A honeycomb activated carbon adsorbent

Through the composite preparation of cork powder, coal-based carbon powder, coconut shell carbon powder and nickel/cobalt hydroxide sheet layer, the problems of honeycomb activated carbon adsorption holes and the singleness of raw materials are solved, and its adsorption performance and sewage treatment are improved. Effect.

CN118491482BActive Publication Date: 2024-11-19广东韩研活性炭科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410911200.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-19
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The adsorption holes of existing honeycomb activated carbons are easily blocked by adhesives, and the single bituminous coal raw material leads to a decrease in adsorption capacity, making it impossible to effectively adsorb large molecules and small molecules in organic waste gas, and the treatment effect is poor.

Method used

Using the composite preparation method of cork powder, coal-based carbon powder and coconut shell carbon powder, the micropore diversity and adsorption capacity of activated carbon are improved by loading rod-shaped nano calcium carbonate and nickel/cobalt hydroxide sheets, and the adsorption of ammonia nitrogen is enhanced. ability.

Benefits of technology

It significantly improves the adsorption performance of honeycomb activated carbon, enhances the removal ability of COD and ammonia nitrogen, and improves the sewage purification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118491482B_ABST
    Figure CN118491482B_ABST
Patent Text Reader

Abstract

The invention discloses a honeycomb activated carbon adsorbent, which belongs to the field of activated carbon technology. The preparation of the honeycomb activated carbon adsorbent includes the following steps: taking cork powder and firing and modifying it in a nitrogen atmosphere to obtain cork charcoal powder; taking cork charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant to mix to obtain coal slime; vacuuming and shaping the coal slime to obtain wet honeycomb charcoal, carbonizing and activating to obtain honeycomb activated carbon; loading rod-shaped calcium carbonate to obtain material B; taking hexahydrated cobalt nitrate, hexahydrated nickel nitrate, hexadecyltrimethylammonium bromide, methanol, and deionized water to mix, stir to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep it warm and stand in a nitrogen atmosphere, cool to room temperature, wash, and dry to obtain a honeycomb activated carbon adsorbent with excellent adsorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of activated carbon, and in particular relates to a honeycomb type activated carbon adsorbent. Background Art

[0002] COD stands for Chemical Oxygen Demand, which refers to the amount of oxidant consumed when a certain strong oxidant is used to treat a water sample under certain conditions. COD is an indicator of the amount of reducing substances in water, and the reducing substances in water include various organic substances, nitrites, sulfides, ferrous salts, etc., but the main ones are organic substances. The amount of organic substances in sewage is much greater than that of inorganic substances. Therefore, COD is generally used to represent the total amount of organic substances in sewage. Excessive ammonia nitrogen content and COD in water have serious harm to the environment and human life. If water with high ammonia nitrogen content is discharged into natural water bodies, algae such as blue algae and green algae will grow in large quantities, and then a large amount of dissolved oxygen in the water will be consumed, causing fish and other aquatic organisms in the water to die of lack of oxygen. If COD is too high, it will cause the death of almost all organisms except microorganisms, destroy the ecosystem of the water body, and further cause the water body to stink anaerobicly, thereby making the water body lose its use function and further affecting the surrounding environment. It can be seen that it is very necessary to treat sewage.

[0003] With the continuous improvement of environmental protection requirements, sewage purification issues have attracted more and more attention. Honeycomb activated carbon is often used as an adsorbent for sewage purification, but honeycomb activated carbon is mainly processed with bituminous coal as a raw material to generate honeycomb activated carbon with a certain adsorption capacity. However, due to the use of traditional process methods, the adsorption pores of the honeycomb activated carbon are easily blocked by adhesives, resulting in a decrease in the adsorption capacity of the activated carbon. On the other hand, since the honeycomb activated carbon uses pure bituminous coal as a raw material, the micropore diameter of bituminous coal is relatively single and the scope of application is limited, resulting in the inability to adsorb large and small molecular gases in organic waste gas, resulting in poor treatment effect. Summary of the invention

[0004] The object of the present invention is to provide a honeycomb type activated carbon adsorbent for improving the adsorption performance of the honeycomb type activated carbon.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0007] S1. Take cork powder in a nitrogen atmosphere, keep it at 350-400°C for 0.5-1h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30-40min, let it stand for 12-14h, and dry it to obtain cork charcoal powder;

[0008] S2, taking the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, MQ-92 lubricant (purchased from Wuhan Meiqilin New Materials Co., Ltd.) and mixing them, stirring in a blender for 4-6 hours to obtain coal slime;

[0009] S3, conveying the coal slime to a vacuum mud mixer and mixing for 3-4 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon;

[0010] S4, configuration calcium ion concentration is 0.1mol / L clear lime water, add concentration is 0.2mol / L magnesium chloride solution, stir 15-20min, make material A, the honeycomb type activated carbon is impregnated in the material A, transfer in a sealed kettle, pass into carbon dioxide gas with a flow rate of 170mL / min to pH 7.2-7.4 under 75-85 ℃ of heating conditions, stop ventilation, cool to room temperature after aging 6-8h, filter, take solid phase drying, make material B;

[0011] S5. Mix cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 10-15 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep it warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb type activated carbon adsorbent.

[0012] As a preferred technical solution of the present invention, in step S1, the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2-4g:1-2g:50mL; and the volume fraction of the ethanol aqueous solution is 50%.

[0013] As a preferred technical solution of the present invention, in step S2, the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25-35:30-40:10-15:15-25:20-30:3-4:2-3.

[0014] As a preferred technical solution of the present invention, in step S3, the drying refers to drying until the water volume content in the wet honeycomb carbon is 3-5%.

[0015] As a preferred technical solution of the present invention, in step S3, the carbonization refers to firing at 500-600° C. for 1-2 hours.

[0016] As a preferred technical solution of the present invention, in step S3, the activation refers to activation with water vapor at 750-850° C. for 8-12 hours.

[0017] As a preferred technical solution of the present invention, in step S4, the ratio of the clarified lime water, magnesium chloride solution and honeycomb activated carbon is 70-80L: 1-2L: 1-1.2cm 3 .

[0018] As a preferred technical solution of the present invention, in step S5, the dosage ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water, and material B is 1.2-1.5mmol:1.4-1.6mmol:1-1.2g:50-70mL:15-20mL:1.2-1.5cm 3 .

[0019] As a preferred technical solution of the present invention, in step S5, the heat preservation and standing refers to standing at 180° C. for 20-30 hours.

[0020] Beneficial effects of the present invention:

[0021] The honeycomb activated carbon adsorbent disclosed in the present invention is prepared by mixing softwood charcoal powder, coal charcoal powder and coconut shell charcoal powder, so that the prepared activated carbon has various micropore types and the adsorption effect is improved; by loading rod-shaped nano calcium carbonate on the surface of the activated carbon as a supporting site, the nickel / cobalt hydroxide sheet layer is firmly attached to the surface of the activated carbon, thereby improving its adsorption capacity; by introducing nickel / cobalt hydroxide nanosheet layers, it has abundant surface active sites and can provide more adsorption sites for adsorbing ammonia nitrogen molecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below in conjunction with the accompanying drawings.

[0023] Figure 1 is a SEM image of the honeycomb type activated carbon adsorbent prepared in Example 1 of the present invention;

[0024] Figure 2 is a SEM image of the honeycomb type activated carbon prepared in Example 1 of the present invention;

[0025] Figure 3 It is a SEM image of material B prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0027] Example 1

[0028] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0029] S1. Take cork powder in a nitrogen atmosphere, keep it at 350°C for 0.5h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30min, let it stand for 12h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2g:1g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0030] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25:30:10:15:20:3:2;

[0031] S3, conveying the coal sludge to a vacuum mud making machine for mixing for 3 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 3%; the carbonization refers to firing at 500° C. for 1 hour; the activation refers to activating it with water vapor at 750° C. for 8 hours;

[0032] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 15min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.2 under 75°C heating condition, stop ventilation, cool to room temperature and age for 6h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 70L:1L:1cm 3 ;

[0033] S5. Mix cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 10 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb activated carbon adsorbent; the dosage ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water and material B is 1.2mmol:1.4mmol:1g:50mL:15mL:1.2cm 3 The heat preservation and standing refers to standing at 180°C for 20 hours.

[0034] As attached Figure 1 As shown in FIG. 1 , it is a SEM image of the honeycomb activated carbon adsorbent prepared in Example 1 of the present application. It can be clearly seen from the image that the nickel / cobalt hydroxide flakes are attached to the surface of the activated carbon. Figure 2 As shown in the figure, micropores of several pore sizes can be seen. By compounding a variety of carbon powders, the diversity of the pore sizes of the activated carbon is increased. Figure 3 As shown, there are many rod-shaped protrusions on the surface of activated carbon, which means that nano-calcium carbonate is loaded on the surface of activated carbon.

[0035] Example 2

[0036] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0037] S1. Take cork powder in a nitrogen atmosphere, keep it at 380℃ for 0.8h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 35min, let it stand for 13h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 3g:1.5g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0038] S2, mix the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stir in a blender for 4-6 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 30:35:12:20:25:3.5:2.5;

[0039] S3, conveying the coal slime to a vacuum mud making machine for mixing for 3.5 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 4%; the carbonization refers to firing at 550°C for 1.5 hours; the activation refers to activating it with water vapor at 800°C for 10 hours;

[0040] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 18min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.3 under 80°C heating condition, stop ventilation, cool to room temperature and age for 7h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 75L:1.5L:1.1cm 3;

[0041] S5. Mix cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 12 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb type activated carbon adsorbent; the dosage ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water and material B is 1.4mmol:1.5mmol:1.1g:60mL:18mL:1.4cm 3 The heat preservation and standing refers to standing at 180°C for 25 hours.

[0042] Example 3

[0043] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0044] S1. Take cork powder in a nitrogen atmosphere and keep it at 400°C for 1 hour, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 40 minutes, let it stand for 14 hours, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 4g:2g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0045] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 6 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 35:40:15:25:30:4:3;

[0046] S3, conveying the coal slime to a vacuum mud making machine for mixing for 4 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 5%; the carbonization refers to firing at 600° C. for 2 hours; the activation refers to activating it with water vapor at 850° C. for 12 hours;

[0047] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 20min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.4 under 85°C heating condition, stop ventilation, cool to room temperature and age for 8h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 80L:2L:1.2cm 3 ;

[0048] S5. Mix cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 15 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb type activated carbon adsorbent; the dosage ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water and material B is 1.5mmol:1.6mmol:1.2g:70mL:20mL:1.5cm 3 The heat preservation and standing refers to standing at 180°C for 30 hours.

[0049] Comparative Example 1

[0050] The difference from Example 1 is that no sodium hydroxide is added in step S1.

[0051] Comparative Example 2

[0052] The difference from Example 1 is that the mass ratio of the softwood charcoal powder, coal charcoal powder and coconut shell charcoal powder in step S2 is 0:30:35.

[0053] Comparative Example 3

[0054] The difference from Example 1 is that the mass ratio of the softwood charcoal powder, coal charcoal powder and coconut shell charcoal powder in step S2 is 25:0:40.

[0055] Comparative Example 4

[0056] The difference from Example 1 is that the mass ratio of the softwood charcoal powder, coal charcoal powder and coconut shell charcoal powder in step S2 is 25:40:0.

[0057] Comparative Example 5

[0058] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0059] S1. Take cork powder in a nitrogen atmosphere, keep it at 350°C for 0.5h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30min, let it stand for 12h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2g:1g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0060] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25:30:10:15:20:3:2;

[0061] S3, conveying the coal sludge to a vacuum mud making machine for mixing for 3 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 3%; the carbonization refers to firing at 500° C. for 1 hour; the activation refers to activating it with water vapor at 750° C. for 8 hours;

[0062] S4, take cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, and deionized water, mix them, stir for 10 minutes, and obtain material C, immerse the honeycomb type activated carbon in the material C, transfer it to a hydrothermal kettle, keep it warm and stand it in a nitrogen atmosphere, cool it to room temperature, wash it, and dry it to obtain the honeycomb type activated carbon adsorbent; the dosage ratio of the cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water, and honeycomb type activated carbon is 1.2mmol:1.4mmol:1g:50mL:15mL:1.2cm 3 The heat preservation and standing refers to standing at 180°C for 20 hours.

[0063] Comparative Example 6

[0064] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0065] S1. Take cork powder in a nitrogen atmosphere, keep it at 350°C for 0.5h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30min, let it stand for 12h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2g:1g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0066] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25:30:10:15:20:3:2;

[0067] S3, conveying the coal sludge to a vacuum mud making machine for mixing for 3 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 3%; the carbonization refers to firing at 500° C. for 1 hour; the activation refers to activating it with water vapor at 750° C. for 8 hours;

[0068] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 15min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.2 under 75°C heating condition, stop ventilation, cool to room temperature and age for 6h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 70L:1L:1cm 3 ;

[0069] S5. Take nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, and deionized water, mix them, stir for 10 minutes, and obtain material C. The material B is immersed in the material C, transferred to a hydrothermal kettle, kept warm and allowed to stand in a nitrogen atmosphere, cooled to room temperature, washed, and dried to obtain the honeycomb type activated carbon adsorbent; the dosage ratio of the nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water, and material B is 2.6mmol:1g:50mL:15mL:1.2cm 3 The heat preservation and standing refers to standing at 180°C for 20 hours.

[0070] Comparative Example 7

[0071] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0072] S1. Take cork powder in a nitrogen atmosphere, keep it at 350°C for 0.5h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30min, let it stand for 12h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2g:1g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0073] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25:30:10:15:20:3:2;

[0074] S3, conveying the coal sludge to a vacuum mud making machine for mixing for 3 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 3%; the carbonization refers to firing at 500° C. for 1 hour; the activation refers to activating it with water vapor at 750° C. for 8 hours;

[0075] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 15min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.2 under 75°C heating condition, stop ventilation, cool to room temperature and age for 6h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 70L:1L:1cm 3 ;

[0076] S5. Mix cobalt nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 10 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb activated carbon adsorbent; the dosage ratio of cobalt nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water and material B is 2.6mmol:1g:50mL:15mL:1.2cm 3 The heat preservation and standing refers to standing at 180°C for 20 hours.

[0077] Comparative Example 8

[0078] A honeycomb type activated carbon adsorbent, wherein the preparation method of the honeycomb type activated carbon adsorbent comprises the following steps:

[0079] S1. Take cork powder in a nitrogen atmosphere, keep it at 350°C for 0.5h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30min, let it stand for 12h, and dry it to obtain cork charcoal powder; the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2g:1g:50mL; the volume fraction of the ethanol aqueous solution is 50%;

[0080] S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4 hours to obtain coal slurry; the mass ratio of the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25:30:10:15:20:3:2;

[0081] S3, conveying the coal sludge to a vacuum mud making machine for mixing for 3 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; the drying refers to drying until the water volume content of the wet honeycomb carbon is 3%; the carbonization refers to firing at 500° C. for 1 hour; the activation refers to activating it with water vapor at 750° C. for 8 hours;

[0082] S4, configure the clear lime water with calcium ion concentration of 0.1mol / L, add the magnesium chloride solution with concentration of 0.2mol / L, stir for 15min, make material A, impregnate the honeycomb type activated carbon in the material A, transfer to a sealed kettle, pass carbon dioxide gas with a flow rate of 170mL / min to pH 7.2 under 75°C heating condition, stop ventilation, cool to room temperature and age for 6h, filter, take solid phase and dry, make material B; the dosage ratio of the clear lime water, magnesium chloride solution and honeycomb type activated carbon is 70L:1L:1cm 3 ;

[0083] Performance Testing

[0084] The activated carbon products prepared in Examples 1-3 and Comparative Examples 1-8 prepared on the basis of Example 1 were used to treat the sewage sampled on the same day, with the standard of adding 2 g of the finished activated carbon product per liter of sewage; according to the test method specified in the "Water and Wastewater Monitoring and Analysis Methods" (Fourth Edition), a UV-visible spectrophotometer model Q-6 of Shanghai Yuanxi Instrument Co., Ltd. was used to perform COD detection and ammonia nitrogen detection on the sewage treated in Examples 1-3 and Comparative Examples 1-8, respectively, to obtain the corresponding removal rate;

[0085] The results are shown in Table 1 below:

[0086] Table 1 Water sample COD, ammonia nitrogen removal rate test results

[0087]

[0088] It can be seen from Table 1 that the honeycomb activated carbon adsorbents prepared in Examples 1-3 of the present application have good adsorption performance; since the cork powder in Comparative Example 1 is not activated with sodium hydroxide, its specific surface area is low and the adsorption performance is reduced; since Comparative Examples 2-4 lack the synergistic effect among cork charcoal powder, coal charcoal powder and coconut shell charcoal powder, the pore size of the activated carbon micropores is relatively single and the adsorption performance is reduced; Comparative Example 5 does not load rod-shaped nano-calcium carbonate on the surface of the activated carbon, resulting in a lack of supporting sites, so that the subsequent loaded nickel / cobalt hydroxide flakes cannot be firmly attached to the surface of the activated carbon, and the adsorption performance is reduced; Comparative Examples 6-8 show that it is through the presence of nickel / cobalt hydroxide flakes that the adsorption effect of activated carbon is improved.

[0089] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A honeycomb activated carbon adsorbent, characterized in that: The preparation method of the honeycomb type activated carbon adsorbent comprises the following steps: S1. Take cork powder in a nitrogen atmosphere, keep it at 350-400°C for 0.5-1h, cool it, mix it with sodium hydroxide and ethanol aqueous solution, stir it for 30-40min, let it stand for 12-14h, and dry it to obtain cork charcoal powder; S2, mixing the softwood charcoal powder, coal charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant, and stirring in a blender for 4-6 hours to obtain coal slurry; S3, conveying the coal slime to a vacuum mud mixer and mixing for 3-4 hours, and then conveying it to an extruder of a honeycomb steel mold for molding to obtain wet honeycomb carbon, and then drying it, carbonizing and activating it in a nitrogen atmosphere to obtain honeycomb activated carbon; S4, configuration calcium ion concentration is 0.1mol / L clear lime water, add concentration is 0.2mol / L magnesium chloride solution, stir 15-20min, make material A, the honeycomb type activated carbon is impregnated in the material A, transfer in a sealed kettle, pass into carbon dioxide gas with a flow rate of 170mL / min to pH 7.2-7.4 under 75-85 ℃ of heating conditions, stop ventilation, cool to room temperature after aging 6-8h, filter, take solid phase drying, make material B; S5. Mix cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol and deionized water, stir for 10-15 minutes to obtain material C, immerse the material B in the material C, transfer to a hydrothermal kettle, keep it warm and stand in a nitrogen atmosphere, cool to room temperature, wash and dry to obtain the honeycomb type activated carbon adsorbent.

2. A honeycomb type activated carbon adsorbent according to claim 1, characterized in that: In step S1, the dosage ratio of the cork powder, sodium hydroxide and ethanol aqueous solution is 2-4g:1-2g:50mL; the volume fraction of the ethanol aqueous solution is 50%.

3. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S2, the mass ratio of the softwood charcoal powder, coal-based charcoal powder, coconut shell charcoal powder, deionized water, coal tar, polyurethane adhesive, and MQ-92 lubricant is 25-35:30-40:10-15:15-25:20-30:3-4:2-3.

4. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S3, the drying refers to drying until the water volume content in the wet honeycomb carbon is 3-5%.

5. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S3, the carbonization refers to firing at 500-600° C. for 1-2 hours.

6. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S3, the activation refers to activation with water vapor at 750-850° C. for 8-12 hours.

7. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S4, the ratio of the clarified lime water, magnesium chloride solution and honeycomb activated carbon is 70-80 L: 1-2 L: 1-1.2 cm 3 .

8. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S5, the dosage ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, hexadecyltrimethylammonium bromide, methanol, deionized water, and material B is 1.2-1.5 mmol: 1.4-1.6 mmol: 1-1.2 g: 50-70 mL: 15-20 mL: 1.2-1.5 cm 3 .

9. The honeycomb activated carbon adsorbent according to claim 1, characterized in that: In step S5, the heat preservation and standing refers to standing at 180° C. for 20-30 hours.