A method for evaluating the flowability of solder for brazing dissimilar materials

By measuring the solder flow area on dissimilar material test pieces and calculating the difference coefficient k, the problem of difficult solder selection in dissimilar material brazing is solved, and high-reliability connection and flow-laying ability evaluation of dissimilar material components are achieved.

CN118465222BActive Publication Date: 2024-10-15CITIC HEAVY INDUSTRIES CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410943282.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-15
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing technology lacks a solder flow ability evaluation method for soldering dissimilar materials, which makes it difficult to select solder and achieve high-reliability connection of dissimilar material components.

Method used

By assembling the test pieces made of material A and material B into test components, placing the solder and heating it to melt it, measuring and recording the total flow area of ​​the solder on each test piece, and calculating the difference coefficient between the flow areas. k, based on the k value, determine the flow-laying ability of the filler metal and determine whether it is suitable for brazing dissimilar materials.

Benefits of technology

It provides a reliable basis for selecting brazing materials, improves the connection reliability of brazing of dissimilar materials, simplifies the test process, reduces errors, and improves the accuracy of test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118465222B_ABST
    Figure CN118465222B_ABST
Patent Text Reader

Abstract

A method for evaluating the flowability of solder for brazing dissimilar materials, comprising: step 1, assembling a test piece A made of material A and a test piece B made of material B into a test assembly according to a preset method; step 2, placing solder at the position where different materials meet in the test assembly, heating the solder to melt the solder, and measuring and recording the total flow area of ​​the solder on the test piece A after the solder solidifies S A总 and the total flow area of ​​the brazing material on the B test piece S B总 ; Step 3, calculate S A总 and S B总 The coefficient of difference between k ,when S A总 > S B总 >0, k = S A总 / S B总 ,when S B总 > S A总 >0, k = S B总 / S A总 ;according to k The value determines whether the brazing filler metal is suitable for brazing dissimilar material components composed of material A and material B. The present invention only needs a small number of tests to complete the brazing filler metal flow ability assessment for dissimilar material brazing. The test method is simple, operability is strong, and the test error is small, which has a strong guiding significance for the selection of brazing filler metal for dissimilar material brazing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of brazing, and in particular relates to a method for evaluating the flowability of brazing filler metals for brazing dissimilar materials. Background Art

[0002] With the rapid development of materials science, new materials such as light metals (aluminum, magnesium, titanium) and lightweight and high-strength ceramics and ceramic-based composites, C / C composites, and intermetallic compounds are constantly emerging, and these materials have put forward new requirements for welding technology. At the same time, in actual production, energy conservation and emission reduction, low-cost manufacturing, and structural and functional integration are gradually taken as the goals, so that composite structures composed of different materials (dissimilar metals or metal-non-metals) are increasingly widely used. The connection of heterogeneous material components can maximize the performance of each material and is the key to obtaining heterogeneous material composite structures with excellent performance. The connection of heterogeneous material components and the safe and long-term use of their connection structures are increasingly valued by related industries, and brazing has gradually become the mainstream method for connecting heterogeneous material components. At present, when brazing heterogeneous material components, there are mainly the following technical difficulties: the difference in wettability of the brazing material to the heterogeneous material components leads to problems such as asynchronous wetting, difficulty in coordinated flow laying, and difficulty in complete filling.

[0003] In the face of the above technical difficulties, in order to achieve reliable brazing of heterogeneous material components, it is necessary to select and evaluate the brazing material according to the heterogeneous material components to be connected before brazing. There are two types of wettability tests, spreadability and filling. Spreadability test, also known as flowability test, is the most convenient and commonly used evaluation method.

[0004] However, the current flowability test does not include a method for evaluating the flowability of solder related to dissimilar materials, so it is difficult to evaluate whether the solder can be used for brazing two materials.

[0005] Therefore, it is urgent to propose a method to evaluate the solder flow ability of dissimilar materials brazing. Summary of the invention

[0006] The purpose of the present invention is to provide a method for evaluating the flow ability of solder for brazing dissimilar materials, to evaluate the flow ability of solder used for brazing dissimilar material components, to provide a reliable basis for the selection of solder, and to achieve high-reliability connection of dissimilar material components.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is: a method for evaluating the flow ability of brazing filler metal for brazing of dissimilar materials, comprising the following steps:

[0008] Step 1: assemble the A test piece made of material A and the B test piece made of material B into a test assembly according to a preset method;

[0009] Step 2: Place the solder to be tested at the location where different materials meet in the test assembly, heat it to melt the solder, and measure and record the total flow area of ​​the solder on the A test piece after the solder solidifies. S A总 and the total flow area of ​​the brazing material on the B test piece S B总 ;

[0010] Step 3: Calculate the total paving area S A总 and S B总 The coefficient of difference between k ,when S A总 > S B总 >0, k = S A总 / S B总 ,when S B总 > S A总 >0, k = S B总 / S A总 ;

[0011] When 1≤ k ≤m, m is the first judgment value, then it is judged that the flow-laying ability of the brazing material on the A test piece and the B test piece is equivalent, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material;

[0012] When m< k ≤n, n is the second judgment value, then it is judged that the flow spreading ability of the brazing material on the A test piece and the B test piece is slightly different, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material while meeting the performance requirements;

[0013] when k >n, it is judged that the flowability of the brazing material on the A test piece and the B test piece is greatly different, and it is not recommended to use the brazing material to braze the dissimilar material components composed of A material and B material.

[0014] The value range of the first judgment value m is 1.3~1.5, the value range of the second judgment value n is 1.5~2, and nm≥0.2.

[0015] Preferably, in step 2, a positioning groove or a positioning hole for placing the solder is provided at the joint position of different materials in the test assembly.

[0016] Based on the above-mentioned evaluation method of brazing filler metal flow ability of dissimilar materials brazing, it can be realized through a variety of technical solutions, among which the first technical solution is:

[0017] Preferably, in step one, the test piece A and the test piece B are both plate-shaped, and the thickness of the test piece A is greater than that of the test piece B. The test piece A is provided with a groove, and the shape and size of the groove are matched with the shape and size of the test piece B. During testing, the test piece B is embedded in the groove, and the upper surface of the test piece B is flush with the upper surface of the test piece A to form the test assembly.

[0018] Furthermore, in step 2, at least two solders are placed at the joint between the B test piece and the A test piece, and the solders are heated to melt. After the solders solidify, the spreading area of ​​the solders on the A test piece is measured and recorded. S A1 , S A2 … S Ai , and the flow area of ​​the solder on the B test piece S B1 , S B2 … S Bj , i and j are the number of solders, and i=j≥2, the total flow area S A总 = S A1 + S A2 +……+ S Ai , S B总 = S B1 + S B2 +……+ S Bj .

[0019] The advantage of this solution is that the total flow area can be obtained through one test component S A总 and S B总 , easy to operate; placing multiple solders, multiple flow areas can be measured in one test, which can reduce the error caused by one data and make the test results more reliable. In addition, in this scheme, the solder is only spread on the plane, which is more convenient for statistics and measurement of the flow area.

[0020] The second technical solution provided by the present invention is:

[0021] Preferably, in step one, the test component includes test component I and test component II, in which the A test piece and the B test piece are both plate-shaped; in test component I, the A test piece is overlapped and placed on the B test piece; in test component II, the B test piece is overlapped and placed on the A test piece.

[0022] Furthermore, in step 2, a solder is placed at the overlap of the A test piece and the B test piece, and the solder is heated to melt the solder. After the solder solidifies, the flow area of ​​the solder on the A test piece is measured and recorded in the test assembly I. S A1 and the flow area of ​​the solder on the B test piece S B1 , measure and record the flow area of ​​the brazing material on the A test piece in the test assembly II S A2 and the flow area of ​​the solder on the B test piece S B2 ; S A总 = S A1 + S A2 , S B总 = S B1 + S B2 .

[0023] The advantages of this solution are: this technical solution uses the overlap form to measure the flow spreading performance of the solder. When measuring the flow spreading area, it is equivalent to measuring the flow spreading area of ​​the solder on the front side of the lower test plate and the back side of the upper test plate, that is, S A总 = S A1 + S A2 = S A正 + S A反 , S B总 = S B1 + S B2 = S B正 + S B反This is similar to the brazing of lap joints in the actual brazing process and is closer to the actual brazing scenario. The influence of the upper and lower position relationship of the parts to be welded on the flow performance of the solder can be considered in advance, which is more conducive to providing guidance for actual brazing and determining the lap length.

[0024] The third technical solution provided by the present invention is:

[0025] Preferably, in step one, in said step one, the test piece A and the test piece B are both rectangular plates, and the test piece A and the test piece B have the same size, two test pieces A and two test pieces B are spliced ​​in a circumferentially alternating arrangement to form the test assembly, and the two test pieces A and the two test pieces B are respectively distributed diagonally.

[0026] Furthermore, a brazing material is placed at the joint position of the two A test pieces and the two B test pieces, and the brazing material is heated to melt the brazing material. After the brazing material solidifies, the flow area of ​​the brazing material on the two A test pieces is measured and recorded. S A1 and S A2 , and the flow area of ​​the brazing material on the two B test pieces S B1 and S B2 , S A总 = S A1 + S A2 , S B总 = S B1 + S B2 .

[0027] Furthermore, a positioning groove for accommodating the solder is provided at the center of the test assembly, and the volume of the positioning groove is smaller than the volume of the solder.

[0028] The advantages of this solution are: This test solution can also reduce the number of test components, and only one test component is used to test once to obtain S A总 = S A1 + S A2 and S B总 = S B1 + S B2 In addition, in this scheme, the solder is only spread in the plane, which makes it easier to count and measure the spread area.

[0029] In addition, the two A test pieces and the two B test pieces are distributed diagonally, which helps to avoid the problem of inaccurate measurement results caused by uneven placement of the test board during testing.

[0030] The beneficial effects of the present invention are as follows: the present invention provides a method for evaluating the flow spreading ability of solder for brazing of different materials, taking a test piece A and a test piece B of different materials as test objects, and testing the total flow spreading area of ​​the solder on the test piece A and the test piece B. S A总 and S B总 , and introduce S A总 and S B总 The coefficient of difference between the two k ,according to k The value can be used to judge the flow ability of the solder on the dissimilar materials, and then provide guidance for the selection of solder for the corresponding dissimilar materials brazing, solving the problem of solder selection in the existing technology for dissimilar materials brazing. S A总 and S B总 It can effectively reduce the test error and improve the accuracy of the test results. For solder with relatively poor flow ability, relatively large data can be obtained, which is convenient for subsequent calculations.

[0031] The solution provided by the present invention only requires a small number of experiments to complete the evaluation of the solder flow ability of the brazing of dissimilar materials. The test method is simple, operability is strong, and the test error is small. It has a strong guiding significance for the selection of solder for the brazing of dissimilar materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 It is a front view of the test assembly of the present invention in Example 1;

[0034] Figure 2 is a top view of the test assembly of the present invention in Example 1;

[0035] Figure 3 A schematic diagram of solder flow laying on the test assembly of the present invention in Example 1;

[0036] Figure 4Schematic diagram of the arrangement of the positioning grooves on the test assembly of the present invention in Example 1;

[0037] Figure 5 It is a front view of the test component I of the present invention in Example 2;

[0038] Figure 6 It is a front view of the test assembly II of the present invention in Example 2;

[0039] Figure 7 Schematic diagram of solder flow laying on the test assembly I of the present invention in Example 2;

[0040] Figure 8 Schematic diagram of solder flow laying on the test assembly II of the present invention in Example 2;

[0041] Fig. 9 This is a schematic diagram of the arrangement of the positioning grooves, taking the test component I as an example in Example 2;

[0042] Fig.10 is a top view of the test assembly of the present invention in Example 3;

[0043] Fig.11 A schematic diagram of solder flow laying on the test assembly of the present invention in Example 3;

[0044] Markings in the figure: 1. Test piece A, 2. Test piece B, 3. Solder, 4. Positioning groove. DETAILED DESCRIPTION

[0045] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the invention in any way.

[0046] Example 1: Figure 1-3 As shown, a method for evaluating the flowability of brazing materials for brazing of dissimilar materials comprises the following steps:

[0047] Step 1: prepare a test piece A 1 and a test piece B 2, wherein the test piece A 1 is made of material A, and the test piece B 2 is made of material B, and assemble the test piece A 1 and the test piece B 2 in a preset manner to form a test assembly;

[0048] Specifically, Figure 1 , 2 As shown, the test piece A 1 and the test piece B 2 are both rectangular flat plates, the thickness of the test piece A 1 is greater than that of the test piece B 2, a groove with the same shape and size as those of the test piece B 2 is set on the upper surface of the test piece A 1, the test piece B is embedded in the groove, and the upper surface of the test piece B is flush with the upper surface of the test piece A, thereby forming the test assembly.

[0049] Step 2: Place two solders 3 to be tested at the connection between the A test piece 1 and the B test piece 2. Preferably, place the two solders at two different side positions of the B test piece 2; heat the solder 3 to melt it, and spread it on the A test piece 1 and the B test piece 2 on both sides. After the solder 3 solidifies, measure and record the spread area of ​​the two solders 3 on the A test piece 1. S A1 and S A2 , and the flow area of ​​the two solders 3 on the B test piece 2 S B1 and S B2 ,like Figure 3 As shown; the total flow area of ​​two solders 3 on the A test piece 1 S A总 = S A1 + S A2 , the total flow area on the B test piece S B总 = S B1 + S B2 .

[0050] Step 3: Calculate the total paving area S A总 and S B总 The coefficient of difference between k , k = S A总 / S B总 ( S A总 > S B总 >0), or k = S B总 / S A总 ( S B总 > S A总 >0);

[0051] When 1≤ k ≤m, m is the first judgment value, then it is judged that the flow spreading ability of the brazing material 3 on the A test piece 1 and the B test piece 2 is equivalent, and the brazing material 3 can be used to braze the dissimilar material components composed of the A material and the B material;

[0052] When m< k≤n, n is the second judgment value, then it is judged that the flow spreading ability of the brazing material 3 on the A test piece 1 and the B test piece 2 is relatively small, and the brazing material 3 can be used to braze the dissimilar material components composed of the A material and the B material while meeting the performance requirements;

[0053] when k >n, it is judged that the flowability of the solder 3 on the A test piece 1 and the B test piece 2 is greatly different, and it is not recommended to use the solder 3 to braze the dissimilar material components composed of A material and B material.

[0054] It should be noted that m and n can be adjusted according to actual needs. When the post-welding performance and service conditions of the dissimilar material brazing workpiece are more stringent, the values ​​of m and n can be appropriately reduced to meet the use requirements of the workpiece; when the post-welding performance and service conditions of the dissimilar material brazing workpiece are generally required, the values ​​of m and n can be appropriately increased to increase the selection range of brazing filler metals and facilitate the rapid determination of suitable brazing filler metals.

[0055] The present invention provides the value range of m and n in general, wherein the value range of m is 1.3-1.5, the value range of n is 1.5-2, and nm≥0.2. Due to the inevitable existence of some experimental errors, if the difference between n and m is too small, the influence of the experimental error will be magnified, which is not conducive to the selection of solder.

[0056] Preferably, a positioning groove 4 is provided at the connection between the A test piece 1 and the B test piece 2 on the test assembly for accommodating the solder 3, and the volume of the positioning groove 4 is smaller than the volume of the solder 3. A portion of the positioning groove 4 is located on the A test piece 1, and the other portion is located on the B test piece 2. Figure 4 The shape of the positioning groove 4 can be adaptively adjusted according to the shape of the solder 3 to be tested. When the solder 3 to be tested is a spherical particle, the positioning groove 4 can be hemispherical. When the solder 3 to be tested is a cylindrical particle, the positioning groove 4 can be cylindrical or semi-cylindrical. When the solder 3 to be tested is a rectangular parallelepiped, the positioning groove 4 can be a rectangular parallelepiped.

[0057] Since the placement of the solder 3 affects the spreading area, if the solder is biased to one side, more spreading may occur on that side. Therefore, the positioning groove 4 can prevent the solder 3 from moving in the mobile test assembly, and can pre-set the placement of the solder 3, reduce the error caused by the placement, and thus ensure the reliability of the test results.

[0058] As a variation of this embodiment, the B test piece 2 is a polygonal plate such as a triangle, pentagon, or hexagon, and the number of solders is equal to the number of sides of the B test piece, with one solder placed on each side of the B test piece. In this case, it is necessary to measure and record the flow area of ​​multiple solders on the A test piece.S A1 , S A2 … S Ai , and the flow area of ​​multiple solders on the B test piece S B1 , S B2 … S Bj , i and j are the number of solders, and i=j, the total flow area S A总 = S A1 + S A2 +……+ S Ai , S B总 = S B1 + S B2 +……+ S Bj .

[0059] In this embodiment, a solder 3 is placed on the side of the B test piece 2. In other embodiments, multiple solders 3 can be placed on one side of the B test piece 2. In this case, a high degree of flatness is required between the A test piece 1 and the B test piece 2 to avoid test errors caused by unevenness.

[0060] Example 2: The difference between this example and Example 1 is that step 1 and step 2 are different, and the evaluation method in step 3 is the same.

[0061] In step 1 of this embodiment, the test assembly includes a test assembly I and a test assembly II. In the test assembly I and the test assembly II, the A test piece 1 and the B test piece 2 are both rectangular plates; the structure of the test assembly I is as follows: Figure 5 As shown, the A test piece 1 is used as the bottom, and the B test piece 2 is overlapped on the upper surface of the A test piece 1, and the overlapping area is smaller than the area of ​​the A test piece 1 and the B test piece 2; the structure of the test assembly II is as follows Figure 6 As shown, with the B test piece 2 as the bottom, the A test piece 1 overlaps the upper surface of the B test piece 2, and the area of ​​the overlapping portion is smaller than the areas of the A test piece 1 and the B test piece 2.

[0062] In step 2 of this embodiment, the solder 3 to be tested is placed at the overlap of the A test piece 1 and the B test piece 2 in the test assembly I and the test assembly II, and the solder 3 is heated to melt. After the solder 3 solidifies, the flow area of ​​the solder 3 on the A test piece 1 is measured and recorded in the test assembly I. S A1 and the flow area of ​​the solder 3 on the B test piece 2 S B1 , in the test assembly II, measure and record the flow area of ​​the brazing material 3 on the A test piece 1 S A2 and the flow area of ​​the solder 3 on the B test piece 2 S B2 ,like Figure 7 , 8 As shown; in test assembly Ⅰ and test assembly Ⅱ, the total flow area of ​​the brazing material 3 on the A test piece 1 S A总 = S A1 + S A2 , the total flow area on the B test piece 2 S B总 = S B1 + S B2 .

[0063] Then, the flowability of the solder 3 was evaluated according to the method of step 3 of Example 1.

[0064] It should be noted that, in this embodiment, when measuring the flow paving area, what is measured is the area of ​​the exposed overlapping area.

[0065] In this embodiment, since the solder 3 needs to be clamped between the A test piece 1 and the B test piece 2 during measurement, this solution is more suitable for measuring the flow performance of sheet, paste or powder solder. In addition, in order to ensure the stability of the overlap structure during testing, a special test bench can be designed to support the upper test board to prevent the upper test board from being displaced or unable to be stably maintained on the lower test board. For example, a support block can be set below the suspended part of the upper test board to support it in a position that does not hinder the flow of the solder.

[0066] Preferably, Fig. 9 As shown, in test components I and test components II, upper and lower positioning grooves 4 are provided at the overlapping positions of test piece A 1 and test piece B 2. The upper and lower positioning grooves 4 are respectively located on test piece A 1 and test piece B 2 to accommodate the solder 3 used for testing, and the sum of the depths of the two positioning grooves 4 is less than the thickness of the solder 3 so that the solder 3 can flow out after being heated and melted.

[0067] Example 3: The difference between this example and Example 1 is that step 1 and step 2 are different, and the evaluation method in step 3 is the same.

[0068] In step 1 of this embodiment, Fig.10 As shown, the test assembly is a field-shaped structure composed of two A test pieces 1 and two B test pieces 2, wherein the A test piece 1 and the B test piece 2 are both rectangular plates, and the A test piece 1 and the B test piece 2 have the same size, and the two A test pieces 1 and the two B test pieces 2 are respectively distributed diagonally.

[0069] In step 2 of this embodiment, the solder 3 to be tested is placed at the center of the upper surface of the test assembly, heated to melt the solder 3, and after the solder 3 solidifies, the flow area of ​​the solder 3 on the two A test pieces 1 is measured and recorded. S A1 and S A2 , and the flow area of ​​the solder 3 on the two B test pieces 2 S B1 and S B2 ,like Fig.11 As shown; the total flow area of ​​solder 3 on the A test piece 1 S A总 = S A1 + S A2 , the total flow area on the B test piece S B总 = S B1 + S B2 .

[0070] Then, the flowability of the solder 3 was evaluated according to the method of step 3 of Example 1.

[0071] Furthermore, a positioning groove 4 for accommodating the solder 3 can be provided at the center of the field-shaped test assembly, and the volume of the positioning groove 4 is smaller than the volume of the solder 3. The shape of the positioning groove 4 can be adaptively adjusted according to the shape of the solder 3 to be tested. When the solder 3 to be tested is a spherical particle, the positioning groove 4 can be hemispherical, when the solder 3 to be tested is cylindrical, the positioning groove 4 can be cylindrical or semi-cylindrical, and when the solder 3 to be tested is a rectangular parallelepiped, the positioning groove 4 can be rectangular parallelepiped.

[0072] Embodiment 4: In addition to the above embodiments, when the present invention is implemented, the test component can also be assembled in the following manner: a first mounting groove is opened on the horizontally placed test piece A 1, and the width of the first mounting groove is equal to the thickness of the test piece B 2. During testing, the test piece B 2 is perpendicular to the test piece A 1 and inserted in the first mounting groove to form an inverted T-shaped first test component; a second mounting groove is opened on the horizontally placed test piece B 2, and the width of the second mounting groove is equal to the thickness of the test piece A 1. During testing, the test piece A 1 is perpendicular to the test piece B 2 and inserted in the second mounting groove to form an inverted T-shaped second test component.

[0073] During the test, the solder 3 is placed at the angle where the A test piece 1 and the B test piece 2 are connected, and the solder 3 is heated to melt. After the solder 3 solidifies, the flow area of ​​the solder 3 on the A test piece 1 is measured and recorded on the first test assembly. S A1 and the flow area of ​​the solder 3 on the B test piece 2 S B1 , in the second test assembly, measure and record the flow area of ​​the solder 3 on the A test piece 1 S A2 and the flow area of ​​the solder 3 on the B test piece 2 S B2 Therefore, in the first test assembly and the second test assembly, the total flow area of ​​the solder 3 on the A test piece 1 is S A总 = S A1 + S A2 , the total flow area on the B test piece 2 S B总 = S B1 + S B2 Finally, the flowability of the solder 3 was evaluated according to the method of step 3 of Example 1.

[0074] In order to prevent the solder position from moving when the test assembly is moved, and to reduce the impact of the solder position placement difference on the accuracy of the test results, a positioning groove 4 for accommodating the solder 3 can be set at the angle position where the A test piece 1 and the B test piece 2 are connected, and the volume of the positioning groove 4 is smaller than the volume of the solder 3, which is conducive to ensuring that the solder 3 can flow along the surface of the test piece after melting. The shape of the positioning groove 4 can be adaptively adjusted according to the shape of the solder 3 to be tested. When the solder 3 to be tested is a spherical particle, the positioning groove 4 can be hemispherical, when the solder 3 to be tested is cylindrical, the positioning groove 4 can be cylindrical or semi-cylindrical, and when the solder 3 to be tested is a rectangular parallelepiped, the positioning groove 4 can be rectangular.

[0075] Embodiment 5: In this embodiment, a composite test assembly is used, and its structure is as follows: the composite test assembly is in an inverted T shape, including a horizontal bottom plate and a vertical upright plate, the horizontal bottom plate is composed of A test piece 1 and B test piece 2, both of which are rectangular plates, assembled in the form of side-jointing, and the upper surfaces of A test piece 1 and B test piece 2 are flush; the vertical upright plate is composed of A test piece 1 and B test piece 2, both of which are rectangular plates and equal in size, with the plate surfaces facing each other, the A test piece 1 in the vertical upright plate and the B test piece 2 in the horizontal bottom plate are connected to form a right angle, and the B test piece 2 in the vertical upright plate and the A test piece 1 in the horizontal bottom plate are connected to form another right angle. A through hole penetrating the vertical upright plate is opened at the position where the vertical upright plate and the horizontal bottom plate are connected, as a positioning hole, and the solder 3 to be tested is placed in the through hole.

[0076] After the test starts, the solder 3 in the composite test assembly is heated to melt. After the solder 3 solidifies, the flow area of ​​the solder 3 on the A test piece 1 and the B test piece 2 in the vertical stand is measured. S A1 and S B1 , and the flow area of ​​the brazing material 3 on the A test piece 1 and the B test piece 2 in the horizontal bottom plate S A2 and S B2 For the composite test assembly, the total flow area of ​​the solder 3 on the A test piece 1 is S A总 = S A1 + S A2 , the total flow area on the B test piece 2 S B总 = S B1 + S B2 Finally, the flowability of the solder 3 was evaluated according to the method of step 3 of Example 1.

[0077] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Those skilled in the art should understand that the specific implementation modes of the present invention may be modified or replaced by equivalents with reference to the above embodiments. Any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention are within the scope of protection of the pending claims.

Claims

1. A method for evaluating the flowability of brazing materials for brazing dissimilar materials, characterized in that: The steps include: Step 1: Assemble a test piece A made of material A and a test piece B made of material B into a test assembly, wherein both the test piece A and the test piece B are plate-shaped, and the thickness of the test piece A is greater than that of the test piece B. A groove is provided on the test piece A, and the shape and size of the groove match the shape and size of the test piece B. During testing, the test piece B is embedded in the groove, and the upper surface of the test piece B is flush with the upper surface of the test piece A, so as to form the test assembly; Step 2: Place the solder to be tested at the location where different materials meet in the test assembly, heat it to melt the solder, and measure and record the total flow area of ​​the solder on the A test piece after the solder solidifies. S A总 and the total flow area of ​​the brazing material on the B test piece S B总 ; Step 3: Calculate the total paving area S A总 and S B总 The coefficient of difference between k ,when S A总 > S B总 >0, k = S A总 / S B总 ,when S B总 > S A总 >0, k = S B总 / S A总 ; When 1≤ k ≤m, m is the first judgment value, then it is judged that the flow-laying ability of the brazing material on the A test piece and the B test piece is equivalent, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material; When m< k ≤n, n is the second judgment value, then it is judged that the flow spreading ability of the brazing material on the A test piece and the B test piece is slightly different, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material while meeting the performance requirements; when k >n, it is judged that the flowability of the brazing material on the A test piece and the B test piece is greatly different, and it is not recommended to use the brazing material to braze the dissimilar material components composed of A material and B material; The value range of the first judgment value m is 1.3~1.5, the value range of the second judgment value n is 1.5~2, and nm≥0.

2.

2. The solder flow ability evaluation method according to claim 1, characterized in that: In step 2, at least two solders are placed at the joint between the B test piece and the A test piece, and the solders are heated to melt. After the solders solidify, the spreading area of ​​the solders on the A test piece is measured and recorded. S A1 , S A2 … S Ai , and the flow area of ​​the solder on the B test piece S B1 , S B2 … S Bj , i and j are the number of solders, and i=j≥2, the total flow area S A总 = S A1 + S A2 +……+ S Ai , S B总 = S B1 + S B2 +……+ S Bj .

3. The method for evaluating solder flowability according to claim 1, characterized in that: In the step 2, positioning grooves or positioning holes for placing solder are provided at the joint positions of different materials in the test assembly.

4. A method for evaluating the flowability of brazing materials for brazing dissimilar materials, characterized in that: The steps include: Step 1: Assemble a test piece A made of material A and a test piece B made of material B into a test assembly, wherein the test assembly includes a test assembly I and a test assembly II, wherein both the test piece A and the test piece B are in a plate shape; In the test assembly I, the A test piece is placed on the B test piece in a overlapping manner; in the test assembly II, the B test piece is placed on the A test piece in a overlapping manner; Step 2: Place the solder to be tested at the location where different materials meet in the test assembly, heat it to melt the solder, and measure and record the total flow area of ​​the solder on the A test piece after the solder solidifies. S A总 and the total flow area of ​​the brazing material on the B test piece S B总 ; Step 3: Calculate the total paving area S A总 and S B总 The coefficient of difference between k ,when S A总 > S B总 >0, k = S A总 / S B总 ,when S B总 > S A总 >0, k = S B总 / S A总 ; When 1≤ k ≤m, m is the first judgment value, then it is judged that the flow-laying ability of the brazing material on the A test piece and the B test piece is equivalent, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material; When m< k ≤n, n is the second judgment value, then it is judged that the flow spreading ability of the brazing material on the A test piece and the B test piece is slightly different, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material while meeting the performance requirements; when k >n, it is judged that the flowability of the brazing material on the A test piece and the B test piece is greatly different, and it is not recommended to use the brazing material to braze the dissimilar material components composed of A material and B material; The value range of the first judgment value m is 1.3~1.5, the value range of the second judgment value n is 1.5~2, and nm≥0.

2.

5. The method for evaluating solder flowability according to claim 4, characterized in that: In step 2, a brazing material is placed at the joint of the A test piece and the B test piece, and the brazing material is heated to melt the brazing material. After the brazing material solidifies, the flow area of ​​the brazing material on the A test piece is measured and recorded in the test assembly I. S A1 and the flow area of ​​the solder on the B test piece S B1 , measure and record the flow area of ​​the brazing material on the A test piece in the test assembly II S A2 and the flow area of ​​the solder on the B test piece S B2 ; S A总 = S A1 + S A2 , S B总 = S B1 + S B2 .

6. The method for evaluating solder flowability according to claim 4, characterized in that: In the step 2, positioning grooves or positioning holes for placing solder are provided at the joint positions of different materials in the test assembly.

7. A method for evaluating the flowability of brazing materials for brazing dissimilar materials, characterized in that: The steps include: Step 1: Assemble an A test piece made of material A and a B test piece made of material B into a test assembly, wherein both the A test piece and the B test piece are rectangular plates, and the A test piece and the B test piece have the same size, and two A test pieces and two B test pieces are spliced ​​in a circumferentially alternating arrangement to form the test assembly, and the two A test pieces and the two B test pieces are respectively distributed diagonally; Step 2: Place the solder to be tested at the location where different materials meet in the test assembly, heat it to melt the solder, and measure and record the total flow area of ​​the solder on the A test piece after the solder solidifies. S A总 and the total flow area of ​​the brazing material on the B test piece S B总 ; Step 3: Calculate the total paving area S A总 and S B总 The coefficient of difference between k ,when S A总 > S B总 >0, k = S A总 / S B总 ,when S B总 > S A总 >0, k = S B总 / S A总 ; When 1≤ k ≤m, m is the first judgment value, then it is judged that the flow-laying ability of the brazing material on the A test piece and the B test piece is equivalent, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material; When m< k ≤n, n is the second judgment value, then it is judged that the flow spreading ability of the brazing material on the A test piece and the B test piece is slightly different, and the brazing material can be used to braze the dissimilar material components composed of the A material and the B material while meeting the performance requirements; when k >n, it is judged that the flowability of the brazing material on the A test piece and the B test piece is greatly different, and it is not recommended to use the brazing material to braze the dissimilar material components composed of A material and B material; The value range of the first judgment value m is 1.3~1.5, the value range of the second judgment value n is 1.5~2, and nm≥0.

2.

8. The method for evaluating solder flowability according to claim 7, characterized in that: In step 2, a brazing material is placed at the joint position of the two A test pieces and the two B test pieces, and the brazing material is heated to melt the brazing material. After the brazing material solidifies, the flow area of ​​the brazing material on the two A test pieces is measured and recorded. S A1 and S A2 , and the flow area of ​​the brazing material on the two B test pieces S B1 and S B2 , S A总 = S A1 + S A2 , S B总 = S B1 + S B2 .

9. The method for evaluating solder flowability according to claim 7, characterized in that: In the step 2, positioning grooves or positioning holes for placing solder are provided at the joint positions of different materials in the test assembly.