Conductive carbon paper and its preparation method and application
By adding elastic additives and modified carbon nanotubes/fibers to carbon fibers, conductive carbon paper with high elasticity and low resistivity was prepared, which solved the problem of increased resistivity after compression of carbon paper in fuel cells, and achieved the Long-term conductivity and gas ventilation of fuel cells.
Patent Information
- Application Number
- CN202410569800.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-09
AI Technical Summary
The existing porous carbon paper deforms when compressed in a fuel cell, resulting in gas leakage, increased resistivity and decreased power generation performance.
Carbon fiber containing elastic additives is used to prepare conductive carbon paper. By adding modified spiral carbon nanotubes and modified spiral carbon fibers to the carbon fiber base paper, the elastic recovery force of carbon paper is increased, and hydrophobized during the carbonization process is carried out to form Carbon paper with high gas ventilation and gas diffusion.
The elastic recovery force of carbon paper and the surface carbon material area are improved, the resistivity is reduced, the long-term conductivity stability and gas ventilation of the fuel cell membrane electrode are maintained, and the problem of increased resistivity after compression is avoided.
Smart Images

Figure GHA0000006222010000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a conductive carbon paper and a preparation method and application thereof. Background Art
[0002] Generally, the basic structure of a solid polymer fuel cell (hereinafter referred to as a fuel cell) is composed of a proton exchange membrane, a catalyst, and a gas diffusion layer arranged at the cathode and anode electrodes. The gas diffusion substrate acts as a battery reaction field and a current collector. In addition, in a general fuel cell, a waterproof layer is arranged between the catalyst and the gas diffusion layer substrate, and a bipolar plate is arranged on the other side of the gas diffusion layer substrate.
[0003] In the prior art, carbon paper, a gas diffusion layer substrate for fuel cells, is a porous sheet material formed by bonding dispersed carbon fibers with carbonized materials. Carbon papers with different porosities can be designed to improve the air permeability and drainage of the carbon paper.
[0004] However, the density, strength and thermal conductivity of porous carbon paper are currently uncompressed values. In fact, when such porous carbon paper is used as a gas diffusion substrate in a fuel cell, the porous carbon sheet will be compressed. When compressed, carbon fibers and carbonized materials are not elastic, and the carbon paper will deform during long-term compression, leading to gas leakage, increased resistivity, and decreased power generation performance.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide a conductive carbon paper and a preparation method and application thereof to solve the above problems.
[0007] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a conductive carbon paper, wherein the conductive carbon paper comprises carbon fibers and a binder component, wherein the binder component contains an elastic additive; when a load of 1 MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.30-0.40 g / cm 3 .
[0009] In a second aspect, the present invention further provides a method for preparing the conductive carbon paper, comprising the following steps:
[0010] S1: preparing a carbon fiber base paper containing the elastic additive;
[0011] S2: placing the carbon fiber base paper in a glue solution for dipping;
[0012] S3: drying, curing and carbonizing the impregnated carbon fiber base paper;
[0013] S4: hydrophobizing the carbonized product to obtain.
[0014] In a third aspect, the present invention also provides an application of the conductive carbon paper in the field of fuel cells.
[0015] Beneficial effects of the present invention:
[0016] The present invention adds an elastic additive when preparing the conductive carbon paper, which, on the one hand, has considerable elastic restoring force, and on the other hand, can fully increase the total area of carbon material exposed on the surface of the carbon paper when the carbon paper is compressed, so that the resistivity in the thickness direction is reduced. At the same time, even if it is compressed for a long time, the gas permeability and gas diffusion are also high. The technical problem that the carbon paper has a high resistivity when compressed and is difficult to recover after compression is solved, so that the membrane electrode of the fuel cell maintains long-term conductive stability during the power generation process. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0019] In these embodiments, unless otherwise specified, the parts and percentages are all based on mass. The raw material ratios not specified in the present invention can be mixed in any ratio.
[0020] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0021] The present invention discloses a conductive carbon paper, comprising carbon fibers and a binder component, wherein the binder component contains an elastic additive; when a load of 1 MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.30-0.40 g / cm 3 .
[0022] The bulk density of the carbon paper when a load of 1 MPa is applied in the thickness direction of the carbon paper is 0.30-0.40 g / cm 3 When the carbon fiber sheet has a high gas permeability and a high gas diffusivity.
[0023] The volume density of the carbon fiber when a load of 1 MPa is applied in the thickness direction of the carbon paper is less than 0.30 g / cm 3 In the case of , the total area of carbon fibers exposed on the surface of the carbon fiber sheet when a load is applied becomes smaller. Therefore, when the gas diffusion substrate is brought into contact with components such as a bipolar plate or a catalyst layer, the contact resistance becomes larger.
[0024] The bulk density of the carbon fibers when a load of 1 MPa is applied in the thickness direction of the carbon paper exceeds 0.40 g / cm 3 , the gas permeability of the carbon fiber sheet decreases.
[0025] The gas diffusion substrate of the present invention preferably has a resistance value of 2-10 mΩ·cm when a load of 1 MPa is applied in the thickness direction of the carbon paper. 2 .
[0026] In some embodiments, the elasticity aid includes 0.2-10 wt % of modified helical carbon nanotubes and / or modified helical carbon fibers.
[0027] Further, in some preferred embodiments, the length of the modified helical carbon nanotube is 30-100 μm and the diameter is 10-20 nm;
[0028] Furthermore, in some preferred embodiments, the length of the modified helical carbon fiber is 50-6000 μm, and the diameter is 50 nm-10000 nm.
[0029] When the content of the modified helical carbon nanotubes and / or modified helical carbon fibers is 0.2-10 wt%, since the modified helical carbon nanotubes and / or modified helical carbon fibers have elasticity, when the carbon paper is compressed, the total area of the carbon material exposed on the surface of the carbon paper can be fully increased. Therefore, when the gas diffusion substrate is brought into contact with components such as a bipolar plate or a catalyst layer, the contact resistance becomes small.
[0030] When the content of modified helical carbon nanotubes and / or modified helical carbon fibers is lower than 0.2wt%, the elastic recovery force of modified helical carbon nanotubes and / or modified helical carbon fibers is relatively small, thus having little effect on the contact resistance during compression and the recovery force of long-term compression.
[0031] When the content of modified helical carbon nanotubes and / or modified helical carbon fibers exceeds 10wt%, when the carbon paper is compressed, too much modified helical carbon nanotubes and / or modified helical carbon fibers are exposed on the surface of the carbon fiber sheet and are easily fallen off, polluting the environment.
[0032] A method for preparing the conductive carbon paper of the present invention comprises the following steps:
[0033] S1: preparing carbon fiber base paper containing the elastic additive.
[0034] In some embodiments, the preparation of carbon fiber base paper is as follows: carbon fiber, elastic additive and dispersant are placed in water, dispersed evenly to obtain a suspension, and the carbon fiber base paper is prepared by a conventional papermaking method.
[0035] In some embodiments, the mass concentration of the carbon fiber is 0.05-0.5 wt %.
[0036] In some embodiments, the mass concentration of the dispersant is 0.01-1wt%; the dispersant includes one or more of sodium polyacrylate, sodium dodecylbenzene sulfonate, polyoxyethylene amine, polyacrylamide, polyvinyl alcohol, polyethylene glycol, polyoxyethylene, carboxymethyl cellulose, hydroxyethyl cellulose or chitosan.
[0037] In some embodiments, the elasticity aid includes modified helical carbon nanotubes and / or modified helical carbon fibers.
[0038] In some preferred embodiments, the mass concentration of the elasticity aid is 0.2-10 wt %.
[0039] Furthermore, the length of the modified helical carbon nanotube is 30-100 μm and the diameter is 10-20 nm;
[0040] Furthermore, the length of the modified spiral carbon fiber is 50-6000 μm, and the diameter is 50 nm-10000 nm.
[0041] Furthermore, the modified helical carbon nanotubes or modified helical carbon fibers are obtained by heat treating the helical carbon nanotubes or helical carbon fibers at 150-400° C. in an oxygen-containing atmosphere for 1-60 minutes. The oxygen-containing atmosphere includes air or other oxygen-containing atmospheres.
[0042] The heat treatment in an oxygen-containing atmosphere can remove moisture, organic pollutants and other substances. When the heat treatment temperature is lower than 150°C, the required heat treatment time is lengthy, which increases the production cost. When the heat treatment temperature is higher than 400°C, the spiral carbon nanotubes or spiral carbon fibers are over-oxidized, resulting in a decrease in mechanical properties.
[0043] S2: placing the carbon fiber base paper in glue solution for dipping.
[0044] In some embodiments, the glue solution is a solution of a bonding resin, and the mass concentration of the bonding resin solution is 0.5-30 wt %.
[0045] S3: drying, curing and carbonizing the impregnated carbon fiber base paper.
[0046] In some embodiments, the curing is performed by pressing the dried carbon fiber base paper at 150-250° C. and 0.1-5 MPa.
[0047] In some embodiments, the carbonization temperature is 1200-2300° C., and the carbonization time is 2-30 min.
[0048] S4: hydrophobizing the carbonized product to obtain the conductive carbon paper, which can be used as a gas diffusion layer substrate for a fuel cell membrane electrode.
[0049] In some embodiments, the hydrophobization is to fully contact the carbonized product with a solution, dispersion or suspension of a hydrophobic material, followed by drying and heat treatment.
[0050] In some preferred embodiments, the hydrophobic material includes fluorine-containing resin.
[0051] In some more preferred embodiments, the hydrophobic material includes one or more of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) or tetrafluoroethylene-ethylene copolymer (ETFE).
[0052] The present invention also provides an application of the conductive carbon paper in the field of fuel cells.
[0053] The carbonized phase of the present invention, as well as the carbon fibers and elastic components contained in the phase, have a stable conductive path. In addition, due to the presence of the elastic components in the material, the gas diffusion layer substrate has elasticity, and the dimensional absorption is improved when the proton exchange membrane layer or the catalyst layer is compressed and bonded during fuel cell manufacturing. Even after long-term compression, the conductive performance does not significantly decrease, thereby maintaining the stable power generation performance of the battery.
[0054] The carbon paper prepared in the embodiment of the present invention was tested, including thickness direction resistivity test, change rate of thickness direction resistivity of carbon paper caused by long-term compression, air permeability and membrane electrode power generation performance test.
[0055] Carbon paper surface morphology: The uniformity of the carbon paper was observed visually.
[0056] Thickness direction resistivity test method: The carbon paper was sandwiched between two gold-plated copper electrodes, a pressure of 1 MPa was applied between the copper electrode plates, and then a 10 mA / cm 2 The current density is read, and the voltage drop at this time is read. The resistivity in the thickness direction of the carbon paper is calculated as follows:
[0057] R(Ω·cm 2 )=(voltage drop (V)×sample area (cm 2 )) / Current(A)
[0058] The rate of change of resistivity in the thickness direction of carbon paper caused by long-term compression: The carbon paper was placed between two gold-plated copper electrodes, and the resistivity in the thickness direction was measured after 5 minutes when the surface pressure was 1.0 MPa. The surface pressure of 1.0 MPa was then continued for 14,400 minutes, and the resistivity in the thickness direction after the continued pressure was measured. The rate of change of the resistivity in the thickness direction caused by long-term compression is calculated as follows:
[0059] Thickness direction resistivity change rate caused by long-term compression (%)
[0060] = [Resistivity in the thickness direction when pressure is applied for 5 minutes (Ω·cm 2 )-Resistivity in thickness direction when pressurized for 14,400 minutes (Ω·cm 2 )] / Resistivity in the thickness direction after 5 minutes of pressure application (Ω·cm 2 )
[0061] Air permeability test method: The carbon paper was clamped with a special tool and installed on the air permeability tester; then 200 mL of air was passed through the thickness direction of the carbon paper, and the gas permeability (mL / hr / cm 2 / mmAq).
[0062] Membrane electrode power generation performance test: The single cell was tested at a fuel cell test station (Changsha Blue Film Technology Co., Ltd.). Under different humidity conditions, the corresponding current decay after the single cell was discharged under constant voltage conditions was used to obtain the membrane electrode performance decay, namely the current density-voltage polarization curve and power density curve.
[0063] The test steps are as follows: the operating temperature of the fuel cell is fixed at 80°C and 20% relative humidity (RH), and humidified pure hydrogen and pure oxygen are supplied to the anode and cathode at 200mL / min, respectively. A back pressure of 55kPa is applied to the exhaust ports on both sides. Before the battery test, the membrane electrode is first activated for 30 minutes using a constant voltage of 0.6V under fully humidified conditions (100% RH) until the current density of the battery reaches a stable state. The polarization curve is measured using a scanning voltage of 1.0V to 0.2V with a step of 20mV s-1.
[0064] The power generation performance can be evaluated from the obtained polarization curve as follows:
[0065] Current density ≥2.5A / cm 2 @0.6V, it is considered good, indicated by the symbol ◎;
[0066] Current density ≥1.5A / cm 2 @0.6V, current density <2.5A / cm 2 When @0.6V, it is considered acceptable, indicated by the symbol △;
[0067] Current density <1.5A / cm 2 When @0.6V, it is counted as difference and represented by the symbol ╳.
[0068] Example 1
[0069] According to the preparation method provided by the present invention, a conductive carbon paper is prepared and its performance is tested. The specific steps are as follows:
[0070] (1) The commercially available helical carbon nanotubes were heat treated in air at 180° C. for 20 min to obtain modified helical carbon nanotubes, wherein the length of the modified helical carbon nanotubes was 30-100 μm and the diameter was 10-20 nm.
[0071] (2) About 1 g of carbon fiber, 10 g of the modified helical carbon nanotubes obtained in step (1) and 1 g of polyvinyl alcohol are placed in 1000 mL of deionized water, dispersed evenly to obtain a suspension, and a conventional papermaking method is used to prepare a carbon fiber base paper.
[0072] (3) Prepare an aqueous solution of about 10 wt% of phenolic resin to form a glue solution.
[0073] (4) Immerse the carbon fiber base paper obtained in step (2) in the glue solution in step (3) for 30 minutes.
[0074] (5) The carbon fiber base paper obtained in step (4) is dried at 120° C., then pressed at 200° C. and 0.5 MPa for 10 min, and then carbonized at 2000° C. for 20 min.
[0075] (6) Immersing the carbonized product in a PTFE aqueous solution with a mass concentration of 10% for 5 minutes, taking it out and drying it, and then sintering it at 350° C. to obtain the conductive carbon paper. The conductive carbon paper includes about 1 wt % of modified helical carbon nanotubes. When a load of 1 MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.33 g / cm 3 .
[0076] Two pieces of the conductive carbon paper were symmetrically placed on both sides of the proton exchange membrane coated with the catalyst, wherein the catalyst coating amount on both sides was 0.5 mg / cm 2 , and hot pressed at 170°C to form a membrane electrode.
[0077] The membrane electrode was sandwiched between two graphite bipolar plates with a single serpentine flow channel and polytetrafluoroethylene was used as a sealing gasket to assemble a single cell.
[0078] Finally, the membrane electrode was tested according to the aforementioned testing method to evaluate its power generation performance.
[0079] The performance test data of the conductive carbon paper and membrane electrode are shown in Table 1.
[0080] Example 2
[0081] According to the preparation method provided by the present invention, a conductive carbon paper is prepared and its performance is tested. The specific steps are as follows:
[0082] (1) The commercially available helical carbon nanotubes were heat treated in air at 200° C. for 20 min to obtain modified helical carbon nanotubes, wherein the length of the modified helical carbon nanotubes was 30-100 μm and the diameter was 10-20 nm.
[0083] (2) About 3 g of carbon fiber, 5 g of the modified helical carbon nanotubes obtained in step (1) and 3 g of polyacrylamide are placed in 1000 mL of deionized water, dispersed evenly to obtain a suspension, and a conventional papermaking method is used to prepare a carbon fiber base paper.
[0084] (3) Prepare an aqueous solution of about 20 wt% of phenolic resin to form a glue solution.
[0085] (4) Immerse the carbon fiber base paper obtained in step (2) in the glue solution in step (3) for 30 minutes.
[0086] (5) The carbon fiber base paper obtained in step (4) was dried at 120° C., then pressed at 150° C. and 1 MPa for 10 min, and then carbonized at 1800° C. for 20 min.
[0087] (6) Immersing the carbonized product in a PFA aqueous solution with a mass concentration of 8% for 5 minutes, taking it out and drying it, and then sintering it at 350° C. to obtain the conductive carbon paper. The conductive carbon paper includes about 0.5 wt % of modified helical carbon nanotubes. When a load of 1 MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.30 g / cm 3 .
[0088] Two pieces of the conductive carbon paper were symmetrically placed on both sides of the proton exchange membrane coated with the catalyst, wherein the catalyst coating amount on both sides was 0.5 mg / cm 2 , and hot pressed at 170°C to form a membrane electrode.
[0089] The membrane electrode was sandwiched between two graphite bipolar plates with a single serpentine flow channel and polytetrafluoroethylene was used as a sealing gasket to assemble a single cell.
[0090] Finally, the membrane electrode was tested according to the aforementioned testing method to evaluate its power generation performance.
[0091] The performance test data of the conductive carbon paper and membrane electrode are shown in Table 1.
[0092] Example 3
[0093] According to the preparation method provided by the present invention, a conductive carbon paper is prepared and its performance is tested. The specific steps are as follows:
[0094] (1) The commercially available helical carbon fiber is heat treated in air at 150° C. for 20 min to obtain a modified helical carbon fiber, wherein the length of the modified helical carbon fiber is 50-6000 μm and the diameter is 50 nm-10000 nm.
[0095] (2) About 1 g of carbon fiber, 50 g of the modified helical carbon fiber obtained in step (1) and 0.5 g of polyvinyl alcohol are placed in 1000 mL of deionized water, dispersed evenly to obtain a suspension, and a conventional papermaking method is used to prepare a carbon fiber base paper.
[0096] (3) Prepare a methanol solution of about 1 wt% phenolic resin to form a glue solution.
[0097] (4) Immerse the carbon fiber base paper obtained in step (2) in the glue solution in step (3) for 60 minutes.
[0098] (5) The carbon fiber base paper obtained in step (4) was dried at 120° C., then pressed at 200° C. and 3 MPa for 10 min, and then carbonized at 1500° C. for 20 min.
[0099] (6) Immersing the obtained carbon paper in a 12% mass concentration FEP aqueous solution for 5 minutes, taking it out and drying it, and then sintering it at 350° C. to obtain the conductive carbon paper. The conductive carbon paper includes about 5wt% of modified spiral carbon fibers. When a load of 1MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.34g / cm 3 .
[0100] Two pieces of the conductive carbon paper were symmetrically placed on both sides of the proton exchange membrane coated with the catalyst, wherein the catalyst coating amount on both sides was 0.5 mg / cm 2 , and hot pressed at 170°C to form a membrane electrode.
[0101] The membrane electrode was sandwiched between two graphite bipolar plates with a single serpentine flow channel and polytetrafluoroethylene was used as a sealing gasket to assemble a single cell.
[0102] Finally, the membrane electrode was tested according to the aforementioned testing method to evaluate its power generation performance.
[0103] The performance test data of the conductive carbon paper and membrane electrode are shown in Table 1.
[0104] Comparative Example 1
[0105] The difference from Example 1 is that when preparing the carbon fiber base paper, no modified helical carbon nanotubes are contained. The performance test data of the obtained conductive carbon paper and membrane electrode are shown in Table 1.
[0106] Comparative Example 2
[0107] The difference from Example 1 is that the amount of modified helical carbon nanotubes added in step (2) is 1 g, and the content of modified helical carbon nanotubes in the obtained conductive carbon paper is about 0.1 wt %. The performance test data of the obtained conductive carbon paper and membrane electrode are shown in Table 1.
[0108] Comparative Example 3
[0109] The difference from Example 1 is that the amount of modified helical carbon nanotubes added in step (2) is 150 g, and the content of modified helical carbon nanotubes in the obtained conductive carbon paper is about 15 wt %. The performance test data of the obtained conductive carbon paper and membrane electrode are shown in Table 1.
[0110] Comparative Example 4
[0111] The difference from Example 1 is that in step (2), unmodified commercially available helical carbon nanotubes are directly used, and the length of the helical carbon nanotubes is 30-100 μm and the diameter is 10-20 nm. The performance test data of the obtained conductive carbon paper and membrane electrode are shown in Table 1.
[0112] Table 1 Performance test of conductive carbon paper obtained in Examples and Comparative Examples
[0113]
[0114] As can be seen from Table 1, the resistivity of Examples 1-3 is relatively low, and the membrane electrode power generation performance is good and stable. Although the resistivity of Comparative Example 3 is also relatively low, due to the excessive amount of modified spiral carbon nanotubes added, when the carbon paper is compressed, too many modified spiral carbon nanotubes are exposed on the surface of the carbon fiber sheet, and there is obvious carbon particle shedding. The amount of modified spiral carbon nanotubes added in Comparative Example 2 is too low, resulting in a significant increase in the resistivity deviation under continuous pressure. Comparative Example 1 does not use modified spiral carbon nanotubes, and Comparative Example 4 uses unmodified spiral carbon nanotubes, and its resistivity, conductive stability and membrane electrode power generation performance are all poor.
[0115] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A conductive carbon paper, comprising carbon fibers and a binder component, characterized in that: The adhesive component contains an elasticity aid; When a load of 1 MPa is applied in the thickness direction of the carbon paper, the volume density of the carbon paper is 0.30-0.40 g / cm 3 ; The elasticity aid comprises 0.2-10 wt% of modified helical carbon nanotubes and / or modified helical carbon fibers; The modified helical carbon nanotube or modified helical carbon fiber is obtained by heat treating the helical carbon nanotube or helical carbon fiber at 150-400° C. in an oxygen-containing atmosphere.
2. The conductive carbon paper according to claim 1, characterized in that The length of the modified helical carbon nanotube is 30-100 μm and the diameter is 10-20 nm.
3. The conductive carbon paper according to claim 1, characterized in that The modified spiral carbon fiber has a length of 50-6000 μm and a diameter of 50 nm-10000 nm.
4. A method for preparing the conductive carbon paper according to any one of claims 1 to 3, characterized in that: The steps include: S1: preparing a carbon fiber base paper containing the elastic additive; S2: placing the carbon fiber base paper in a glue solution for dipping; S3: drying, curing and carbonizing the impregnated carbon fiber base paper; S4: hydrophobizing the carbonized product to obtain; In step S1, the preparation of carbon fiber base paper comprises: placing carbon fiber, elastic additive and dispersant in water, dispersing them evenly to obtain a suspension, and using a conventional papermaking method to prepare carbon fiber base paper; The mass concentration of the carbon fiber is 0.05-0.5 wt %; The mass concentration of the dispersant is 0.01-1 wt %; The elasticity aid includes modified helical carbon nanotubes and / or modified helical carbon fibers; The mass concentration of the elasticity additive is 0.2-10 wt %; The modified helical carbon nanotube or modified helical carbon fiber is obtained by heat treating the helical carbon nanotube or helical carbon fiber at 150-400° C. in an oxygen-containing atmosphere.
5. The preparation method according to claim 4, characterized in that: In step S2, the glue solution is a solution of an adhesive resin; The mass concentration of the adhesive resin solution is 0.5-30 wt %.
6. The preparation method according to claim 5, characterized in that In step S2, the mass concentration of the adhesive resin solution is 0.5-20 wt%.
7. The preparation method according to claim 4, characterized in that: In step S3, the curing is to press the dried carbon fiber base paper at 150-250° C. and 0.1-5 MPa; The carbonization temperature is 1200-2300° C., and the carbonization time is 2-30 minutes.
8. The preparation method according to claim 4, characterized in that: In step S4, the hydrophobization is to fully contact the carbonized product with a solution or dispersion of a hydrophobic material, followed by drying and heat treatment.
9. The preparation method according to claim 8, characterized in that: In step S4, the hydrophobic material includes fluorine-containing resin.
10. The preparation method according to claim 9, characterized in that: In step S4, the hydrophobic material includes one or more of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer or tetrafluoroethylene-ethylene copolymer.