A method for preparing a neodymium iron boron magnet
Through the combination technology of the dual alloy method and nano ZrO2/Zn-Al2O3 composite coating, the corrosiveness of neodymium iron boron magnets in high temperature and high humidity environments is solved, significantly improving its corrosion resistance and maintaining magnetic properties.
Patent Information
- Application Number
- CN202410480257.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-10-23
AI Technical Summary
Neodymium iron boron magnets are prone to corrosion in high temperature, high humidity or electrochemical environments, resulting in a decline in magnetic properties. The existing technology is difficult to effectively improve its corrosion resistance, especially due to the grain boundary electrochemical corrosion caused by uneven distribution of alloying elements. .
A dual alloy method is used to prepare neodymium iron boron magnets containing Ce and Ga, and a nano ZrO2/Zn-Al2O3 composite coating is prepared on its surface. Through component optimization and process step control, the corrosion resistance of the magnet is improved.
The corrosion resistance of neodymium iron boron magnets is significantly improved, while maintaining its magnetic properties. By uniformly distributing rare earth elements and forming a dense coating, it hinders the entry of corrosive media and extends the protection time of magnets in a corrosive environment.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This application is a divisional application with application number 202311370864.8, application date October 23, 2023, and invention name “A corrosion-resistant NdFeB magnet and its preparation method”. Technical Field
[0002] The invention relates to the technical field of neodymium iron boron magnets, in particular to a method for preparing a neodymium iron boron magnet. Background Art
[0003] Since its introduction in the 1980s, sintered NdFeB magnets have been widely used in many fields such as wind power generation, automotive industry and medical equipment due to their superior magnetic properties and high cost performance, playing an important role in the development of the national economy. However, NdFeB magnets have a multi-phase structure with a large potential difference between phases, especially the chemical activity of the rare earth-rich phase at the grain boundary is high. They are easily corroded at high temperature, high humidity or in contact with corrosive media, resulting in a decrease in magnetic properties, which seriously restricts the application of magnets in high temperature, high humidity, electrochemical environments and other fields that require magnets to have corrosion resistance. Therefore, the study of corrosion behavior and corrosion resistance of NdFeB magnets has become the focus of attention.
[0004] At present, the industry usually adopts alloying method and surface protection technology to improve the corrosion resistance of sintered NdFeB permanent magnet materials. For example, in the prior art, Dy element is introduced into sintered NdFeB powder by vacuum sputtering deposition, and the surface of powder particles is ground by air flow. However, this method only introduces Dy element at the grain boundary, and fails to simultaneously control the content of other alloying elements in the magnet, which easily changes the electrochemical corrosion potential of the grain boundary phase, thereby affecting the corrosion resistance. There is also a technology that utilizes the advantages of aluminum having gloss and good ductility, can form an oxide film on the surface in the air, and has excellent corrosion resistance, and aluminum is coated on the surface of NdFeB magnets. Conventional aluminum plating methods are generally ion aluminum plating and organic solution aluminum plating, but ion aluminum plating equipment is expensive and costly, and the organic solution aluminum plating electrolyte is difficult to prepare and the process is complicated. Therefore, it is urgent to find a coating technology that is simple to operate and easy to control.
[0005] The present invention uses a double alloy method to prepare a neodymium iron boron magnet containing Ce and Ga, improves the magnetic properties of the magnet by optimizing the composition, and further prepares nano ZrO 2 / Zn-Al 2 O 3 The composite coating significantly improves the corrosion resistance of NdFeB magnets while ensuring the magnetic properties of the magnets. Summary of the invention
[0006] The technical problem solved by the present invention is to provide a method for preparing a NdFeB magnet, thereby solving the problem of poor corrosion resistance of the NdFeB magnet.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A method for preparing a neodymium iron boron magnet. The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and a double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The main alloy casting sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps:
[0009] (1) The main alloy and auxiliary alloy ingots of the casting sheet are air-milled into powder with a particle size of 1-4μm, pressed into shape under a magnetic field strength of 1.8-2.2T and a pressure of 0.8-1.5MPa, cold isostatically pressed at a pressure of 150-250Mpa for 5-15min, then vacuum sintered at 1050-1150℃ for 2-5h, tempered at 900-1000℃ for 4-6h, cooled to 450-520℃, kept warm for 1-3h, and naturally cooled to room temperature to obtain NdFeB magnets.
[0010] (2) The NdFeB magnet is chamfered by a chamfering machine for 4-8 hours, alkaline washed and degreased in a sodium hydroxide solution for 10-20 minutes, ultrasonically cleaned in deionized water for 2-4 minutes, then pickled and derusted in a nitric acid solution for 0.5-1 minutes, and then ultrasonically cleaned in deionized water for 1-2 minutes. After drying with cold air, the pretreated NdFeB magnet is obtained.
[0011] (3) Add KH550 to a mixed solution of ethanol and water, add glacial acetic acid to adjust the pH of the system to 10-12, stir and hydrolyze at 30-40°C for 5-8h, and then add nano ZrO 2 Particles were ultrasonically dispersed for 2-4 hours to obtain doped nano ZrO 2 of silane solution.
[0012] (4) Zinc powder, doped nano ZrO 2The silane solution and deionized water are mixed evenly at a speed of 500-800r / min, and then a wetting agent, a dispersant, a thickener, a defoamer and high-purity alumina powder are added, and stirred at a speed of 700-950r / min for 20-50min to obtain nano ZrO 2 / Zn-Al 2 O 3 Composite coating liquid.
[0013] (5) Nano ZrO 2 / Zn-Al 2 O 3 The composite coating liquid is put into the coating bucket, the pre-treated NdFeB magnet is added into the basket, the lifting switch is operated, the basket and the sample are immersed in the coating bucket for 10-30 seconds, and then the basket is raised to leave the coating liquid, and the basket is dried at a speed of 150-300r / min, and the clockwise and counterclockwise rotations are respectively dried for 10-20 seconds to obtain NdFeB Zn-Al 2 O 3 / ZrO 2 The composite coating is pre-cured at 110-130°C for 5-15 minutes for leveling, and then cured at 230-280°C for 20-40 minutes to obtain a corrosion-resistant NdFeB magnet.
[0014] Furthermore, in step (1), the materials are calculated by weight, with the main alloy for the casting sheet accounting for 100 parts and the auxiliary alloy for the casting ingot accounting for 3-20 parts.
[0015] Furthermore, in step (2), the mass fraction of sodium hydroxide is 2-5%, and the mass fraction of nitric acid solution is 3-6%.
[0016] Furthermore, in step (3), the substances are calculated by weight: KH550 is 100 parts, nano ZrO 2 For 5-35 portions.
[0017] Furthermore, in step (4), the wetting agent is polyethylene glycol, the dispersant is AEO-9, the thickener is hydroxyethyl cellulose, and the defoaming agent is isooctyl alcohol.
[0018] Furthermore, in step (4), the substances are calculated by weight: zinc powder is 100 parts, doped nano ZrO 2 The silane solution is 10-30 parts, the deionized water is 300-500 parts, the wetting agent is 8-15 parts, the dispersant is 0.5-1.2 parts, the thickener is 0.5-0.8 parts, the defoamer is 3-6 parts, and the high-purity alumina powder is 15-25 parts.
[0019] Furthermore, the thickness of the coating in step (5) is 10-25 μm.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) Using dual alloy process: in the auxiliary alloy (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The introduction of rare earth elements such as Ce and Ga that can replace Nd reduces the enrichment and oxidation of Nd, and can be evenly dispersed in the Nd-based alloy during sintering. 14 Fe 80 B 6 A uniform liquid phase isolation layer is formed around the main alloy powder particles based on the NdFeB magnet, which improves the sintering density and coercive force of the magnet. By controlling the auxiliary alloy composition, the liquid phase can well infiltrate the main alloy phase particles, play a demagnetizing coupling role, and improve the coercive force of the NdFeB magnet.
[0022] (2) Preparation of nano ZrO 2 / Zn-Al 2 O 3 Composite coating: By preventing the external corrosive medium from directly contacting the magnet surface, the poor corrosion resistance of the magnet is fundamentally solved. 2 / Zn-Al 2 O 3 The composite coating has the passivation and physical shielding effects of the Zn-Al coating. 2 , so that it is dispersed between Zn-Al, which can not only improve the density of the coating, but also enhance the physical shielding effect of the coating, hinder the corrosive medium from entering the surface of the substrate, and further improve the corrosion resistance of NdFeB.
[0023] (3) Using dip coating-centrifugal process: Nano ZrO 2 The particles have a strong affinity, and the surface of NdFeB is coated with nano ZrO 2 / Zn-Al 2 O 3 The composite coating has no pores between the coating and the substrate, and the bonding is relatively tight. The thickness of the coating is controllable, and the coating process is immersed in the coating for a short time, causing almost no damage to the magnet itself, that is, it improves the corrosion resistance of the NdFeB magnet without affecting its magnetic properties. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The main alloy casting sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps: 100 parts of the casting sheet main alloy and 3 parts of the auxiliary alloy ingot by mass are air flow ground into a powder with a particle size of 3μm, pressed into shape under a magnetic field intensity of 2T and a pressure of 1.2MPa, cold isostatically pressed for 10min at a pressure of 200Mpa, then vacuum sintered at 1100℃ for 4h, tempered at 950℃ for 5h, cooled to 500℃, kept warm for 2h, and naturally cooled to room temperature to obtain a NdFeB magnet.
[0027] Example 2
[0028] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7The main alloy sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps: 100 parts of the main alloy of the sheet and 7 parts of the auxiliary alloy ingot by mass are air-milled into a powder with a particle size of 3 μm, pressed into shape under a magnetic field strength of 2T and a pressure of 1.2MPa, cold isostatically pressed for 10 minutes at a pressure of 200Mpa, then vacuum sintered at 1100°C for 4 hours, tempered at 950°C for 5 hours, cooled to 500°C, kept warm for 2 hours, and naturally cooled to room temperature to obtain a NdFeB magnet.
[0029] Example 3
[0030] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The main alloy casting sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps: 100 parts of the casting sheet main alloy and 11 parts of the auxiliary alloy ingot by mass are air flow ground into a powder with a particle size of 3μm, pressed into shape under a magnetic field intensity of 2T and a pressure of 1.2MPa, cold isostatically pressed for 10min at a pressure of 200Mpa, then vacuum sintered at 1100℃ for 4h, tempered at 950℃ for 5h, cooled to 500℃, kept warm for 2h, and naturally cooled to room temperature to obtain a NdFeB magnet.
[0031] Example 4
[0032] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al8 B 7 The main alloy casting sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps: 100 parts of the main alloy of the casting sheet and 15 parts of the auxiliary alloy ingot by mass are air flow ground into a powder with a particle size of 3μm, pressed into shape under a magnetic field intensity of 2T and a pressure of 1.2MPa, cold isostatically pressed for 10min at a pressure of 200Mpa, then vacuum sintered at 1100℃ for 4h, tempered at 950℃ for 5h, cooled to 500℃, kept warm for 2h, and naturally cooled to room temperature to obtain a NdFeB magnet.
[0033] Example 5
[0034] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The main alloy sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps: 100 parts of the main alloy of the sheet and 20 parts of the auxiliary alloy ingot by mass are air flow ground into a powder with a particle size of 3μm, pressed into shape under a magnetic field intensity of 2T and a pressure of 1.2MPa, cold isostatically pressed for 10min at a pressure of 200Mpa, then vacuum sintered at 1100℃ for 4h, tempered at 950℃ for 5h, cooled to 500℃, kept warm for 2h, and naturally cooled to room temperature to obtain a NdFeB magnet.
[0035] Magnetic performance test: NIM-2000 DC permanent magnet material magnetic property tester is used to measure the magnetic performance.
[0036]
[0037] It can be seen from the test results in the above table that with the increase of the content of the auxiliary alloy component in the NdFeB magnet, the magnetic properties of the magnet are improved to a certain extent. When the amount of the auxiliary alloy added is between 7% and 15%, that is, from Example 2 to Example 4, the coercive force of the magnet increases rapidly, and the remanence does not change much. Then, when the content of the auxiliary alloy is increased, the magnetic properties of the magnet decrease. This is because rare earth elements such as Ce and Ga that can replace Nd are introduced into the auxiliary alloy component. Ce and Ga are mainly distributed at the grain boundaries, which strengthen the grain boundaries. With the increase of the Ce and Ga content, the grain boundary organization and structure are changed, the grain boundaries are further strengthened, and the coercive force is also improved accordingly. In addition, a dual alloy process is adopted, and the auxiliary alloy component is controlled to make its liquid phase well infiltrated, and a continuous and uniform rare earth-rich phase thin layer is formed around the main alloy grains in the auxiliary alloy liquid phase, which plays a demagnetizing coupling role, thereby improving the coercive force of the magnet and having little effect on the remanence performance.
[0038] From the above analysis, it can be seen that the optimal addition content of the auxiliary alloy is 15%, so in the subsequent experiments, the auxiliary alloy is added at a content of 15%, and then the next test is carried out.
[0039] Example 6
[0040] The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B 6 , auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga 8 Ti 3 Cu 2 Nb 3 Al 8 B 7 The main alloy casting sheet is smelted by a vacuum rapid solidification induction furnace, and the auxiliary alloy ingot is smelted by a vacuum arc furnace. The preparation method is carried out according to the following steps:
[0041] (1) 100 parts by mass of the main alloy of the cast sheet and 15 parts of the auxiliary alloy ingot were air-milled into a powder with a particle size of 4 μm, pressed into powder under a magnetic field strength of 1.8 T and a pressure of 1.5 MPa, and cold isostatically pressed for 15 min at a pressure of 150 MPa, followed by vacuum sintering at 1150°C for 2 h, tempering at 90°C for 6 h, cooling to 520°C, keeping warm for 3 h, and naturally cooling to room temperature to obtain NdFeB magnets.
[0042] (2) The NdFeB magnet was chamfered with a chamfering machine for 4 h, alkaline washed and degreased in a 5% by mass sodium hydroxide solution for 20 min, ultrasonically cleaned in deionized water for 2 min, then pickled and derusted in a 6% by mass nitric acid solution for 0.5 min, ultrasonically cleaned in deionized water for 2 min, and dried with cold air to obtain the pretreated NdFeB magnet.
[0043] (3) Add 100 parts by mass of KH550 to a mixed solution of ethanol and water, add glacial acetic acid to adjust the pH of the system to 11, stir and hydrolyze at 35°C for 8 hours, and then add 30 parts of nano ZrO 2 The particles were dispersed by ultrasonic for 3 h to obtain doped nano ZrO 2 of silane solution.
[0044] (4) 100 parts by mass of zinc powder and 10 parts by mass of doped nano ZrO 2 Silane solution and 450 parts of deionized water were mixed at a speed of 600 r / min, and then 9 parts of polyethylene glycol, 1.1 parts of AEO-9, 0.6 parts of hydroxyethyl cellulose, 5 parts of isooctyl alcohol and 25 parts of high-purity alumina powder were added, and stirred at a speed of 950 r / min for 30 minutes to obtain nano ZrO 2 / Zn-Al 2 O 3 Composite coating liquid.
[0045] (5) Nano ZrO 2 / Zn-Al 2 O 3 The composite coating liquid is put into the coating bucket, the pre-treated NdFeB magnet is added into the basket, the lifting switch is operated, the basket and the sample are immersed in the coating bucket for 20 seconds, and then the basket is raised to leave the coating liquid, and the drying process is carried out at a speed of 220r / min, and the clockwise and counterclockwise drying are carried out for 15s each to obtain NdFeB Zn-Al 2 O 3 / ZrO 2 The composite coating has a thickness of 10 μm. The coating is pre-cured at 12° C. for 10 minutes for leveling and then cured at 240° C. for 40 minutes to obtain a corrosion-resistant NdFeB magnet.
[0046] Example 7
[0047] The difference between this embodiment and embodiment 6 is that in step (4), nano ZrO is doped 2 The amount of silane solution added was 15 parts, and other conditions remained the same.
[0048] Example 8
[0049] The difference between this embodiment and embodiment 6 is that in step (4), nano ZrO is doped 2 The amount of silane solution added was 20 parts, and other conditions remained the same.
[0050] Example 9
[0051] The difference between this embodiment and embodiment 6 is that in step (4), nano ZrO is doped 2 The amount of silane solution added was 25 parts, and other conditions remained the same.
[0052] Example 10
[0053] The difference between this embodiment and embodiment 6 is that in step (4), nano ZrO is doped 2 The amount of silane solution added was 30 parts, and other conditions remained the same.
[0054] Comparative Example 1
[0055] The difference between this comparative example and Example 6 is that in step (4), no doped nano ZrO 2 of silane solution, and other conditions remained the same.
[0056] Comparative Example 2
[0057] The difference between this comparative example and Example 6 is that the coating liquid in step (5) is doped with nano ZrO 2 of silane solution, and other conditions remained the same.
[0058] Comparative Example 3
[0059] The difference between this comparative example and Example 6 is that the NdFeB magnet obtained in step (1) is not subjected to coating treatment, and other conditions remain the same.
[0060] Corrosion resistance test: According to GB / T10124-1988 "Metallic Materials Laboratory Uniform Corrosion Full Immersion Test Method", 5% HCl solution (acidic), 3.5% NaCl solution (neutral), and 5% NaOH solution (alkaline) were selected as corrosive media. The corrosion resistance of NdFeB magnets was tested through static immersion experiments. The average corrosion rate of the magnets in different corrosive media was calculated according to the following formula.
[0061] V = (m 1 -m 2 ) / St
[0062] In the above formula: V is the average corrosion rate of the magnet, mg·mm -2 ·h -1 ;m 1 The mass of the magnet before the experiment, mg; m 2is the mass of the magnet after cleaning the corrosion products and drying, mg; S is the surface area of the magnet, mm 2 ; t is the soaking time, h.
[0063]
[0064] From the test results in the table above, we can see that NdFeB magnets coated with nano ZrO 2 / Zn-Al 2 O 3 After the composite coating, the corrosion rate is gradually reduced, and it has good corrosion resistance. However, there are certain differences in its corrosion resistance in different corrosive media: in the acidic 5% HCl solution, the average corrosion rate is the highest. This is because the HCl solution will cause double corrosion to the composite coating. First, H + The composite coating is uniformly corroded, followed by Cl - The composite coating will be pitted. In the alkaline 5% NaOH solution, the average corrosion rate is the lowest, indicating that the NaOH solution will not cause serious corrosion to the composite coating. The reason is that the composite coating will be passivated in the NaOH solution, and a passivation film with a certain protective effect will be formed on the surface, which prevents the invasion of the corrosive medium. In the neutral 3.5% NaCl solution, the average corrosion rate of the composite coating is not as fast as that in the HCl solution, but stronger than that in the NaOH solution. This is because the NaCl solution contains Cl with strong penetrability. - , which will also cause pitting corrosion to the composite coating.
[0065] Comparative Example 1 is a single Zn / Al coating, and Comparative Example 2 is a single nano ZrO 2 / silane coating, comparative example 3 is a single NdFeB magnet without coating. From the data in the above table, it can be seen that the corrosion rates of comparative examples 1 and 2 are slower than those of comparative example 3, but significantly faster than those of the embodiment, indicating that the nano ZrO prepared by the present invention 2 / Zn-Al 2 O 3 The composite coating has a synergistic anti-corrosion effect, which is due to the nano ZrO 2 / Zn-Al 2 O 3 The protective effect of the composite coating combines the passivation effect and physical shielding effect of the Zn-Al coating. 2 The doping can not only improve the density of the coating, but also enhance the physical shielding effect of the coating, hinder the corrosive medium from entering the substrate surface, prolong the protection time of the composite coating in the corrosive environment, and further improve the corrosion resistance of the magnet.
[0066] Magnetic performance test: NIM-2000 DC permanent magnet material magnetic property tester is used to measure the magnetic performance.
[0067]
[0068] From the test data in the table above, it can be seen that the coating of nano ZrO 2 / Zn-Al 2 O 3 Composite coating embodiment 10, coating nano ZrO 2 Compared with Comparative Example 1 coated with ZrO / silane, Comparative Example 2 coated with Zn-Al and Comparative Example 3 not coated with any coating, the ZrO / silane coating in Example 10 2 / Zn-Al 2 O 3 The changes in the remanence and coercivity of the composite coating magnet are very small and can be ignored, indicating that ZrO 2 The particle-modified Zn-Al coating can significantly improve the corrosion protection effect of the Zn-Al coating on sintered NdFeB magnets while ensuring the magnetic properties of the magnets.
[0069] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a neodymium iron boron magnet, characterized in that: The raw materials used are industrial pure Nd, Fe, Pr, Dy, Ce, Ga, Ti, Cu, Nb, Al and B-Fe. The ingredients are prepared according to the designed composition and the double alloy process is adopted. The main alloy component is Nd 14 Fe 80 B6, auxiliary alloy composition is (PrNdDy) 21 Fe 28 Ce 20 Ga8Ti3Cu2Nb3Al8B7, using a vacuum rapid solidification induction furnace to smelt the main alloy casting sheet, and using a vacuum arc furnace to smelt the auxiliary alloy ingot, the preparation method is carried out according to the following steps: (1) Grinding the main alloy and auxiliary alloy ingots into powder with a particle size of 1-4 μm by air flow grinding, pressing and molding under a magnetic field strength of 1.8-2.2 T and a pressure of 0.8-1.5 MPa, cold isostatic pressing for 5-15 min at a pressure of 150-250 MPa, and then vacuum sintering at 1050-1150°C for 2-5 h, tempering at 900-1000°C for 4-6 h, cooling to 450-520°C, keeping warm for 1-3 h, and naturally cooling to room temperature to obtain NdFeB magnets; (2) The NdFeB magnet is chamfered by a chamfering machine for 4-8 hours, alkaline-washed and degreased in a sodium hydroxide solution for 10-20 minutes, ultrasonically cleaned in deionized water for 2-4 minutes, then pickled and derusted in a nitric acid solution for 0.5-1 minutes, and then ultrasonically cleaned in deionized water for 1-2 minutes, and dried with cold air to obtain a pretreated NdFeB magnet; (3) Add KH550 to a mixed solution of ethanol and water, add glacial acetic acid to adjust the pH of the system to 10-12, stir and hydrolyze at 30-40°C for 5-8 hours, then add nano ZrO2 particles and ultrasonically disperse for 2-4 hours to obtain a silane solution doped with nano ZrO2; (4) After zinc powder, silane solution doped with nano-ZrO2 and deionized water are uniformly mixed at a speed of 500-800 r / min, a wetting agent, a dispersant, a thickener, a defoaming agent and high-purity alumina powder are added, and the mixture is stirred at a speed of 700-950 r / min for 20-50 min to obtain a nano-ZrO2 / Zn-Al2O3 composite coating liquid; (5) The nano ZrO2 / Zn-Al2O3 composite coating liquid is loaded into a coating bucket, and the pretreated NdFeB magnet is added into the basket. The lifting switch is operated to immerse the basket and the sample into the coating bucket for 10-30 seconds. The basket is then raised to leave the coating liquid and spun dry at a speed of 150-300 r / min for 10-20 seconds each in clockwise and counterclockwise directions to obtain a NdFeB Zn-Al2O3 / ZrO2 composite coating. The coating is pre-cured at 110-130°C for 5-15 minutes for leveling, and then cured at 230-280°C for 20-40 minutes to obtain a corrosion-resistant NdFeB magnet. In step (4), the wetting agent is polyethylene glycol, the dispersant is AEO-9, the thickener is hydroxyethyl cellulose, and the defoaming agent is isooctyl alcohol; In step (4), the substances are calculated by weight as follows: 100 parts of zinc powder, 10-30 parts of silane solution doped with nano-ZrO2, 300-500 parts of deionized water, 8-15 parts of wetting agent, 0.5-1.2 parts of dispersant, 0.5-0.8 parts of thickener, 3-6 parts of defoaming agent, and 15-25 parts of high-purity alumina powder.
2. The method for preparing a NdFeB magnet according to claim 1, wherein: The thickness of the coating in step (5) is 10-25 μm.
3. The method for preparing a NdFeB magnet according to claim 1, characterized in that: In step (1), the materials are calculated by weight: the main alloy for the casting sheet is 100 parts, and the auxiliary alloy for the casting ingot is 3-20 parts.
4. The method for preparing a NdFeB magnet according to claim 1, characterized in that: In step (2), the mass fraction of sodium hydroxide is 2-5%, and the mass fraction of nitric acid solution is 3-6%.
Citation Information
Patent Citations
A method for preparing high-performance sintered NdFeB with low dysprosium content
CN102280240A
Preparation method of high-coercivity sintered Nd-Fe-B and product
CN104505206A
Permanent magnetic material and method for producing the same
EP0249973A1
Method of forming a starting material for producing rare earth permanent magnets from recycled materials and corresponding starting material
EP4066963A1
Method for preparing high-coercivity sintered nd-fe-b and product obtained thereby
WO2016086398A1