A method for preparing a membrane electrode suitable for low humidity and low back pressure working conditions
By performing plasma doping of carbon materials and wet sulfonation treatment, a water-retaining layer is constructed with alkylimidazole-based proton-type ionic liquid, it solves the difficulty of water loss and proton conduction in fuel cell membrane electrodes under low humidity and low back pressure conditions. The problem is that the performance and stability of the membrane electrode are significantly improved.
Patent Information
- Application Number
- CN202410744968.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing fuel cell membrane electrodes are prone to water loss under low humidity and low back pressure conditions, making proton conduction difficult, resulting in rapid performance decline.
By performing plasma doping and wet sulfonation treatment on the carbon material, oxysulfur co-doped carbon material is prepared, and alkyl imidazole-based proton-type ionic liquid is added to the membrane electrode to build a water-retaining layer and enhance the water-retaining ability of the catalytic layer. and proton conduction capability.
The performance of the membrane electrode under low humidity and low back pressure conditions is significantly improved, the peak power density and current density are improved, the stable running time of the membrane electrode is extended, and performance degradation is avoided.
Smart Images

Figure CN118472285B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a fuel cell membrane electrode. Background Art
[0002] Proton exchange membrane fuel cells (PEMFC) have been widely favored by the industry due to their high energy conversion, low pollution, fast startup speed, low temperature, etc. Membrane Electrode Assembly (MEA), as the most important component of PEMFC, is mainly composed of Proton Exchange Membrane (PEM), anode / cathode catalyst layer (CL), and anode / cathode gas diffusion layer (GDL). Its characteristics directly affect the performance of PEMFC.
[0003] Water is crucial to the operation of membrane electrodes. The perfluorosulfonic acid polymer membrane used in existing fuel cell membrane electrodes and the perfluorosulfonic acid resin used as a binder in the catalyst layer need to be in a hydrated state to conduct protons well. When the water content in the membrane electrode is too low, the proton conduction ability of the perfluorosulfonic acid membrane and the perfluorosulfonic acid resin in the catalyst layer will be weakened or even disappear. Under low humidity conditions with a relative humidity (RH) of less than 20%, the membrane electrode will lose water due to the difficulty in preserving water, which will seriously affect the performance of the membrane electrode.
[0004] The catalyst layer is an important component of the membrane electrode and is the main place where chemical reactions occur. Protons are oxidized in the anode catalyst layer, transferred to the cathode catalyst layer through the proton exchange membrane, and react with oxygen at the active site of Pt. Under low back pressure conditions of hydrogen back pressure less than 115kPa and air back pressure less than 100kPa, the gas diffusion rate will be slow and the concentration of the reaction gas in the catalyst layer will be low. In a low humidity and low back pressure environment, the protons generated at the anode are difficult to conduct to the cathode, resulting in a significant decrease in the ORR reaction rate and reduced electrochemical performance of the catalyst layer.
[0005] The existing method of humidifying the membrane electrode of a proton exchange membrane fuel cell is to add hydrophilic inorganic oxide nanoparticles such as SiO2, TiO2, ZnO, Al2O3 or substances containing water-retaining groups such as polyols and polysaccharides to the catalyst layer. However, since most hydrophilic substances are non-conductors, their addition seriously affects the electron conductivity of the anode catalyst layer, increases the charge transfer impedance of the membrane electrode, and causes a significant decrease in the performance of the membrane electrode. Summary of the invention
[0006] The present invention aims to solve the problem that the existing membrane electrode is easy to lose water and has difficulty in proton conduction under low humidity and low back pressure conditions, resulting in rapid performance degradation, and to provide a method for preparing a membrane electrode suitable for low humidity and low back pressure conditions.
[0007] The preparation method of the membrane electrode adapted to low humidity and low back pressure working conditions of the present invention is carried out according to the following steps:
[0008] 1. Processing of carbon materials:
[0009] (1) Preparation of oxygen-doped carbon material: The carbon material is placed in a vacuum chamber of a chemical vapor deposition device, and the vacuum chamber is purged with high-purity argon gas for 10 to 30 minutes to ensure that there is no other residual gas when the plasma is excited, and then the carbon material is plasma treated for 20 to 60 minutes under the conditions of an argon pressure of 20 to 50 Pa and a frequency generator (RF) power of 200 to 500 W in the vacuum chamber to obtain an oxygen-doped carbon material C1;
[0010] (2) Preparation of oxygen-sulfur co-doped carbon materials:
[0011] According to the mass ratio of oxygen-doped carbon material C1, aminobenzenesulfonate and deionized water being 1: (0.2-0.8): (5-10), oxygen-doped carbon material C1, aminobenzenesulfonate and deionized water are weighed respectively and added into an ultrasonic cell disruptor, and crushed and dispersed in an ice bath for 0.5-1h to obtain a dispersion; then, under the protection of nitrogen, the dispersion is added into a reactor with a reflux device, heated to 75-90°C and kept under reflux for 12-20h; after the reaction is completed, it is washed with N,N-dimethylacetamide (DMAc) and deionized water, and vacuum dried at 60°C for 2-4h to obtain oxygen-sulfur co-doped carbon material C2;
[0012] 2. Preparation of alkyl imidazolium-based ionic liquids:
[0013] Purify 1-alkyl imidazole by distillation and then dry it with molecular sieves; mix bis(trifluoromethylsulfonyl)imide and 1-alkyl imidazole in a molar ratio of 1:(1-3) in an argon-protected glove box to obtain a mixed solution; and then place the mixed solution in a vacuum oven at a temperature of 25-30° C. and vacuum dry it for 24-48 hours to obtain a 1-alkyl imidazole bis(trifluoromethylsulfonyl)imide salt ionic liquid;
[0014] 3. Preparation of water-retaining layer slurry:
[0015] The oxygen-sulfur co-doped carbon material C2, 1-alkyl imidazole bis (trifluoromethanesulfonyl) imide salt, and the organic solvent are uniformly mixed in a mass ratio of 6:3: (30-150), and then placed in a water bath at a temperature of 60-80° C. for 1-3 hours, and cooled to room temperature to obtain slurry I;
[0016] 4. Preparation of water retention layer:
[0017] The slurry I was loaded into the ultrasonic spraying equipment, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 60-90°C. The slurry I was evenly sprayed on the cathode side of the proton exchange membrane until the mixture loading was 0.05-0.3 mg / cm 2 , this layer is the water-retaining layer;
[0018] 5. Preparation of membrane electrode catalyst layer slurry:
[0019] According to the mass ratio of Pt / C catalyst, isopropanol and deionized water of 0.01:(200-500):(300-500), Pt / C catalyst, isopropanol and deionized water are weighed and mixed evenly to obtain a mixed solution; then a Nafion solution with a mass percentage concentration of 5.% is added dropwise to the mixed solution to obtain slurry II, and the I / C ratio of slurry II is 0.7-09; wherein the I / C ratio refers to the mass ratio of the ionomer in slurry II to the carbon in the Pt / C catalyst;
[0020] 6. Preparation of membrane electrode:
[0021] (1) Preparation of cathode catalyst layer: Slurry II was loaded into ultrasonic spray equipment, and the proton exchange membrane loaded with a water-retaining layer was adsorbed on the adsorption platform of the ultrasonic spray equipment, with the water-retaining layer facing upward. The temperature of the adsorption platform was controlled at 70-90°C, and slurry II was evenly sprayed on the water-retaining layer until the Pt loading was 0.2-0.4 mg / cm 2 , this surface is used as cathode surface (C-MEA);
[0022] (2) Preparation of the anode surface: Slurry II is loaded into an ultrasonic spraying device, and the proton exchange membrane is adsorbed on the adsorption platform of the ultrasonic spraying device. The temperature of the adsorption platform is controlled at 70-90°C. Slurry II is evenly sprayed onto the other side of the proton exchange membrane until the Pt spraying loading is 0.025-0.1 mg / cm 2 , this surface is used as the anode surface (A-MEA);
[0023] (3) The sprayed membrane loaded with the water-retaining layer and the catalytic layer and the gas diffusion layer are hot-pressed at 130 to 160° C. for 3 to 5 minutes to obtain a membrane electrode adapted to low humidity and low back pressure conditions.
[0024] Furthermore, the carbon material in step 1 (1) is one or a combination of Vulcan XC-72, EC300J, EC600JD, BP2000, acetylene black, single-walled carbon nanotubes and multi-walled carbon nanotubes.
[0025] Furthermore, the aminobenzenesulfonate in step 1 (2) is one or a combination of sodium aminobenzenesulfonate, potassium aminobenzenesulfonate and magnesium aminobenzenesulfonate;
[0026] Furthermore, the 1-alkylimidazole in step 2 is 1-methylimidazole, 1-ethylimidazole or 1-butylimidazole, and the corresponding 1-alkylimidazole bis(trifluoromethylsulfonyl)imide salt is 1-methylimidazole bis(trifluoromethylsulfonyl)imide salt, 1-ethylimidazole bis(trifluoromethylsulfonyl)imide salt, 1-butylimidazole bis(trifluoromethylsulfonyl)imide salt;
[0027] Furthermore, the organic solvent in step three is one or a combination of isopropanol, ethylene glycol, N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAc).
[0028] Furthermore, the proton exchange membrane described in step 4 is a proton exchange membrane Chemours Nafion 115, Nafion 117, Nafion 212, Gore 8μm, Gore 12μm or Gore 15μm.
[0029] Furthermore, the Pt / C catalyst described in step five is JM 20% Pt / C catalyst, JM 40% Pt / C catalyst, JM50% Pt / C catalyst, JM60% Pt / C catalyst, TKK 20% Pt / C catalyst, TKK 40% Pt / C catalyst, TKK 50% Pt / C catalyst or TKK 60% Pt / C catalyst.
[0030] Furthermore, the gas diffusion layer in step six (3) is Avcarb MB30, Avcarb GDS5130 or AvcarbGDS2130.
[0031] The design of the water-retaining layer in the novel low-humidity and low-back-pressure membrane electrode of the present invention is based on the following two perspectives:
[0032] (1) The carbon material is oxygen-doped using plasma. This method can be performed at room temperature and does not require additional chemical reagents. The plasma treatment enhances the formation of oxygen vacancies on the carbon surface, thereby promoting the hydroxylation (-OH) of the material. The carbon material is sulfur-doped using aminobenzenesulfonate. After the sulfonation treatment, a large amount of sulfonate ions (-SO3 2- ). Hydroxyl (-OH) and sulfonate (-SO3 2- ) are hydrophilic groups that have strong interactions with water, and contain a large number of hydroxyl groups (-OH) and sulfonate groups (-SO3 2-) can effectively lock water molecules, inhibit the loss of water molecules in the membrane electrode under low humidity conditions, enhance the water retention capacity and water content of the catalyst layer, promote the proton dissociation and hydration of the perfluorosulfonic acid resin in the proton exchange membrane and the catalyst layer, and the transport of protons between the hydration domains at the nanoscale and the migration in the hydrogen bond network. Improve the performance of the membrane electrode under low humidity and low back pressure conditions.
[0033] (2) An alkyl imidazole-based ionic liquid is quantitatively added to the water-retaining layer. The ionic liquid has a special molecular structure and properties, and can form ligands with the hydrophilic groups doped on the carbon material, promote its interaction with water molecules, and improve the surface activity of the carbon material; and the dissociable protons contained in the ionic liquid can serve as donors of proton acids and hydrogen bonds, greatly promoting proton conduction. They have good thermal and electrochemical stability at the operating temperature and voltage of the fuel cell and can exist stably in the membrane electrode. Under low humidity conditions, the proton dissociation degree of perfluorosulfonic acid ionomers decreases sharply. Adding proton-type imidazole derivative ionic liquids to the water-retaining layer can provide more dissociated protons for the cathode catalyst layer while cooperating with the hydrophilic groups doped on the surface of the carbon material to retain water, enhance the conduction rate of protons in the catalyst layer, and facilitate the rapid transfer of protons generated at the anode to the active sites on the Pt surface to participate in the oxygen reduction reaction, so that the performance of the membrane electrode is effectively improved.
[0034] The peak power density of the membrane electrode of the present invention can reach up to 1.44 W / cm2 in a H2 / O2 environment with a back pressure of 100 kPa and a relative low humidity (RH) of 20%. 2 , which is 8.3% higher than the traditional membrane electrode. The stack polarization test shows that the current density of the invented membrane electrode reaches 1.65A / cm at 0.65V. 2 , which can be improved by 16% compared with traditional membrane electrodes and can be used in the field of proton exchange membrane fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the XPS oxygen element peak diagram of the oxygen-sulfur co-doped carbon material C2 obtained in step 1 in Example 1.
[0036] Figure 2 This is the XPS sulfur element peak diagram of the oxygen-sulfur co-doped carbon material C2 obtained in step 1 in Example 1.
[0037] Figure 3 This is a comparison chart of the water retention rates of the proton exchange membrane with a water retention layer prepared in step 4 of Examples 1 to 3 and the Gore 12 μm proton exchange membrane in Comparative Example 1.
[0038] Figure 4 Schematic diagram of the structure of a single cell assembled using the membrane electrode prepared in Examples 1 to 3 and Comparative Example 1.
[0039] Figure 5 It is the polarization curve diagram of the membrane electrode prepared by Examples 1 to 3 and Comparative Example 1 under low humidity;
[0040] Figure 6 It is a polarization curve diagram of a battery stack of a single cell assembled using the membrane electrodes prepared in Examples 1 to 3 and Comparative Example 1 under low humidity. DETAILED DESCRIPTION
[0041] The beneficial effects of the present invention are verified by the following examples.
[0042] Embodiment 1: The preparation method of the membrane electrode adapted to low humidity and low back pressure working conditions of this embodiment is carried out according to the following steps:
[0043] 1. Processing of carbon materials:
[0044] (1) Preparation of oxygen-doped carbon material: 1 g of XC-72 carbon was placed in a vacuum chamber of a BTF-1200C chemical vapor deposition device, and the vacuum chamber was purged with high-purity argon gas for 10 min to ensure that there was no other residual gas when the plasma was excited. Then, the XC-72 carbon was plasma treated for 40 min under the conditions of an argon pressure of 20 Pa and a frequency generator (RF) power of 200 W in the vacuum chamber to obtain an oxygen-doped carbon material C1.
[0045] (2) Preparation of oxygen-sulfur co-doped carbon materials:
[0046] 1 g of oxygen-doped carbon material C1, 0.8 g of sodium aminobenzenesulfonate and 8 mL of deionized water were weighed and added to a JY96-IIN ultrasonic cell disruptor, and crushed and dispersed for 0.5 h in an ice bath to obtain a dispersion; then, under the protection of nitrogen, the dispersion was added to a reactor with a reflux device, heated to 75 ° C and kept under reflux for 12 h to allow the benzenesulfonate group to fully react with the carbon; after the reaction was completed, it was filtered and washed three times with N, N-dimethylacetamide (DMAc) and deionized water in turn to remove the influence of impurities, and then dried at 60 ° C for 3 h to obtain 0.9 g of oxygen-sulfur co-doped carbon material C2;
[0047] 2. Preparation of alkyl imidazolium-based ionic liquids:
[0048] 1-Methylimidazole was purified by distillation and then dried with molecular sieves; bis(trifluoromethylsulfonyl)imide and 1-methylimidazole were mixed evenly in a molar ratio of 1:1 in an argon-protected glove box, and the treated solution was placed in a vacuum oven at a temperature of 30° C. and vacuum dried for 24 hours to obtain 1-methylimidazole bis(trifluoromethylsulfonyl)imide salt ionic liquid;
[0049] 3. Preparation of water-retaining layer slurry:
[0050] 0.6 g of oxygen-sulfur co-doped carbon material C2, 0.3 g of 1-methylimidazole bis(trifluoromethanesulfonyl)imide salt, and 18 mL of isopropanol were uniformly mixed, and then placed in a water bath at a temperature of 75°C for 2 h, and cooled to room temperature to obtain slurry I;
[0051] 4. Preparation of water retention layer:
[0052] Slurry I was loaded into the ultrasonic spraying equipment, and the Gore 12μm proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 85℃. Slurry I was evenly sprayed on the cathode side of the proton exchange membrane and monitored by XRF Hitachi detector until the mixture loading reached 0.3mg / cm 2 , this layer is the water-retaining layer;
[0053] 5. Preparation of membrane electrode catalyst layer slurry:
[0054] 0.2 mg of JM 60% Pt / C catalyst, 10 g of isopropanol and 10 g of deionized water were weighed and mixed and ultrasonically dispersed for 30 min to obtain a mixed solution; 1.6 mg of a 5% mass percent Nafion solution was then added dropwise to the mixed solution and mixed evenly to obtain slurry II;
[0055] 6. Preparation of membrane electrode:
[0056] (1) Preparation of cathode catalyst layer: Slurry II was loaded into ultrasonic spray equipment, and the proton exchange membrane loaded with a water-retaining layer was adsorbed on the adsorption platform of the ultrasonic spray equipment, with the water-retaining layer facing upward. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed on the water-retaining layer until the Pt loading reached 0.3 mg / cm 2 , this surface is used as cathode surface (C-MEA);
[0057] (2) Preparation of the anode surface: Slurry II was loaded into an ultrasonic spraying device, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying device. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed onto the other side of the proton exchange membrane until the Pt spraying loading reached 0.1 mg / cm 2 , this surface is used as the anode surface (A-MEA);
[0058] (3) The sprayed membrane loaded with the water-retaining layer and the catalytic layer and the gas diffusion layer Avcarb MB30 were hot-pressed at 150° C. for 4 min to obtain a membrane electrode adapted to low humidity and low back pressure conditions.
[0059] Example 2: The preparation of a novel membrane electrode adapted to low humidity and low back pressure conditions in this example is specifically carried out in the following steps:
[0060] 1. Processing of carbon materials:
[0061] (1) Preparation of oxygen-doped carbon material: 1 g of EC300J carbon was placed in a vacuum chamber of a BTF-1200C chemical vapor deposition device, and the vacuum chamber was purged with high-purity argon gas for 10 min to ensure that there was no other residual gas when the plasma was excited. Then, the EC300J carbon was plasma treated for 40 min under the conditions of an argon pressure of 20 Pa and a frequency generator (RF) power of 200 W in the vacuum chamber to obtain an oxygen-doped carbon material C1.
[0062] (2) Preparation of oxygen-sulfur co-doped carbon materials:
[0063] 1 g of oxygen-doped carbon material C1, 0.4 g of sodium aminobenzenesulfonate and 6 mL of deionized water were weighed and added to a JY96-IIN ultrasonic cell disruptor, and crushed and dispersed in an ice bath for 1 h to obtain a dispersion; then, under the protection of nitrogen, the dispersion was added to a reactor with a reflux device, heated to 75 ° C and kept refluxed for 12 h to allow the benzenesulfonate group to fully react with the carbon; after the reaction was completed, it was filtered and washed three times with N, N-dimethylacetamide (DMAc) and deionized water in turn to remove the influence of impurities, and then dried at a temperature of 60 ° C for 3 h to obtain 0.85 g of oxygen-sulfur co-doped carbon material C2;
[0064] 2. Preparation of alkyl imidazolium-based ionic liquids:
[0065] 1-ethylimidazole was purified by distillation and then dried with molecular sieves; bis(trifluoromethylsulfonyl)imide and 1-ethylimidazole were mixed evenly in a molar ratio of 1:1 in an argon-protected glove box, and the treated solution was placed in a vacuum oven at a temperature of 25° C. and vacuum dried for 30 hours to obtain 1-ethylimidazole bis(trifluoromethylsulfonyl)imide salt ionic liquid;
[0066] 3. Preparation of water-retaining layer slurry:
[0067] 0.6 g of oxygen-sulfur co-doped carbon material C2, 0.3 g of 1-ethylimidazole bis(trifluoromethylsulfonyl)imide salt, and 24 mL of ethylene glycol were uniformly mixed, and then placed in a water bath at 80° C. for 2 h, and cooled to room temperature to obtain slurry I;
[0068] 4. Preparation of water retention layer:
[0069] Slurry I was loaded into the ultrasonic spraying equipment, and the Gore 15μm proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 85°C. Slurry I was evenly sprayed on the cathode side of the proton exchange membrane and monitored by XRF Hitachi detector until the mixture loading reached 0.3 mg / cm 2 , this layer is the water-retaining layer;
[0070] 5. Preparation of membrane electrode catalyst layer slurry:
[0071] 0.3 mg of JM 50% Pt / C catalyst, 8 g of isopropanol, and 10 g of deionized water were weighed, mixed, and ultrasonically dispersed for 30 min to obtain a mixed solution; 1.9 mg of a 5% mass percent Nafion solution was then added dropwise to the mixed solution, and mixed evenly to obtain slurry II;
[0072] 6. Preparation of membrane electrode:
[0073] (1) Preparation of cathode catalyst layer: Slurry II was loaded into ultrasonic spray equipment, and the proton exchange membrane loaded with a water-retaining layer was adsorbed on the adsorption platform of the ultrasonic spray equipment, with the water-retaining layer facing upward. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed on the water-retaining layer until the Pt loading reached 0.3 mg / cm 2 , this surface is used as cathode surface (C-MEA);
[0074] (2) Preparation of the anode surface: Slurry II was loaded into an ultrasonic spraying device, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying device. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed onto the other side of the proton exchange membrane until the Pt spraying loading reached 0.1 mg / cm 2 , this surface is used as the anode surface (A-MEA);
[0075] (3) The sprayed membrane loaded with the water-retaining layer and the catalytic layer and the gas diffusion layer Avcarb GDS5130 are hot-pressed at 150° C. for 4 minutes to obtain a membrane electrode adapted to low humidity and low back pressure conditions.
[0076] Example 3: The preparation of a novel membrane electrode adapted to low humidity and low back pressure conditions in this example is specifically carried out in the following steps:
[0077] 1. Processing of carbon materials:
[0078] (1) Preparation of oxygen-doped carbon material: 1 g of BP2000 carbon was placed in a vacuum chamber of a BTF-1200C chemical vapor deposition device, and the vacuum chamber was purged with high-purity argon gas for 10 min to ensure that there was no other residual gas when the plasma was excited. Then, the BP2000 carbon was plasma treated for 60 min under the conditions of an argon pressure of 20 Pa and a frequency generator (RF) power of 200 W in the vacuum chamber to obtain an oxygen-doped carbon material C1.
[0079] (2) Preparation of oxygen-sulfur co-doped carbon materials:
[0080] 1 g of oxygen-doped carbon material C1, 0.8 g of sodium aminobenzenesulfonate and 8 mL of deionized water were weighed and added to a JY96-IIN ultrasonic cell disruptor, and crushed and dispersed for 1 h in an ice bath to obtain a dispersion; then, under the protection of nitrogen, the dispersion was added to a reactor with a reflux device, heated to 60 ° C and kept under reflux for 14 h to allow the benzenesulfonate group to fully react with the carbon; after the reaction was completed, it was filtered and washed three times with N, N-dimethylacetamide (DMAc) and deionized water in turn to remove the influence of impurities, and then dried at 60 ° C for 3 h to obtain 0.87 g of oxygen-sulfur co-doped carbon material C2;
[0081] 2. Preparation of alkyl imidazolium-based ionic liquids:
[0082] Purify 1-butylimidazole by distillation and then dry it with molecular sieves; mix bis(trifluoromethylsulfonyl)imide and 1-butylimidazole in a molar ratio of 1:1 in an argon-protected glove box, and place the treated solution in a vacuum oven at 30° C. for vacuum drying for 24 hours to obtain 1-butylimidazole bis(trifluoromethylsulfonyl)imide salt ionic liquid;
[0083] 3. Preparation of water-retaining layer slurry:
[0084] 0.6 g of oxygen-sulfur co-doped carbon material C2, 0.3 g of 1-butylimidazole bis(trifluoromethylsulfonyl)imide salt, and 20 mL of N,N-dimethylacetamide (DMAc) were uniformly mixed, and then placed in a water bath at 80°C for 2 h, and cooled to room temperature to obtain slurry I;
[0085] 4. Preparation of water retention layer:
[0086] Slurry I was loaded into the ultrasonic spraying equipment, and the Gore 8μm proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 85°C. Slurry I was evenly sprayed on the cathode side of the proton exchange membrane and monitored by XRF Hitachi detector until the mixture loading reached 0.3 mg / cm 2 , this layer is the water-retaining layer;
[0087] 5. Preparation of membrane electrode catalyst layer slurry:
[0088] 0.25 mg of JM 60% Pt / C catalyst, 6 g of isopropanol, and 8 g of deionized water were weighed, mixed, and ultrasonically dispersed for 30 min to obtain a mixed solution; 1.27 mg of a 5% mass percent Nafion solution was then added dropwise to the mixed solution, and mixed evenly to obtain slurry II;
[0089] 6. Preparation of membrane electrode:
[0090] (1) Preparation of cathode catalyst layer: Slurry II was loaded into ultrasonic spray equipment, and the proton exchange membrane loaded with a water-retaining layer was adsorbed on the adsorption platform of the ultrasonic spray equipment, with the water-retaining layer facing upward. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed on the water-retaining layer until the Pt loading reached 0.3 mg / cm 2 , this surface is used as cathode surface (C-MEA);
[0091] (2) Preparation of the anode surface: Slurry II was loaded into an ultrasonic spraying device, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying device. The temperature of the adsorption platform was controlled at 85°C, and slurry II was evenly sprayed onto the other side of the proton exchange membrane until the Pt spraying loading reached 0.1 mg / cm 2 , this surface is used as the anode surface (A-MEA);
[0092] (3) The sprayed membrane loaded with the water-retaining layer and the catalytic layer and the gas diffusion layer Avcarb GDS2130 are hot-pressed at 150° C. for 4 minutes to obtain a membrane electrode adapted to low humidity and low back pressure conditions.
[0093] Comparative Example 1: This comparative example is a traditional method for preparing a membrane electrode, which is specifically carried out in the following steps: weigh 0.2 mg JM60% Pt / C catalyst, 10 g isopropanol, and 10 g deionized water, mix them, and then ultrasonically disperse them for 30 minutes to make them evenly mixed to obtain a slurry. The slurry is loaded into an automatic sprayer and evenly sprayed onto both sides of a Gore 12 μm proton exchange membrane, one side being the cathode and the other side being the anode, wherein the cathode Pt loading is 0.3 mg / cm 2 , the anode Pt loading is 0.1 mg / cm 2 The sprayed membrane and the diffusion layer of Avcarb MB300 were hot pressed at 150°C for 4 minutes to obtain a traditional membrane electrode.
[0094] XPS characterization was performed on the oxygen-sulfur co-doped carbon material C2 obtained in step 1 of Example 1, and the obtained oxygen element peak diagram was as follows: Figure 1 As shown, the sulfur element peak diagram is as follows Figure 2 As shown. Figure 1 and Figure 2 It can be seen that the carbon material exhibits obvious characteristic peaks of oxygen and sulfur elements, proving that oxygen and sulfur are successfully chemically doped into the carbon material, and hydrophilic groups such as hydroxyl groups and sulfonic acid groups are introduced on the surface of the carbon material.
[0095] The proton exchange membrane with a water-retaining layer prepared in step 4 of Examples 1 to 3 and the Gore 12μm proton exchange membrane in Comparative Example 1 were placed in a vacuum drying oven at 80°C for 6 hours and the membrane weight was measured as m; then the membrane was immersed in a water bath at 80°C for 4 hours, the excess water on the surface was wiped off quickly and the weight of the membrane was measured as M. The water-retaining capacity of the membrane is expressed by the water absorption rate: ΔM(w t %)=(Mm) / m.
[0096] The water retention rates of the proton exchange membrane with a water retention layer prepared in step 4 of Examples 1 to 3 and the Gore 12 μm proton exchange membrane in Comparative Example 1 are as follows: Figure 3 As shown, from Figure 3 It can be seen that the water retention rate of the proton exchange membrane with a water retention layer in Examples 1 to 3 is 45% to 50%, which proves that the water retention performance of the water retention layer is good, while the water retention rate of the proton exchange membrane without a water retention layer in Comparative Example 1 is only 12%, and the water retention effect is poor. This shows that by adding a water retention layer, the water retention capacity of the membrane electrode can be effectively improved, which is beneficial to the low-humidity operation of the fuel cell.
[0097] The membrane electrodes prepared in Examples 1 to 3 and Comparative Example 1 were assembled into a single cell. The structural schematic diagram of the single cell is shown in FIG. Figure 4 As shown, the proton exchange membrane 1-1, the water retention layer 1-2, the cathode catalyst layer 1-3, the anode catalyst layer 1-4 and the gas diffusion layer 1-5 constitute the membrane electrode assembly 1, wherein the water retention layer 1-2 is located between the proton exchange membrane 1-1 and the cathode catalyst layer 1-3; the anode catalyst layer 1-4 is located on the other side of the proton exchange membrane 1-1, and there are gas diffusion layers 1-5 outside the cathode catalyst layer 1-3 and the anode catalyst layer 1-4; a flow field plate 2 is arranged outside the gas diffusion layer 1-5, and the membrane electrode assembly 1 and the flow field plate 2 constitute a single cell. The membrane electrode hydrogen-air polarization performance test was carried out under the national standard test conditions using the Qunyi 850e membrane electrode test system. All membrane electrodes were subjected to the following four cycles in a H2 / O2 environment with a temperature of 80°C, a back pressure of 100kPa, and a relative low humidity (RH) of 20%:
[0098] (i) Maintain a constant voltage of 0.65 V for 2 min;
[0099] (ii) Maintain a constant voltage of 0.4 V for 6 min;
[0100] (iii) maintaining a constant voltage of 0.2 V for 2 min;
[0101] (iv) The voltage was scanned from 1.0 V to 0.2 V for 2 min per point. The H2 / O2 polarization diagrams were measured from open circuit voltage (OCV) to 0.2 V for 2 min per point at a fixed flow rate of 0.5 L / min for H2 and O2, respectively.
[0102] The polarization curves of the membrane electrodes prepared in Examples 1 to 3 and Comparative Example 1 are as follows: Figure 5 As shown, from Figure 5 It can be seen that the membrane electrodes prepared in Examples 1 to 3 have higher peak power density than the conventional membrane electrode in Comparative Example 1 under the same hydrogen-air conditions; and the membrane electrodes prepared in Examples 1 to 3 effectively improve the performance degradation problem caused by water loss and improve the stability of the membrane electrode. The peak power density of the membrane electrodes prepared in Examples 1 to 3 under low humidity conditions can reach up to 1.44 W / cm 2 The peak power density of the membrane electrode prepared by the traditional method under low humidity conditions is 1.32W / cm 2 The performance of the membrane electrode prepared in Examples 1 to 3 was improved by 8.3%.
[0103] The cell stack polarization test was performed on the single cell assembled with the membrane electrode prepared in Examples 1 to 3 and Comparative Example 1, and the steps were as follows: after checking the air tightness of the cell, the open circuit potential was scanned to 0.55V, and each current was run for 3 minutes, the anode stoichiometric ratio was 1.2, the cathode stoichiometric ratio was 2.5, the humidity was 20% RH, the hydrogen back pressure was 115kPa, the air back pressure was 100kPa, the anode was set to 75°C, the cathode was set to 75°C, and the cell temperature was set to 75°C. The obtained polarization curve is as follows: Figure 6 As shown, from Figure 6 It can be seen that the performance of Examples 1 to 3 with the addition of the water-retaining layer is significantly better. At 0.65 V, the current density of the battery of Examples 1 to 3 can reach 1.65 A / cm 2 , while the current density of comparative example 1 is 1.38A / cm 2 It is proved that in Examples 1 to 3, by improving the water retention capacity of the catalyst layer, the conduction of protons from the anode to the cathode is improved, the reaction rate of the membrane electrode is promoted, and the fuel cell achieves a higher performance output.
[0104] The present invention sequentially performs ion dry oxygen doping and wet sulfonation sulfur doping treatments on carbon materials, and adds a quantitative alkyl imidazole-based ionic liquid to jointly construct a water-retaining layer in the membrane electrode between the cathode catalyst layer and the proton exchange membrane. The water-retaining layer is composed of hydroxyl groups and sulfonate ions that can lock water molecules and ionic liquids that can enhance proton conduction. It can not only enhance the ability of the membrane electrode to operate stably under low humidity and low back pressure conditions, but also reduce the charge transfer impedance of MEA, effectively improving the problem of performance degradation caused by easy water loss and difficult proton conduction of the membrane electrode under low temperature and low pressure. Compared with traditional water-retaining measures, the present invention does not affect the electron-conducting capacity of the catalyst layer, and can also significantly improve the performance of the membrane electrode.
Claims
1. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions, characterized in that The method proceeds as follows:
1. Processing of carbon materials: (1) Preparation of oxygen-doped carbon material: The carbon material was placed in a vacuum chamber of a chemical vapor deposition device, and the vacuum chamber was purged with high-purity argon gas for 10 to 30 min to ensure that there was no other residual gas when the plasma was excited. Then, the carbon material was plasma treated for 20 to 60 min under the conditions of an argon pressure of 20 to 50 Pa and a frequency generator power of 200 to 500 W in the vacuum chamber to obtain an oxygen-doped carbon material C1. (2) Preparation of oxygen-sulfur co-doped carbon materials: According to the mass ratio of oxygen-doped carbon material C1, aminobenzenesulfonate and deionized water being 1: (0.2-0.8): (5-10), oxygen-doped carbon material C1, aminobenzenesulfonate and deionized water were weighed respectively and added into an ultrasonic cell disruptor, and crushed and dispersed in an ice bath for 0.5-1 h to obtain a dispersion; then, under the protection of nitrogen, the dispersion was added into a reactor with a reflux device, heated to 75-90 °C and kept under reflux for 12-20 h; after the reaction was completed, it was washed with N,N-dimethylacetamide and deionized water, and vacuum dried at 60 °C for 2-4 h to obtain oxygen-sulfur co-doped carbon material C2; 2. Preparation of alkyl imidazolium-based ionic liquids: Purify 1-alkyl imidazole by distillation and then dry it with molecular sieves; mix bis(trifluoromethylsulfonyl)imide and 1-alkyl imidazole in a molar ratio of 1:(1-3) in an argon-protected glove box to obtain a mixed solution; then place the mixed solution in a vacuum oven at a temperature of 25-30°C and vacuum dry it for 24-48 hours to obtain 1-alkyl imidazole bis(trifluoromethylsulfonyl)imide salt ionic liquid; 3. Preparation of water-retaining layer slurry: The oxygen-sulfur co-doped carbon material C2, 1-alkyl imidazole bis (trifluoromethanesulfonyl) imide salt, and organic solvent are uniformly mixed in a mass ratio of 6:3: (30-150), and then placed in a water bath at a temperature of 60-80°C for 1-3 h, and then cooled to room temperature to obtain slurry I; 4. Preparation of water retention layer: Slurry I was loaded into the ultrasonic spraying equipment, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 60-90 °C. Slurry I was evenly sprayed on the cathode side of the proton exchange membrane until the mixture loading was 0.05-0.3 mg / cm 2 , this layer is the water-retaining layer; 5. Preparation of membrane electrode catalyst layer slurry: According to the mass ratio of Pt / C catalyst, isopropanol and deionized water of 0.01: (200-500): (300-500), Pt / C catalyst, isopropanol and deionized water are weighed and mixed evenly to obtain a mixed solution; then a Nafion solution with a mass percentage concentration of 5% is added dropwise to the mixed solution to obtain slurry II, and the I / C ratio of slurry II is 0.7-09; wherein the I / C ratio refers to the mass ratio of the ionomer in slurry II to the carbon in the Pt / C catalyst; 6. Preparation of membrane electrode: (1) Preparation of cathode catalyst layer: Slurry II was loaded into ultrasonic spray equipment, and the proton exchange membrane loaded with a water-retaining layer was adsorbed on the adsorption platform of the ultrasonic spray equipment, with the water-retaining layer facing upward. The temperature of the adsorption platform was controlled at 70-90 °C, and slurry II was evenly sprayed on the water-retaining layer until the Pt loading was 0.2-0.4 mg / cm 2 , this surface is used as cathode surface; (2) Preparation of the anode surface: Slurry II was loaded into the ultrasonic spraying equipment, and the proton exchange membrane was adsorbed on the adsorption platform of the ultrasonic spraying equipment. The temperature of the adsorption platform was controlled at 70-90 °C. Slurry II was evenly sprayed onto the other side of the proton exchange membrane until the Pt spraying loading was 0.025-0.1 mg / cm 2 , this surface is used as the anode surface; (3) The membrane loaded with the water-retaining layer and the catalytic layer after spraying and the gas diffusion layer are hot pressed at 130-160 °C for 3-5 min to obtain a membrane electrode suitable for low humidity and low back pressure conditions.
2. The method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1, characterized in that: The carbon material in step 1 (1) is one or a combination of Vulcan XC-72, EC300J, EC600JD, BP2000, acetylene black, single-walled carbon nanotubes and multi-walled carbon nanotubes.
3. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The aminobenzenesulfonate salt in step 1 (2) is one or a combination of sodium aminobenzenesulfonate, potassium aminobenzenesulfonate and magnesium aminobenzenesulfonate.
4. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The 1-alkylimidazole in step 2 is 1-methylimidazole, 1-ethylimidazole or 1-butylimidazole.
5. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The organic solvent described in step three is one or a combination of isopropanol, ethylene glycol, N,N-dimethylformamide and N,N-dimethylacetamide.
6. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The proton exchange membrane described in step 4 is a proton exchange membrane Chemours Nafion 115, Nafion 117, Nafion 212, Gore 8 µm, Gore 12 µm or Gore 15 µm.
7. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The Pt / C catalyst described in step 5 is JM 20% Pt / C catalyst, JM 40% Pt / C catalyst, JM 50% Pt / C catalyst, JM 60% Pt / C catalyst, TKK 20% Pt / C catalyst, TKK 40% Pt / C catalyst, TKK 50% Pt / C catalyst or TKK 60% Pt / C catalyst.
8. A method for preparing a membrane electrode adapted to low humidity and low back pressure conditions according to claim 1 or 2, characterized in that: The gas diffusion layer in step six (3) is Avcarb MB30, Avcarb GDS5130 or Avcarb GDS2130.
Citation Information
Patent Citations
Self-humidification membrane electrode for proton exchange membrane fuel cell and preparation method thereof
CN103078122A
Water retention layer, preparation method and application thereof, and anode water retention membrane electrode
CN116454334A
Regulation and control method for three-phase interface of catalyst layer of proton exchange membrane fuel cell
CN116845253A
Membrane electrode assembly and fuel cell
JP2009080967A
Electrode catalyst for membrane electrode of fuel cell and its method of preparation and fuel cell membrane electrode
US20120107719A1