

[0078] Example 4

[0079] The difference from Example 1 is that the photoinitiator is photoinitiator 1173.

[0080] The polyurethane coating obtained in this example was subjected to the same performance test as in Example 1:

[0081] (1) Sagging performance test: It was found that the coating did not sag when applied thickly at 1700 μm.

[0082] (2) Viscosity test: The viscosity is 18100 mPa·s.

[0083] (3) Hydrophobic performance test: contact angle is 168°.

[0084] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 99.7%.

[0085] (5) Self-repair performance: The tensile strength can be restored to 64.3% of the original.

[0086] Comparative Example 1

[0087] The difference from Example 1 is that the surface of the modified hydroxypropyl methylcellulose is not loaded with nano zinc oxide.

[0088] The polyurethane coating obtained in this comparative example was subjected to the same performance test as in Example 1:

[0089] (1) Sagging performance test: It was found that it did not sag when applied thickly at 1500 microns.

[0090] (2) Viscosity test: The viscosity is 17200 mPa·s.

[0091] (3) Hydrophobic performance test: contact angle is 165°.

[0092] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 90.5%.

[0093] (5) Self-repair performance: The tensile strength can be restored to 65.2% of the original value.

[0094] By comparing Example 1 and Comparative Example 1, it can be seen that if nano zinc oxide is not loaded, the sagging performance, viscosity performance and bactericidal performance will be affected; mainly because nano zinc oxide is loaded on the surface of hydroxypropyl methylcellulose, which can not only interact with the fluid molecular orbitals to enhance the adhesion performance, but also can synergistically enhance the antibacterial performance.

[0095] Comparative Example 2

[0096] The difference from Example 1 is that the hydroxypropyl methylcellulose is not modified.

[0097] The polyurethane coating obtained in this comparative example was subjected to the same performance test as in Example 1:

[0098] (1) Sagging performance test: It was found that it did not sag when applied thickly at 1500 microns.

[0099] (2) Viscosity test: The viscosity is 16800 mPa·s.

[0100] (3) Hydrophobic performance test: contact angle is 142°.

[0101] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 85.4%.

[0102] (5) Self-repair performance: The tensile strength can be restored to 50.2% of the original value.

[0103] By comparing Example 1 and Comparative Example 2, it can be seen that if the hydroxypropyl methylcellulose in the coating is not modified, the hydrophobicity, antibacterial property and self-repairing property will be greatly affected.

[0104] Comparative Example 3

[0105] The difference from Example 1 is that the polymer is not modified.

[0106] The polyurethane coating obtained in this comparative example was subjected to the same performance test as in Example 1:

[0107] (1) Sagging performance test: It was found that the coating did not sag when applied thickly at 1400 μm.

[0108] (2) Viscosity test: The viscosity is 15700 mPa·s.

[0109] (3) Hydrophobic performance test: contact angle is 150°.

[0110] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 99.8%.

[0111] (5) Self-repair performance: The tensile strength can be restored to 55.2% of the original value.

[0112] By comparing Example 1 and Comparative Example 3, it can be seen that if the polymer in the coating is not modified, the sagging performance, viscosity performance, hydrophobicity and self-healing performance will be greatly affected.

[0113] Comparative Example 4

[0114] The difference from Example 1 is that modified hydroxypropyl methylcellulose is not included, and the added amount of the modified polymer is the sum of the added amounts of the modified hydroxypropyl methylcellulose and the modified polymer in Example 1.

[0115] The polyurethane coating obtained in this comparative example was subjected to the same performance test as in Example 1:

[0116] (1) Sagging performance test: It was found that the coating did not sag when applied thickly at 1600 μm.

[0117] (2) Viscosity test: The viscosity is 16200 mPa·s.

[0118] (3) Hydrophobic performance test: contact angle is 151°.

[0119] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 84.7%.

[0120] (5) Self-repair performance: The tensile strength can be restored to 52.6% of the original value.

[0121] By comparing Example 1 and Comparative Example 4, it can be seen that if the coating does not include modified hydroxypropyl methylcellulose, the sagging performance, viscosity performance, hydrophobicity and self-repairing performance will be affected to a certain extent, and the antibacterial performance will be greatly affected.

[0122] Comparative Example 5

[0123] The difference from Example 1 is that no modified polymer is included, and the added amount of modified hydroxypropyl methylcellulose is the sum of the added amounts of modified hydroxypropyl methylcellulose and modified polymer in Example 1.

[0124] The polyurethane coating obtained in this comparative example was subjected to the same performance test as in Example 1:

[0125] (1) Sagging performance test: It was found that the coating did not sag when applied thickly at 1400 μm.

[0126] (2) Viscosity test: The viscosity is 15200 mPa·s.

[0127] (3) Hydrophobic performance test: contact angle is 147°.

[0128] (4) Antibacterial performance test: The antibacterial rate against Escherichia coli can reach 99.9%.

[0129] (5) Self-repair performance: The tensile strength can be restored to 54.2% of the original value.

[0130] By comparing Example 1 and Comparative Example 5, it can be seen that if the coating does not include modified hydroxypropyl methylcellulose, the sagging performance, viscosity performance, hydrophobicity and self-healing performance will be affected to a certain extent.

[0131] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A polyurethane rheology modifier for imparting water resistance to a paint film, characterized in that: The polyurethane rheology modifier comprises modified hydroxypropyl methylcellulose and a modified polymer in a mass ratio of (1-1.5):1; The preparation method of the modified hydroxypropyl methylcellulose comprises: A1, uniformly mixing olefinated hydroxyapatite, hydroxypropyl methylcellulose, undecene aldehyde and deionized water, and then adding sodium dodecylbenzene sulfonate and ammonium persulfate to react to obtain substituted hydroxypropyl methylcellulose; A2, dispersing zinc oxide in anhydrous ethanol to form a zinc oxide dispersion, and then immersing the substituted hydroxypropyl methylcellulose obtained in A1 in the zinc oxide dispersion to obtain modified hydroxypropyl methylcellulose; In step A1, the reaction temperature is 60-70°C and the reaction time is 3-5 h; In step A2, the concentration of the zinc oxide dispersion is 10-30%; The step A2 further comprises drying the impregnated material, wherein the drying is vacuum drying, the drying temperature is 40-80° C., and the drying time is 4-10 h; The preparation method of the modified polymer comprises: S1, adding oleic acid and N,N-dimethylpropylenediamine in a molar ratio of 1:1.1 to a mixed solution of acetone and ethanol, and reacting at 120-150° C. for 12-24 h in a nitrogen environment to obtain an oleic acid amidopropyl dimethyl tertiary amine mixed solution; S2, cooling the oleamidopropyl dimethyl tertiary amine mixed solution obtained in S1 to 80-90° C., adding allyl chloride and reacting for 8-10 hours to obtain a hydrophobic monomer; S3. Add the hydrophobic monomer obtained in S2 to an acrylamide solution with a concentration of 20-40%, add cocamidopropyl betaine as a dispersant, adjust the pH to 6.5-7, lower the reaction temperature, pass nitrogen to deoxygenate at 0-5°C for 30 min, use sodium formate as a chain transfer agent, continue to pass nitrogen for 2 min and then stop passing nitrogen, and react adiabatically for 6-8 h to obtain a transparent rubber block. After drying and crushing, extract and purify it with acetone-ethanol for 12-16 h to obtain a modified polymer.

2. The polyurethane rheology modifier for imparting water resistance to a paint film according to claim 1, characterized in that: The preparation method of the alkenylated hydroxyapatite comprises: uniformly mixing nano-hydroxyapatite, γ-methacryloxypropyltrimethoxysilane and ethanol, and reacting at 60-70° C. for 5-8 hours to obtain the alkenylated hydroxyapatite.

3. The polyurethane rheology modifier for imparting water resistance to a paint film according to claim 1, characterized in that: Based on 100 g of hydroxypropyl methylcellulose, the amount of olefinated hydroxyapatite in A1 is 7-15 g, the amount of undecylenic aldehyde is 18-25 g, the amount of sodium dodecylbenzene sulfonate is 8-11 g, the amount of ammonium persulfate is 1.5-2 g, and the amount of deionized water is 3500-3800 g.

4. The method for preparing a polyurethane rheology modifier for imparting water resistance to a paint film according to any one of claims 1 to 3, characterized in that: The preparation method comprises: mixing modified hydroxypropyl methylcellulose and a modified polymer in a mass ratio of (1-1.5):1 to obtain a polyurethane rheology modifier.

5. A polyurethane coating, characterized in that: The polyurethane coating comprises: 60-100 parts by weight of waterborne polyurethane, 5-10 parts by weight of polyurethane rheology modifier and 1-3 parts by weight of photoinitiator, wherein the polyurethane rheology modifier is the polyurethane rheology modifier according to any one of claims 1-3.

6. The polyurethane coating according to claim 5, characterized in that: The photoinitiator includes photoinitiator 1173 or photoinitiator 184 .

7. The method for preparing the polyurethane coating according to claim 5 or 6, characterized in that: The preparation method comprises: stirring 60-100 parts by weight of waterborne polyurethane and 5-10 parts by weight of polyurethane rheology modifier once, and then adding 1-3 parts by weight of photoinitiator and stirring again to obtain polyurethane coating.

8. The method for preparing the polyurethane coating according to claim 7, characterized in that: The stirring rate is 1500-2000 r / min, and the stirring time is 0.5-1h; The secondary stirring rate is 1500-2000 r / min, and the secondary stirring time is 1-4 h.