A production process for preparing hollow fiber and elastic yarn by recycling polyester bottle flakes

Activated polyester powder is prepared by pretreatment and thermal degradation of polyester bottle flakes, and combined with reinforcing agents and modified titanium dioxide, it solves the mechanical properties and dyeing uniformity problems of hollow fiber and elastic yarn, and achieves high quality Preparation of fibers and recycling of polyester bottle flakes.

CN118480888BActive Publication Date: 2024-10-18ANHUI BAOERYING NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410936295.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-18
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

In the existing technology, hollow fibers made from recycled polyester bottle flakes and elasticized yarn have poor mechanical properties and the dyeing uniformity and color fastness need to be improved, making it difficult to meet the market's demand for high-quality fibers.

Method used

Activated polyester powder is prepared by pretreatment and thermal degradation of waste polyester bottle flakes, combined with reinforcing agent and modified titanium dioxide, and hollow fiber elastic yarn is prepared by hot stretching and twisting and then winding to improve Its mechanical properties and dyeing properties.

Benefits of technology

It achieves an improvement in the comprehensive performance of hollow fiber plus elastic yarn, improves mechanical properties, dyeing uniformity and color fastness, meets the demand for high-quality fiber, and achieves effective recycling and regeneration of polyester bottle flakes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, belongs to the technical field of fiber yarn processing, and is used to solve the technical problem that the mechanical properties, dyeing uniformity and color fastness of the hollow fiber elastic yarn prepared by recycling polyester bottle flakes in the prior art need to be further improved; the invention comprises the following steps: respectively adding activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven, and drying until the moisture of the material is less than 30ppm. The invention is a method for preparing hollow fiber elastic yarn by optimizing the regeneration of polyester bottle flakes, which not only effectively improves the mechanical properties and dyeing properties of the hollow fiber elastic yarn prepared by regenerating polyester powder, but also improves the color fastness and friction resistance of the hollow fiber elastic yarn, so as to realize the recycling of waste polyester bottle flakes to prepare high-quality fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber filament processing, and in particular to a production process for preparing hollow fiber elastic filaments by recycling polyester bottle flakes. Background Art

[0002] Polyester bottle flakes are mainly made of polyethylene terephthalate (PET), an important plastic material with good heat resistance, transparency and mechanical properties. They are widely used in the manufacture of various containers, such as beverage bottles, cooking oil bottles, etc. With the increasing awareness of environmental protection and the increasing scarcity of resources, the utilization of renewable resources has become a hot topic of global concern. As a common plastic waste, the recycling and reuse of polyester bottle flakes has important environmental and economic value.

[0003] At present, the recycling technology of polyester bottle flakes mainly includes two methods: physical recycling and chemical recycling. Physical recycling mainly converts polyester bottle flakes into recycled polyester raw materials through sorting, cleaning, crushing, melting and other steps; chemical recycling decomposes polyester bottle flakes into monomers or oligomers through chemical methods, and then generates new polyester materials through polymerization reactions. The physical recycling method is widely used because of its simple process and low cost.

[0004] Hollow fiber is a chemical fiber with a special structure, which has one or more cavities inside. Hollow fiber is usually prepared by melt spinning, that is, polyester melt is ejected through a spinneret to form primary fibers, which are then made through cooling, stretching, curling and other processes. Due to its unique structure, hollow fiber has excellent properties such as light weight, warmth retention, and breathability, and is widely used in clothing, home textiles, filtration and other fields.

[0005] However, in the prior art, when recycling polyester bottle flakes to prepare hollow fiber elastic yarns, the recycled polyester materials often contain a certain amount of impurities such as pigments, dyes, additives, etc., which will directly affect the purity and performance of the hollow fibers. In addition, when recycling polyester bottle flakes, the polyester materials need to undergo physical or chemical treatments, which may cause degradation or aging of the fibers, resulting in further reduction in the physical properties of the fibers. The mechanical properties of the recycled fibers need to be further improved. At the same time, when preparing hollow fiber elastic yarns, pigments are usually added thereto to prepare fiber yarns of different colors. However, due to the compatibility between the pigments and the fiber matrix, the dyeing uniformity and color fastness of the hollow fiber elastic yarns need to be further improved. The hollow fiber elastic yarns prepared by recycling polyester bottle flakes are difficult to meet the market demand for high-quality fibers. Summary of the invention

[0006] The purpose of the present invention is to provide a production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, which is used to solve the technical problems that the mechanical properties of the hollow fiber elastic yarn prepared by recycling polyester bottle flakes in the prior art are poor, the dyeing uniformity and color fastness of the hollow fiber elastic yarn need to be further improved, and the hollow fiber elastic yarn prepared by recycling polyester bottle flakes is difficult to meet the market demand for high-quality fibers.

[0007] The object of the present invention can be achieved by the following technical scheme: A production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, comprising the following steps:

[0008] S1. Add activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven respectively, and dry until the moisture content of the material is less than 30ppm;

[0009] S2, adding the dried activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a screw extruder, melting and extruding into a spinning machine through a metering pump, extruding from a hollow spinneret, and air-cooling and curing to obtain a hollow fiber filament crude product;

[0010] S3. The hollow fiber filament crude product is oiled with liquid paraffin and then heat-stretched to prepare the hollow fiber filament. Several groups of hollow fiber filaments are sequentially passed through a hot box and a false twister, and wound into a fiber-stretched yarn.

[0011] Further, in step S2, the weight ratio of the activated polyester powder, the reinforcing agent, the modified titanium dioxide, the pigment and the auxiliary additive is 60-80:20-30:8-14:5-7:3-4, the pigment is an inorganic pigment, and the auxiliary additive is composed of a plasticizer, a dispersant, an antioxidant and an antistatic agent in a weight ratio of 5:2:1:1; the plasticizer is a phthalate, the dispersant is one or more of calcium stearate, zinc stearate, magnesium stearate, and copper stearate, and the antioxidant is one or more of antioxidant DPPD, antioxidant PPD, and antioxidant H, The antistatic agent is octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, the temperatures of the six temperature sections of the screw extruder from the feed end to the discharge end are 280°C, 285°C, 290°C, 290°C, 290°C, and 300°C respectively, the spinning temperature of the spinning machine is 280-285°C, and the diameter of the spinneret hole is 35-45 μm; in step S3, the oiling rate of the hollow fiber filament crude product is 1-2%, the hot stretching temperature is 180-200°C, the stretching ratio is 1.5-2 times, and the false twist twist of the false twister is 2600-2800 T / M.

[0012] Furthermore, the activated polyester powder is obtained by processing the following steps:

[0013] A1. Crush the waste polyester bottle flakes and pass them through an 80-mesh sieve to prepare polyester powder;

[0014] A2, adding polyester powder and pretreatment solution into a reactor, raising the temperature of the reactor to 60-70°C, keeping the temperature for 30-50 minutes, and post-treating to obtain pretreated polyester powder;

[0015] The preparation principle of pretreated polyester powder is:

[0016] PET polyester powder is pretreated by using a mixed liquid consisting of sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water to improve the wettability and dispersibility of the polyester powder, adjust its crystallinity, and promote the thermal degradation reaction of the polyester powder through physical or chemical effects.

[0017] A3. Add the pretreated polyester powder and N-methylpyrrolidone into the reactor and stir. The temperature of the reactor is increased to 80-90°C. Stir until the system is dissolved. Add the catalyst into the reactor. The temperature of the reactor is increased to 190-200°C. Heat preservation treatment is performed for 60-80 minutes. The temperature of the reactor is reduced to 100-120°C. Add activated carbon into the reactor. Heat preservation treatment is performed for 2-3 hours. Post-treatment is performed to obtain activated polyester powder.

[0018] The preparation principle of activated polyester powder is:

[0019] Under the action of high temperature and catalyst, the pretreated polyester powder undergoes thermal degradation to generate polyester molecules modified with carboxyl groups. By controlling and optimizing the composition of the catalyst, the carboxyl content of the activated polyester powder is increased, and then it is decolorized by activated carbon to obtain activated polyester powder without pigment interference.

[0020] Further, in step A2, the pretreatment solution is composed of sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water in a dosage ratio of 10g:3g:5g:30mL:70mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with anhydrous ethanol for 3 times and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and vacuum dried to constant weight to obtain a pretreated polyester powder; in step A3, the pretreated polyester powder, N-methylpyrrole The dosage ratio of alkane, catalyst and activated carbon is 10g:100mL:0.1g:1g, the catalyst is composed of nickel chloride and molybdenum dioxide in a weight ratio of 3:1, and the post-treatment operation includes: after the reaction is completed, filtering while hot, transferring the filtrate to a reactor without a heat source and stirring, dropping purified water into the reactor, stirring for 40-60min at room temperature, filtering, washing the filter cake with purified water for 3 times and then draining, transferring the filter cake to a drying oven with a temperature of 65-75°C, and vacuum drying to constant weight to obtain activated polyester powder.

[0021] Further, the reinforcing agent is obtained by processing the following steps:

[0022] B1. Add dodecamethylcyclohexasiloxane, 5-hexenyltrimethoxysilane and emulsion into a reaction kettle and stir. Add dodecylbenzenesulfonic acid into the reaction kettle to adjust the pH value of the system to 4.2-4.8. Stir at room temperature for 30-50 minutes to obtain a polysiloxane emulsion.

[0023] The reaction equations involved in the preparation of polysiloxane emulsions include:

[0024]

[0025]

[0026] Where: “*” indicates the grafting active site of the molecular structure R, which is distinguished from other methyl groups.

[0027] The reaction principle involved in the preparation of polysiloxane emulsion is:

[0028] During the reaction, the hydrogen ions ionized from dodecylbenzenesulfonic acid can be combined with the oxygen atoms of dodecamethylcyclohexasiloxane to reduce the bond energy of the silicon-oxygen bond, thereby weakening the silicon-oxygen bond. At the same time, the dodecylbenzenesulfonate ions can attack the silicon atoms to form a nucleophilic substitution reaction, which promotes the ring opening of dodecamethylcyclohexasiloxane. The silicon cations formed by the ring-opening dodecamethylcyclohexasiloxane will be electrophilic and further attack the silicon-oxygen bonds of other molecules, resulting in more dodecamethylcyclohexasiloxane molecules opening and connecting to the chain, thereby achieving chain growth. The hydrolysis of the siloxane bonds on 5-hexenyltrimethoxysilane can condense with the hydroxyl groups on the siloxane chain segments. As dodecamethylcyclohexasiloxane is consumed, the concentration of silicon cations in the solution gradually decreases. When the concentration of silicon cations decreases to a certain level, it combines with the sulfonate ions to form a stable compound, thereby terminating the chain growth reaction, and then preparing a polysiloxane emulsion containing sulfonate ions and olefin-modified siloxane chain segments.

[0029] B2. Add 4-vinylbenzoic acid, styrene, isooctyl acrylate, dieneamine salt and emulsion into a reactor and stir. Raise the temperature of the reactor to 70-80°C. Add initiator solution dropwise into the reactor. After the reaction is initiated, add polysiloxane emulsion dropwise into the reactor at the same time. Keep the reaction warm for 3-5 hours and obtain the enhancer by post-processing.

[0030] The reaction equation involved in the preparation of the enhancer is:

[0031]

[0032] The reaction principle involved in the preparation of enhancers is:

[0033] Under the action of a free radical initiator, 4-vinylbenzoic acid, styrene, isooctyl acrylate, dienamine salt and olefin double bonds on the polysiloxane emulsion undergo free radical polymerization to prepare a reinforcing agent.

[0034] Furthermore, in step B1, the amount ratio of dodecamethylcyclohexasiloxane, 5-hexenyltrimethoxysilane and emulsion is 5g:1g:20mL; in step B2, the amount ratio of 4-vinylbenzoic acid, styrene, isooctyl acrylate, dieneamine salt, emulsion, initiator solution and polysiloxane emulsion is 2g:3g:1g:2g:40mL:2g:15mL, and the initiator solution is composed of potassium persulfate and purified water in a weight ratio of 1:3. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed 3 times with 50wt% ethanol and then dried, and the filter cake is transferred to a drying oven at a temperature of 65-75°C, and vacuum dried to constant weight to obtain an enhancer.

[0035] Furthermore, the emulsion is composed of sodium dodecylbenzene sulfonate, Tween-80, octanol polyoxyethylene ether and purified water in a weight ratio of 6g:3g:2g:200mL.

[0036] Furthermore, the preparation method of the dienamine salt is: diallylamine, epichlorohydrin and purified water are added to a reactor and stirred, the temperature of the reactor is increased to 45-50°C, the reaction is kept warm until the system is divided into two layers, the temperature of the reactor is increased to 75-85°C, the reaction is kept warm for 3-4 hours, and the dienamine salt is obtained by post-treatment.

[0037] The reaction equation for the synthesis of dienamine salts is:

[0038]

[0039] The reaction principle involved in the synthesis of dienamine salts is:

[0040] Under heating conditions, the epoxy group in epichlorohydrin reacts with the amino group of diallylamine to form an amino compound intermediate. The halogen on the amino intermediate undergoes intermolecular condensation in a high temperature environment to prepare a dienamine salt. After testing, the mass spectrum data of the dienamine salt is as follows:

[0041] m / z: 189.0970(100.0%), 191.0932(32.0%), 190.0981(9.7%), 192.0976(3.1%).

[0042] Furthermore, the dosage ratio of diallylamine and epichlorohydrin is 1 mol:1 mol, the dosage ratio of epichlorohydrin and purified water is 1 g:2 mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is kept at 75-85° C., and the solvent is evaporated under reduced pressure to obtain a dienamine salt.

[0043] Furthermore, the preparation method of the modified titanium dioxide is: titanium dioxide, 5,6-epoxyhexyltriethoxysilane, and anhydrous ethanol are added to a reactor and stirred, the temperature of the reactor is increased to 50-60°C, potassium hydroxide solution is added to the reactor, the reaction is kept warm for 2-3 hours, and the modified titanium dioxide is obtained by post-treatment.

[0044] The synthetic reaction formula of modified titanium dioxide is:

[0045]

[0046] In the formula, Titanium dioxide particles.

[0047] The reaction principle involved in the synthesis of modified titanium dioxide is:

[0048] In an alkaline environment, the siloxane bonds on 5,6-epoxyhexyltriethoxysilane are promoted to hydrolyze and react with the active groups on the surface of titanium dioxide, so that 5,6-epoxyhexyltriethoxysilane is coated and grafted on the surface of titanium dioxide molecules to form epoxy-modified modified titanium dioxide.

[0049] Furthermore, the dosage ratio of the titanium dioxide, 5,6-epoxyhexyltriethoxysilane, anhydrous ethanol and potassium hydroxide solution is 5g:2g:30mL:6mL, the concentration of the potassium hydroxide solution is 0.1mol / L, and the post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with 50wt% ethanol for 3 times and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and dried to constant weight to obtain modified titanium dioxide.

[0050] The present invention has the following beneficial effects:

[0051] 1. The polyester bottle flakes of the present invention are recycled to prepare hollow fiber elastic yarns. During the preparation process, waste polyester bottle flakes are used as raw materials, pretreated and thermally degraded to improve the molecular activity of the polyester powder, and then mixed with a reinforcing agent. Modified titanium dioxide is used as a cross-linking agent to promote molecular cross-linking of the hollow fiber and improve the mechanical properties of the hollow fiber. In addition, the modified titanium dioxide and the reinforcing agent cooperate with each other to help promote uniform dispersion of inorganic pigments in the fiber substrate and improve the color fastness and wear resistance of the hollow fiber. The hollow fiber is twisted and then wound after hot stretching, so that the comprehensive performance of the hollow fiber elastic yarn prepared by recycling polyester bottle flakes is improved, and the recycling of waste polyester bottle flakes is realized.

[0052] 2. The polyester bottle flakes of the present invention are recycled to prepare hollow fiber elastic yarns. After the polyester bottle flakes are powdered, they are pretreated to improve the wettability and dispersibility of the polyester powder, and the crystallinity thereof is adjusted, so that it is easier to be thermally degraded under the action of a catalyst during the heat treatment process, thereby increasing the carboxyl content on the activated polyester powder molecules; 4-vinylbenzoic acid, styrene, isooctyl acrylate, dieneamine salt and polysiloxane undergo free radical polymerization under the action of an initiator to form a reinforcing agent with a polyolefin structure, a large number of benzene rings introduced into the reinforcing agent molecules help to increase the rigidity of the reinforcing agent, and the modified polysiloxane chain segments and isooctane long alkane side chains on the reinforcing agent molecules help to increase the flexibility of the plasticizer, optimize the rigid chain segments and flexible composition of the reinforcing agent, so that the reinforcing agent and the activated polyester powder cooperate with each other to improve the mechanical properties of the hollow fiber; the carboxyl groups on the reinforcing agent and the activated polyester powder molecules undergo condensation reaction with the epoxy groups on the modified titanium dioxide to form a multi-dimensional cross-linked structure with the titanium dioxide as an anchor point, thereby further improving the mechanical properties of the material.

[0053] 3. The polyester bottle flakes of the present invention are recycled to prepare hollow fiber elastic yarns. The prepared diene amine salt is used as the synthetic monomer of the reinforcing agent. Its diene structure can promote the intermolecular crosslinking of the reinforcing agent, making the connection between the reinforcing agent molecules tighter and firmer, thereby enhancing the overall strength, toughness and durability of the reinforcing agent. When the reinforcing agent is combined with the activated polyester powder, it can more effectively withstand and disperse the external stress, thereby improving the physical properties of the polyester fiber. In addition, the higher crosslinking degree can make the reinforcing agent better dispersed in the activated polyester powder, reduce the agglomeration phenomenon, and thus improve The compatibility between the two further improves the overall performance of the fiber; when preparing hollow fiber filaments, modified titanium dioxide is used as a reinforcing agent and a cross-linking agent to enhance the cross-linking degree of the fiber filaments. At the same time, similar compatibility is used to promote the uniform dispersion of inorganic fillers and titanium dioxide in the matrix. The sulfonic acid groups and amine salts on the reinforcing agent molecules enhance the polarity and stability of the hollow fiber matrix, thereby enhancing the bonding performance between the polar inorganic filler and the hollow fiber matrix, making the inorganic filler more firmly bonded to the vacuum fiber matrix, and improving the color fastness and wear resistance of the material. DETAILED DESCRIPTION

[0054] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] Example 1

[0056] This embodiment provides a production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, comprising the following steps:

[0057] S1. Preparation of activated polyester powder

[0058] The waste polyester bottle flakes are crushed and passed through an 80-mesh sieve to prepare polyester powder;

[0059] Sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water were mixed uniformly in an amount ratio of 10 g: 3 g: 5 g: 30 mL: 70 mL to obtain a pretreatment solution for standby use;

[0060] The polyester powder was completely immersed in a reactor containing a pretreatment solution, the reactor temperature was raised to 60°C, and the temperature was kept for 30 minutes. After the reaction was completed, the reactor temperature was lowered to room temperature, and the filter cake was filtered, and the filter cake was washed with anhydrous ethanol for 3 times and then dried. The filter cake was transferred to a drying oven at a temperature of 65°C and vacuum dried to constant weight to obtain the pretreated polyester powder;

[0061] Weigh: 500g of pretreated polyester powder and 5L of N-methylpyrrolidone are added to the reactor and stirred. The temperature of the reactor is raised to 80°C and stirred until the system is dissolved. 5g of catalyst is added to the reactor. The temperature of the reactor is raised to 190°C and the reactor is kept warm for 60min. The temperature of the reactor is lowered to 100°C. 50g of activated carbon is added to the reactor and kept warm for 2h. After the reaction is completed, it is filtered while hot. The filtrate is transferred to a reactor without a heat source and stirred. Purified water is added dropwise to the reactor and stirred at room temperature for 40min. The filter cake is washed 3 times with purified water and then dried. The filter cake is transferred to a drying oven at a temperature of 65°C and vacuum dried to constant weight to obtain activated polyester powder, wherein the catalyst is composed of nickel chloride and molybdenum dioxide in a weight ratio of 3:1.

[0062] S2. Preparation of Dienamine Salt

[0063] Weigh: 97.2 g of diallylamine, 92.5 g of epichlorohydrin and 185 mL of purified water, add into a reactor and stir, raise the temperature of the reactor to 45°C, and keep warm until the system is separated into two layers, raise the temperature of the reactor to 75°C, and keep warm for 3 hours. After the reaction is completed, keep the temperature of the reactor at 75°C, and evaporate the solvent under reduced pressure to obtain a dienamine salt.

[0064] S3. Preparation of enhancer

[0065] Sodium dodecylbenzene sulfonate, Tween-80, octanol polyoxyethylene ether and purified water were uniformly mixed in a weight ratio of 6g:3g:2g:200mL to obtain an emulsion for standby use;

[0066] Weigh: 30 g of dodecamethylcyclohexasiloxane, 6 g of 5-hexenyltrimethoxysilane, and 120 mL of emulsion, add them into a reactor and stir, add dodecylbenzenesulfonic acid into the reactor to adjust the pH of the system to 4.2, stir at room temperature for 30 min, and obtain a polysiloxane emulsion;

[0067] Weigh: 40g of 4-vinylbenzoic acid, 60g of styrene, 20g of isooctyl acrylate, 40g of dieneamine salt and 800mL of emulsion, add them into a reactor and stir, raise the temperature of the reactor to 70°C, add 40g of initiator solution dropwise into the reactor, after the reaction is initiated, add 300mL of polysiloxane emulsion dropwise into the reactor at the same time, and keep the reaction warm for 3h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50wt% ethanol 3 times and then drain, transfer the filter cake to a drying oven at a temperature of 65°C, and vacuum dry to constant weight to obtain an enhancer, wherein the initiator solution consists of potassium persulfate and purified water in a weight ratio of 1:3.

[0068] S4. Preparation of modified titanium dioxide

[0069] Weigh: 20 g of titanium dioxide, 8 g of 5,6-epoxyhexyltriethoxysilane, and 120 mL of anhydrous ethanol, add into the reactor and stir, raise the temperature of the reactor to 50°C, add 24 mL of 0.1 mol / L potassium hydroxide solution into the reactor, and keep warm for 2 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50 wt% ethanol 3 times and then drain, transfer the filter cake to a drying oven at 65°C, and dry to constant weight to obtain modified titanium dioxide.

[0070] S5. Preparation of hollow fiber with elastic yarn

[0071] Dioctyl phthalate, calcium stearate, antioxidant DPPD and octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate are uniformly mixed in a weight ratio of 5:2:1:1 to obtain an auxiliary additive for standby use;

[0072] Add activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven respectively, and dry until the moisture content of the material is less than 30ppm;

[0073] After drying, weigh: 600g of activated polyester powder, 200g of reinforcing agent, 80g of modified titanium dioxide, 50g of inorganic pigment and 30g of auxiliary additives are added to a screw extruder, and the temperatures of the six temperature sections of the screw extruder from the feed end to the discharge end are 280°C, 285°C, 290°C, 290°C, 290°C, and 300°C, respectively, and are melt-extruded into a spinning machine through a metering pump, and the spinning temperature is set to 280°C, and extruded from a hollow spinneret with a spinneret hole having a diameter of 35 μm, and air-cooled and solidified to obtain a hollow fiber filament crude product;

[0074] The hollow fiber filament crude product was oiled with liquid paraffin and then heat-stretched to prepare a hollow fiber finished product, wherein the hollow fiber oiling rate was 1%, the heat-stretching temperature was 180°C, and the stretching ratio was 1.5 times;

[0075] A plurality of groups of hollow fiber filaments are put into a heating box with a temperature of 100°C and then enter a false twister. After being twisted by the false twister, the fiber is wound to form a fiber with a stretch yarn, wherein the twist of the false twister is 2600T / M.

[0076] Example 2

[0077] This embodiment provides a production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, comprising the following steps:

[0078] S1. Preparation of activated polyester powder

[0079] The waste polyester bottle flakes are crushed and passed through an 80-mesh sieve to prepare polyester powder;

[0080] Sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water were mixed uniformly in an amount ratio of 10 g: 3 g: 5 g: 30 mL: 70 mL to obtain a pretreatment solution for standby use;

[0081] The polyester powder was completely immersed in a reactor containing a pretreatment solution, the reactor temperature was raised to 65°C, and the temperature was kept for 40 minutes. After the reaction was completed, the reactor temperature was lowered to room temperature, and the filter cake was filtered, and the filter cake was washed with anhydrous ethanol for 3 times and then dried. The filter cake was transferred to a drying oven at a temperature of 70°C and vacuum dried to constant weight to obtain the pretreated polyester powder;

[0082] Weigh: 500g of pretreated polyester powder and 5L of N-methylpyrrolidone are added to the reactor and stirred. The temperature of the reactor is raised to 85°C and stirred until the system is dissolved. 5g of catalyst is added to the reactor, the temperature of the reactor is raised to 195°C, and the reactor is kept warm for 70min. The temperature of the reactor is lowered to 110°C, 50g of activated carbon is added to the reactor, and the reactor is kept warm for 2.5h. After the reaction is completed, it is filtered while hot, and the filtrate is transferred to a reactor without a heat source and stirred. Purified water is added dropwise to the reactor, and stirred for 50min at room temperature. Filter, wash the filter cake with purified water 3 times and then drain it. The filter cake is transferred to a drying oven at a temperature of 70°C and vacuum dried to constant weight to obtain activated polyester powder, wherein the catalyst is composed of nickel chloride and molybdenum dioxide in a weight ratio of 3:1.

[0083] S2. Preparation of Dienamine Salt

[0084] Weigh: 97.2 g of diallylamine, 92.5 g of epichlorohydrin and 185 mL of purified water, add into a reactor and stir, raise the temperature of the reactor to 47°C, and keep warm until the system is separated into two layers, raise the temperature of the reactor to 80°C, and keep warm for 3.5 hours. After the reaction is completed, keep the temperature of the reactor at 80°C, and evaporate the solvent under reduced pressure to obtain a dienamine salt.

[0085] S3. Preparation of enhancer

[0086] Sodium dodecylbenzene sulfonate, Tween-80, octanol polyoxyethylene ether and purified water were uniformly mixed in a weight ratio of 6g:3g:2g:200mL to obtain an emulsion for standby use;

[0087] Weigh: 30 g of dodecamethylcyclohexasiloxane, 6 g of 5-hexenyltrimethoxysilane, and 120 mL of emulsion, add them into a reactor and stir, add dodecylbenzenesulfonic acid into the reactor to adjust the pH of the system to 4.5, stir at room temperature for 40 min, and obtain a polysiloxane emulsion;

[0088] Weigh: 40g of 4-vinylbenzoic acid, 60g of styrene, 20g of isooctyl acrylate, 40g of dieneamine salt and 800mL of emulsion, add them into a reactor and stir, raise the temperature of the reactor to 75°C, add 40g of initiator solution dropwise into the reactor, after the reaction is initiated, add 300mL of polysiloxane emulsion dropwise into the reactor at the same time, and keep the reaction for 4h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50wt% ethanol 3 times and then drain, transfer the filter cake to a drying oven at a temperature of 70°C, and vacuum dry to constant weight to obtain an enhancer, wherein the initiator solution consists of potassium persulfate and purified water in a weight ratio of 1:3.

[0089] S4. Preparation of modified titanium dioxide

[0090] Weigh: 20 g of titanium dioxide, 8 g of 5,6-epoxyhexyltriethoxysilane, and 120 mL of anhydrous ethanol, add into the reactor and stir, raise the temperature of the reactor to 55°C, add 24 mL of 0.1 mol / L potassium hydroxide solution into the reactor, and keep warm for 2.5 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50 wt% ethanol three times and then drain, transfer the filter cake to a drying oven at 70°C, and dry to constant weight to obtain modified titanium dioxide.

[0091] S5. Preparation of hollow fiber with elastic yarn

[0092] Di-n-octyl phthalate, zinc stearate, antioxidant PPD and octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate are uniformly mixed in a weight ratio of 5:2:1:1 to obtain an auxiliary additive for standby use;

[0093] Add activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven respectively, and dry until the moisture content of the material is less than 30ppm;

[0094] After drying, weigh: 700g of activated polyester powder, 250g of reinforcing agent, 110g of modified titanium dioxide, 60g of inorganic pigment and 35g of auxiliary additives are added to a screw extruder, and the temperatures of the six temperature sections of the screw extruder from the feed end to the discharge end are 280°C, 285°C, 290°C, 290°C, 290°C, and 300°C, respectively, and are melt-extruded into a spinning machine through a metering pump, and the spinning temperature is set to 283°C, and extruded from a hollow spinneret with a spinneret hole having a diameter of 40μm, and air-cooled and solidified to obtain a hollow fiber filament crude product;

[0095] The hollow fiber filament crude product was oiled with liquid paraffin and then heat-stretched to prepare a hollow fiber finished product, wherein the hollow fiber oiling rate was 1.5%, the heat-stretching temperature was 190° C., and the stretching ratio was 1.7 times;

[0096] A plurality of groups of hollow fiber filaments are passed through a heating box with a temperature of 115°C and then enter a false twister. After being twisted by the false twister, the fiber is wound and formed to obtain a fiber-stretched yarn, wherein the twist of the false twister is 2700T / M.

[0097] Example 3

[0098] This embodiment provides a production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, comprising the following steps:

[0099] S1. Preparation of activated polyester powder

[0100] The waste polyester bottle flakes are crushed and passed through an 80-mesh sieve to prepare polyester powder;

[0101] Sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water were mixed uniformly in an amount ratio of 10 g: 3 g: 5 g: 30 mL: 70 mL to obtain a pretreatment solution for standby use;

[0102] The polyester powder was completely immersed in a reactor containing a pretreatment solution, the reactor temperature was raised to 70°C, and the temperature was kept for 50 minutes. After the reaction was completed, the reactor temperature was lowered to room temperature, and the filter cake was filtered, and the filter cake was washed with anhydrous ethanol for 3 times and then dried. The filter cake was transferred to a drying oven at a temperature of 75°C and vacuum dried to constant weight to obtain the pretreated polyester powder;

[0103] Weigh: 500g of pretreated polyester powder and 5L of N-methylpyrrolidone are added to the reactor and stirred. The temperature of the reactor is raised to 90°C and stirred until the system is dissolved. 5g of catalyst is added to the reactor. The temperature of the reactor is raised to 200°C and the reactor is kept warm for 80min. The temperature of the reactor is lowered to 120°C. 50g of activated carbon is added to the reactor and kept warm for 3h. After the reaction is completed, it is filtered while hot. The filtrate is transferred to a reactor without a heat source and stirred. Purified water is added dropwise to the reactor and stirred at room temperature for 60min. The filter cake is washed 3 times with purified water and then dried. The filter cake is transferred to a drying oven at a temperature of 75°C and vacuum dried to constant weight to obtain activated polyester powder, wherein the catalyst is composed of nickel chloride and molybdenum dioxide in a weight ratio of 3:1.

[0104] S2. Preparation of Dienamine Salt

[0105] Weigh: 97.2 g of diallylamine, 92.5 g of epichlorohydrin and 185 mL of purified water, add into a reactor and stir, raise the temperature of the reactor to 50°C, and keep warm until the system is separated into two layers, raise the temperature of the reactor to 85°C, and keep warm for 4 hours. After the reaction is completed, keep the temperature of the reactor at 85°C, and evaporate the solvent under reduced pressure to obtain a dienamine salt.

[0106] S3. Preparation of enhancer

[0107] Sodium dodecylbenzene sulfonate, Tween-80, octanol polyoxyethylene ether and purified water were uniformly mixed in a weight ratio of 6g:3g:2g:200mL to obtain an emulsion for standby use;

[0108] Weigh: 30 g of dodecamethylcyclohexasiloxane, 6 g of 5-hexenyltrimethoxysilane, and 120 mL of emulsion, add them into a reactor and stir, add dodecylbenzenesulfonic acid into the reactor to adjust the pH of the system to 4.8, stir at room temperature for 50 min, and obtain a polysiloxane emulsion;

[0109] Weigh: 40g of 4-vinylbenzoic acid, 60g of styrene, 20g of isooctyl acrylate, 40g of dieneamine salt and 800mL of emulsion, add them into a reactor and stir, raise the temperature of the reactor to 80°C, add 40g of initiator solution dropwise into the reactor, after the reaction is initiated, add 300mL of polysiloxane emulsion dropwise into the reactor at the same time, and keep the reaction for 5h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50wt% ethanol 3 times and then drain, transfer the filter cake to a drying oven at a temperature of 75°C, and vacuum dry to constant weight to obtain an enhancer, wherein the initiator solution consists of potassium persulfate and purified water in a weight ratio of 1:3.

[0110] S4. Preparation of modified titanium dioxide

[0111] Weigh: 20 g of titanium dioxide, 8 g of 5,6-epoxyhexyltriethoxysilane, and 120 mL of anhydrous ethanol, add into the reactor and stir, raise the temperature of the reactor to 60°C, add 24 mL of 0.1 mol / L potassium hydroxide solution into the reactor, and keep warm for 3 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 50 wt% ethanol 3 times and then dry it, transfer the filter cake to a drying oven at 75°C, and dry it to constant weight to obtain modified titanium dioxide.

[0112] S5. Preparation of hollow fiber with elastic yarn

[0113] Diisobutyl phthalate, magnesium stearate, antioxidant H and octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate are uniformly mixed in a weight ratio of 5:2:1:1 to obtain an auxiliary additive for standby use;

[0114] Add activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven respectively, and dry until the moisture content of the material is less than 30ppm;

[0115] After drying, weigh: 800g of activated polyester powder, 300g of reinforcing agent, 140g of modified titanium dioxide, 70g of inorganic pigment and 40g of auxiliary additives are added to a screw extruder, the temperatures of the six temperature sections of the screw extruder from the feed end to the discharge end are 280°C, 285°C, 290°C, 290°C, 290°C, 300°C, melt-extruded into a spinning machine through a metering pump, the spinning temperature is set to 285°C, extruded from a hollow spinneret with a spinneret hole diameter of 45μm, air-cooled and solidified, and a hollow fiber filament crude product is obtained;

[0116] After the hollow fiber filament crude product was oiled with liquid paraffin, it was heat-stretched to prepare a hollow fiber finished product, wherein the hollow fiber oiling rate was 2%, the heat-stretching temperature was 200°C, and the stretching ratio was 2 times;

[0117] A plurality of groups of hollow fiber filaments are passed through a heating box with a temperature of 130°C and then enter a false twister. After being twisted by the false twister, the fiber is wound and formed to obtain a fiber-stretched yarn, wherein the twist of the false twister is 2800T / M.

[0118] Comparative Example 1

[0119] The difference between this comparative example and Example 3 is that in step S1, the pretreatment operation of the polyester powder is cancelled, and the polyester powder is used instead of the pretreated polyester powder to participate in the preparation of the activated polyester powder.

[0120] Comparative Example 2

[0121] The difference between this comparative example and Example 3 is that in step S1, when preparing the activated polyester powder, the catalyst is molybdenum dioxide.

[0122] Comparative Example 3

[0123] The difference between this comparative example and Example 3 is that step S2 is eliminated and no dienamine salt is added in step S3.

[0124] Comparative Example 4

[0125] The difference between this comparative example and Example 3 is that step S4 is eliminated, and the titanium dioxide in step S4 replaces the modified titanium dioxide in step S5.

[0126] Performance Test:

[0127] The breaking strength, breaking elongation, curl shrinkage, curl stability, dyeing uniformity, color fastness and wear resistance of the hollow fiber elastic yarn prepared in Examples 1-3 and Comparative Examples 1-4 were tested, wherein the breaking strength, breaking elongation, curl shrinkage, curl stability and dyeing uniformity of the samples were tested with reference to the standard GB / T 14460-2015 "Polyester low-elastic yarn", and the color fastness of the samples was spun into standard samples for testing according to the standards GB / T 3921-2008 "Textiles - Tests for Color Fastness - Color Fastness to Soaping" and GB / T 3920-2008 "Textiles - Tests for Color Fastness - Color Fastness to Rubbing", and the color fastness to soaping and the color fastness to rubbing of the samples were rated according to the standard GB / T 6151-2016 "General Rules for Tests for Color Fastness of Textiles", and the wear resistance was tested with reference to the standard GB / T 21196.2-2007 "Determination of the abrasion resistance of textiles by the Martindale method - Part 2: Determination of specimen damage" The specimen is spun into a standard specimen to determine the number of frictions when the specimen is worn. The specific test results are shown in Table 1 below:

[0128]

[0129] Data Analysis:

[0130] Comparative analysis of the data in the above table shows that the fracture strength of the hollow fiber elastic yarn sample prepared by the present invention reaches 5.31 cN / detx, the fracture elongation reaches 46.2%, the curl shrinkage reaches 15.6%, the curl stability reaches 86.8%, the dyeing uniformity (gray card) reaches level 5, the color fastness to soaping reaches level 5, the color fastness to friction reaches level 5, and the number of times the sample is rubbed to wear reaches 82710 times. All the performances are better than those of the comparative example, which shows that the present invention prepares activated polyester powder by pre-treating and thermally degrading the polyester powder in sequence, and then cooperates with the reinforcing agent, modified titanium dioxide and inorganic pigment to effectively improve the mechanical properties and dyeing properties of the hollow fiber elastic yarn prepared with the activated polyester powder as the basic material, and also improves the color fastness and friction resistance of the hollow fiber elastic yarn, improves the comprehensive performance of the hollow fiber elastic yarn prepared by recycling polyester bottle flakes, and realizes the recycling of waste polyester bottle flakes.

[0131] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0132] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0133] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes, characterized in that: The following steps are involved: S1. Add activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a drying oven respectively, and dry until the moisture content of the material is less than 30ppm; S2, adding the dried activated polyester powder, reinforcing agent, modified titanium dioxide, pigment and auxiliary additives into a screw extruder, melting and extruding into a spinning machine through a metering pump, extruding from a hollow spinneret, and air-cooling and curing to obtain a hollow fiber filament crude product; S3, using liquid paraffin to oil the hollow fiber filament crude product and then heat stretch it to prepare hollow fiber filaments, and passing several groups of hollow fiber filaments through a hot box and a false twister in sequence, and winding and forming them to obtain fiber-stretched yarns; The activated polyester powder is obtained by processing the following steps: A1. Crush the waste polyester bottle flakes and pass them through an 80-mesh sieve to prepare polyester powder; A2, adding polyester powder and pretreatment solution into a reactor, raising the temperature of the reactor to 60-70°C, heat preservation treatment for 30-50min, and post-treating to obtain pretreated polyester powder, wherein the pretreatment solution is composed of sodium carbonate, sodium dodecyl sulfate, polyethylene glycol 200, tetrahydrofuran and purified water in a dosage ratio of 10g:3g:5g:30mL:70mL; A3, adding the pretreated polyester powder and N-methylpyrrolidone to the reactor and stirring, raising the temperature of the reactor to 80-90°C, stirring until the system is dissolved, adding the catalyst to the reactor, raising the temperature of the reactor to 190-200°C, and heat preservation for 60-80min, lowering the temperature of the reactor to 100-120°C, adding activated carbon to the reactor, and heat preservation for 2-3h. After the reaction is completed, filtering while hot, the filtrate is transferred to a reactor without a heat source and stirred, and purified water is added dropwise to the reactor, stirred at room temperature for 40-60min, filtered, the filter cake is washed 3 times with purified water and then drained, and the filter cake is transferred to a drying oven at a temperature of 65-75°C, and vacuum dried to constant weight to obtain activated polyester powder, wherein the amount ratio of the pretreated polyester powder, N-methylpyrrolidone, catalyst and activated carbon is 10g:100mL:0.1g:1g, and the catalyst is composed of nickel chloride and molybdenum dioxide in a weight ratio of 3:1; The reinforcing agent is obtained by processing the following steps: B1. Add dodecamethylcyclohexasiloxane, 5-hexenyltrimethoxysilane and emulsion into a reaction kettle and stir. Add dodecylbenzenesulfonic acid into the reaction kettle to adjust the pH value of the system to 4.2-4.

8. Stir at room temperature for 30-50 minutes to obtain a polysiloxane emulsion. B2, adding 4-vinylbenzoic acid, styrene, isooctyl acrylate, dieneamine salt and emulsion into a reaction kettle and stirring, raising the temperature of the reaction kettle to 70-80°C, dropping initiator solution into the reaction kettle, and after the reaction is initiated, dropping polysiloxane emulsion into the reaction kettle at the same time, keeping the temperature for reaction for 3-5h, and post-processing to obtain an enhancer; The preparation method of the modified titanium dioxide is as follows: titanium dioxide, 5,6-epoxyhexyltriethoxysilane and anhydrous ethanol are added into a reaction kettle and stirred, the temperature of the reaction kettle is increased to 50-60° C., potassium hydroxide solution is added into the reaction kettle, the reaction is carried out by heat preservation for 2-3 hours, and the modified titanium dioxide is obtained by post-processing.

2. The production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes according to claim 1, characterized in that: In step S2, the weight ratio of the activated polyester powder, the reinforcing agent, the modified titanium dioxide, the pigment and the auxiliary additive is 60-80:20-30:8-14:5-7:3-4, the pigment is an inorganic pigment, and the auxiliary additive is composed of a plasticizer, a dispersant, an antioxidant and an antistatic agent in a weight ratio of 5:2:1:

1. The spinning temperature of the spinning machine is 280-285°C, and the diameter of the spinneret hole is 35-45 μm; in step S3, the oiling rate of the hollow fiber filament crude product is 1-2%, the hot stretching temperature is 180-200°C, the stretching ratio is 1.5-2 times, and the false twist twist of the false twister is 2600-2800T / M.

3. The production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes according to claim 1, characterized in that: In step B1, the dosage ratio of dodecamethylcyclohexasiloxane, 5-hexenyltrimethoxysilane and emulsion is 5g:1g:20mL; in step B2, the dosage ratio of 4-vinylbenzoic acid, styrene, isooctyl acrylate, dienamine salt, emulsion, initiator solution and polysiloxane emulsion is 2g:3g:1g:2g:40mL:2g:15mL, and the initiator solution is composed of potassium persulfate and purified water in a weight ratio of 1:

3.

4. The production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes according to claim 1, characterized in that: The emulsion is composed of sodium dodecylbenzene sulfonate, Tween-80, octanol polyoxyethylene ether and purified water in a weight ratio of 6g:3g:2g:200mL.

5. The production process for preparing hollow fiber elastic yarn by recycling polyester bottle flakes according to claim 1, characterized in that: The preparation method of the dienamine salt is as follows: diallylamine, epichlorohydrin and purified water are added into a reaction kettle and stirred, the temperature of the reaction kettle is increased to 45-50° C., the reaction is carried out by heat preservation until the system is divided into two layers, the temperature of the reaction kettle is increased to 75-85° C., the reaction is carried out by heat preservation for 3-4 hours, and the dienamine salt is obtained by post-treatment.

Citation Information

Patent Citations

  • Preparation method of low-melting-point regenerated copolyester

    CN104327259A