Composite film, lithium metal battery and application thereof

By using a composite film of gradient pore size structure and anthraquinone functional groups in lithium metal batteries, the problem of lithium dendrites is solved, the circulation performance and safety of lithium batteries are improved, and the service life of the battery is extended.

CN118493959BActive Publication Date: 2024-11-05天能新能源(湖州)有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961515.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-05
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Lithium metal negative electrode materials are prone to form lithium dendrites during the charge and discharge cycle, resulting in a reduction in battery safety and energy density. The prior art is difficult to effectively inhibit the generation of lithium dendrites by optimizing the SEI film.

Method used

A composite film is designed, including a multilayer film structure, gradient pore size and anthraquinone functional group separation layer, which inhibits the formation of lithium dendrites by guiding the uniform deposition of lithium ions and stabilizing their transmission path.

Benefits of technology

It significantly improves the circulation performance and safety of lithium batteries, extends the battery life, and ensures the integrity of the battery structure through the high mechanical and chemical stability of polyamide anthraquinone modified materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118493959B_ABST
    Figure CN118493959B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery material technology, and specifically to a composite membrane, a lithium metal battery and applications. The present application can optimize the transmission path and deposition mode of lithium ions by setting a gradient pore structure and providing a separation layer containing anthraquinone functional groups, thereby achieving faster ion transmission and more uniform lithium ion deposition, effectively inhibiting the formation of lithium dendrites on the surface of the lithium metal negative electrode, and significantly improving the cycle effect and safety of the lithium battery. On this basis, the present application further enhances the mechanical strength and chemical stability of the composite membrane by selecting the separation layer material, and can achieve long-term spatial confinement of lithium dendrites. The polymer phase distribution of the polyamide anthraquinone modified material is highly uniform, which accelerates the uniform migration of lithium ions in the membrane and improves the conductivity and cycle stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a composite film, a lithium metal battery and applications. Background Art

[0002] In recent years, the rapid rise of electric vehicles and energy storage technology has not only opened up a wider application space for the lithium-ion battery market, but also put forward higher requirements for the energy density and service life of lithium-ion batteries. As the core component of lithium batteries, negative electrode materials are the most critical factor in determining battery energy density and service life.

[0003] Compared with traditional carbon-based negative electrode materials, lithium metal negative electrode materials are regarded as the first choice for high energy density battery negative electrodes due to their high specific capacity and low electrochemical potential. However, the current lithium metal negative electrode technology still faces a major challenge, namely the battery safety caused by the formation of lithium dendrites. The so-called lithium dendrite refers to the dendritic metal lithium deposition structure formed by the uneven reduction of lithium ions on the surface of the lithium metal negative electrode during the charge and discharge cycle. Since lithium ions tend to deposit in the electron-dense area of ​​lithium dendrites, as the charge and discharge cycle continues, lithium dendrites will continue to extend to the positive electrode, and eventually penetrate the diaphragm inside the battery, contact the positive electrode, cause a battery short circuit, and affect the safety of the product. At the same time, the formation of lithium dendrites will also reduce the content of active lithium, affect the energy density and service life of the battery, and hinder its application in actual production.

[0004] In order to alleviate the excessive generation of lithium dendrites and improve the performance of lithium metal negative electrodes, lithium metal negative electrode batteries on the market mainly improve their performance by optimizing the solid electrolyte interface (SEI) film. In essence, the SEI film is a film formed by the reaction of lithium ions with byproducts in the electrolyte (such as anions, impurities, etc.) during the charging process of the lithium battery, and then accumulated on the surface of the lithium metal negative electrode. Generally, this kind of film is not completely dense and has poor mechanical properties. In order to increase the stability of the SEI film, the components of the battery electrolyte are often improved, such as adding SEI film-forming additives to the electrolyte, so as to promote the in-situ generation of a more stable SEI film during the electrochemical behavior of lithium metal. However, the biggest disadvantage of this method is that the mechanical modulus of the constructed SEI is small, which is not enough to inhibit the damage of lithium dendrites to the SEI film. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a new type of composite film. By setting the composite film on the surface of the lithium metal negative electrode, the uniform deposition of lithium ions can be promoted, the growth of lithium dendrites can be inhibited, and the cycle performance of the battery cell can be improved. This is specifically achieved through the following technical solutions:

[0006] A composite membrane, comprising at least two membrane layers; the membrane layers are provided with pores and ion channels for lithium ions to pass through are formed between the pores of each membrane layer; the pore sizes of each membrane layer are arranged to decrease unidirectionally along the thickness direction of the composite membrane; the membrane layer at the end of the composite membrane with a smaller pore size is a separation layer, the separation layer is used to connect with the surface of a lithium metal negative electrode, and the separation layer material contains anthraquinone functional groups.

[0007] This application optimizes the transmission path and deposition mode of lithium ions by setting a gradient pore structure and providing a separation layer containing anthraquinone functional groups, which can achieve faster ion transmission and more uniform lithium ion deposition, effectively inhibit the formation of lithium dendrites on the surface of lithium metal negative electrodes, and significantly improve the cycle effect and safety of lithium batteries. Specifically:

[0008] From the perspective of structural design, the present application sets two or more membrane layers with unidirectional pore size gradients, and utilizes the ion flow channels formed by the pores between the membrane layers to guide lithium ions to migrate toward the lithium metal negative electrode in a more orderly and uniform manner. During the discharge of the battery, the lithium ions inside the positive electrode material are gradually deintercalated and migrate to the negative electrode under the mediation of the electrolyte. Affected by various factors, in fact, the lithium ions are disorderly distributed when they reach the side of the composite membrane close to the positive electrode. The ion flow channels with different pore sizes on different membrane layers of the present application can realize the step-by-step screening of lithium ions, prompting the lithium ions to tend to be evenly distributed in the process of passing through the composite membrane, laying the foundation for the lithium ions to pass through the separation layer and be uniformly deposited on the lithium metal surface.

[0009] From the perspective of material selection, the present application designs a separation layer containing anthraquinone functional groups at a special position of the contact interface between the composite membrane and the lithium metal negative electrode, which can further promote the balanced permeation of lithium ions through the composite membrane and evenly deposit and distribute on the surface of the lithium metal negative electrode by means of the interaction between the anthraquinone functional group and the lithium ions. The carbonyl group in the anthraquinone functional group is a dipole that can have a strong ion-dipole interaction with lithium ions. When the surface of the lithium metal negative electrode locally reaches the critical point of deposition, the anthraquinone functional group stabilizes the dissociation state of lithium ions through its unique chemical properties, preventing lithium ions from being unnecessarily reduced to the lithium metal form, thereby effectively curbing the formation of lithium dendrites. At the same time, the anthraquinone structure can also serve as an anchor point, guided by ion-dipole interactions, ensuring that lithium ions are evenly configured near the separation layer, thereby promoting the deposition of lithium ions in areas that have not reached saturation. This design significantly alleviates the problems triggered by the local excess concentration of lithium ions, and provides a strong guarantee for improving the safety and cycle stability of the battery system. In addition, the anthraquinone functional group has a strong affinity for lithium, which can promote the lithium ion conduction process to a certain extent.

[0010] Preferably, the separation layer material is a polyamide anthraquinone modified material.

[0011] The polyamide anthraquinone modified material of the present application has excellent mechanical strength, and can effectively resist mechanical stress when the battery undergoes multiple charge and discharge cycles, prevent membrane damage and the formation of lithium dendrites, and ensure the stability and safety of the battery structure. On this basis, its excellent chemical stability ensures that even in long-term electrochemical reactions, it can resist the corrosion of the electrolyte to a great extent, reduce the occurrence of side reactions, maintain the integrity of the protective film, and significantly extend the service life of the battery. In addition, the polymer phase distribution of the polyamide anthraquinone modified material is highly uniform, which accelerates the uniform migration of lithium ions in the membrane and improves the conductivity and cycle stability of the battery.

[0012] Preferably, the polyamide anthraquinone modified material is obtained by polymerizing a material comprising a first monomer, a second monomer and a third monomer; wherein: the first monomer is selected from piperazine and / or diamine; the second monomer is selected from acyl chloride; and the third monomer is selected from sulfonyl chloride containing anthraquinone functional group.

[0013] Preferably, the separation layer material further comprises a phosphate functional group; the raw material for preparing the polyamide anthraquinone modified material further comprises a fourth monomer, and the fourth monomer is selected from amino phosphate.

[0014] This technical solution can improve the thermal stability of the separation layer by cleverly integrating phosphate functional groups into the separation layer material.

[0015] Preferably, the diamine includes at least one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, xylylenediamine, ethylenediamine, propylenediamine, 1,3-diaminocyclohexane and 1,2-diaminocyclohexane; the acyl chloride includes at least one of isophthaloyl chloride, terephthaloyl chloride and 1,3,5-trimesoyl chloride; the third monomer includes at least one of anthraquinone-2,6-disulfonyl chloride and 9,10-anthraquinone-2-sulfonyl chloride; and the aminophosphoric acid salt is 2,2′-diaminobibenzyl diphosphate.

[0016] Preferably, the membrane layer further comprises a buffer layer and a support layer sequentially arranged on one side of the separation layer; the pore size of the separation layer is 0.5-1 nm; the pore size of the buffer layer is 0.2-0.4 μm; the pore size of the support layer is 0.4-0.8 μm. Preferably, the material of the buffer layer is selected from polyethylene or polypropylene; the material of the support layer is selected from cellulose membrane or non-woven fabric.

[0017] Preferably, the separation layer has a thickness of 60-75 nm, the buffer layer has a thickness of 5-20 μm, and the support layer has a thickness of 20-50 μm.

[0018] Preferably, the porosity of the composite membrane is 38-63%, wherein the porosity of the separation layer is 20-40%, the porosity of the buffer layer is 30-50%, and the porosity of the support layer is 50-70%.

[0019] Application of any of the above composite films in lithium metal batteries.

[0020] The present application also provides a lithium metal battery, wherein a composite film as described above is arranged between the positive and negative electrodes of the lithium metal battery.

[0021] Compared with the prior art, this application has the following beneficial effects:

[0022] This application can optimize the transmission path and deposition pattern of lithium ions by setting a gradient pore structure and providing a separation layer containing anthraquinone functional groups, achieve faster ion transmission and more uniform lithium ion deposition, effectively inhibit the formation of lithium dendrites on the surface of the lithium metal negative electrode, and significantly improve the cycle effect and safety of lithium batteries. On this basis, this application further enhances the mechanical strength and chemical stability of the composite membrane by selecting the separation layer material, and can achieve long-term spatial confinement of lithium dendrites. The polymer phase distribution of the polyamide anthraquinone modified material is highly uniform, which accelerates the uniform migration of lithium ions in the membrane and improves the conductivity and cycle stability of the battery. In addition, this application can also improve the thermal stability of the separation layer by integrating phosphate functional groups into the separation layer material, broadening the application scenarios of batteries equipped with such composite membranes. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to clearly illustrate the embodiments, the following is a brief introduction to the accompanying drawings:

[0024] Figure 1 A schematic diagram of a composite membrane structure of the present application;

[0025] Figure 2 This is a schematic diagram of the structure of a lithium metal battery cell of the present application. DETAILED DESCRIPTION

[0026] The present application will be further described below by way of examples. Those of ordinary skill in the art will be able to implement the present application based on these descriptions. In addition, the examples of the present application involved in the following description are generally only examples of a part of the present application, rather than all of the examples. Therefore, all other examples obtained by those of ordinary skill in the art without creative work based on the examples in the present application should fall within the scope of protection of the present application.

[0027] In the following embodiments, the preparation method of the composite film comprises the following steps:

[0028] S1, dissolving the first monomer in a polar solvent, stirring and mixing to obtain an interfacial polymerization aqueous phase reaction prepolymer. The polar solvent is water or a mixture of water and ethanol (V 水 :V 乙醇 =2:3); in the interfacial polymerization aqueous phase reaction prepolymer, the volume concentration of the first monomer is 1~2% (g / mL).

[0029] S2. Dissolve the second monomer and the third monomer in a non-polar solvent, stir and mix to obtain an interfacial polymerization oil phase reaction prepolymer. The non-polar solvent is n-hexane, cyclohexane or n-heptane, etc.; in the interfacial polymerization oil phase reaction prepolymer, the volume concentration of the second monomer is 0.5-1% (g / mL), and the volume concentration of the third monomer is 0.04~0.3% (g / mL). In some embodiments, a fourth monomer is also involved. The fourth monomer is dissolved in a non-polar solvent simultaneously with the second monomer and the third monomer. In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of the fourth monomer is 0.008-0.05% (g / mL).

[0030] S3. The membrane layers except the separation layer are hot-pressed and composited, and the side with smaller pore size of the membrane layer is immersed in the interfacial polymerization water phase reaction prepolymer, and allowed to stand for 10 to 60 minutes. After being taken out and the surface reaction solution is scraped flat, it is immersed in the interfacial polymerization oil phase reaction prepolymer. After reacting for 2 to 10 minutes, it is taken out and placed in a vacuum oven for heat treatment. The heat treatment conditions are: temperature 80 to 100°C, time 30 to 60 minutes, and finally a composite membrane is obtained.

[0031] The method of using the composite film is to cold press the composite film on the surface of the lithium metal negative electrode. The cold pressing conditions are: pressure 0.5~2MPa, time 20~60s. In the subsequent lithium battery assembly process, the composite film is installed between the positive and negative electrodes. The rest of the process follows the conventional process of existing semi-solid lithium-ion batteries and will not be described in detail in this section.

[0032] Example 1

[0033] This embodiment discloses a composite membrane, which includes the following three membrane layers: a separation layer with a pore size of about 0.5-0.7 nm, a thickness of 60-70 nm, and a porosity of 20%; a buffer layer with a pore size of 0.2 μm, a thickness of 5 μm, and a porosity of 30%; and a support layer with a pore size of 0.4 μm, a thickness of 20 μm, and a porosity of 50%. The porosity of the composite membrane is about 38%.

[0034] In this embodiment, the separation layer uses a polyamide anthraquinone modified material, and the polyamide anthraquinone modified material is prepared from four monomers: piperazine, 1,3,5-trimethylbenzene carboxylic acid chloride, 9,10-anthraquinone-2-sulfonyl chloride and 2,2′-diaminobibenzyl diphosphate. Specifically, in the interfacial polymerization water phase reaction prepolymer, the volume concentration of piperazine is 1% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of 1,3,5-trimethylbenzene carboxylic acid chloride is 0.5% (g / mL), the volume concentration of 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.04% (g / mL), and the volume concentration of 2,2′-diaminobibenzyl diphosphate is 0.008% (g / mL). The buffer layer is a polyethylene film, and the support layer is a cellulose film. This embodiment also discloses a lithium metal battery, which contains the above-mentioned composite membrane.

[0035] Example 2

[0036] This embodiment discloses a composite membrane, which includes the following three membrane layers: a separation layer with a pore size of 0.6-0.9 nm, a thickness of 65-70 nm, and a porosity of 25%; a buffer layer with a pore size of 0.2 μm, a thickness of 10 μm, and a porosity of 35%; and a support layer with a pore size of 0.5 μm, a thickness of 30 μm, and a porosity of 55%. The porosity of the composite membrane is 50%.

[0037] In this embodiment, the separation layer uses a polyamide anthraquinone modified material, and the polyamide anthraquinone modified material is prepared from four monomers: m-phenylenediamine, 1,3,5-trimethylbenzene chloride, 9,10-anthraquinone-2-sulfonyl chloride and 2,2′-diaminobibenzyl diphosphate. Specifically, in the interfacial polymerization water phase reaction prepolymer, the volume concentration of m-phenylenediamine is 2% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of 1,3,5-trimethylbenzene chloride is 0.6% (g / mL), the volume concentration of 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.1% (g / mL), and the volume concentration of 2,2′-diaminobibenzyl diphosphate is 0.01% (g / mL). The buffer layer is a polyethylene film, and the support layer is a cellulose film. This embodiment also discloses a lithium metal battery, which contains the above-mentioned composite film.

[0038] Example 3

[0039] This embodiment discloses a composite membrane, which includes the following three membrane layers: a separation layer with a pore size of 0.7-0.9 nm, a thickness of 68-72 nm, and a porosity of 28%; a buffer layer with a pore size of 0.3 μm, a thickness of 12 μm, and a porosity of 40%; a support layer with a pore size of 0.6 μm, a thickness of 40 μm, and a porosity of 60%. The porosity of the composite membrane is 55%. In this embodiment, the separation layer uses a polyamide anthraquinone modified material, which is prepared from four monomers: piperazine, 1,3,5-benzene trimesoyl chloride, 9,10-anthraquinone-2-sulfonyl chloride, and 2,2′-diaminobibenzyl diphosphate. Specifically, in the interfacial polymerization aqueous phase reaction prepolymer, the piperazine volume concentration is 1% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of 1,3,5-benzene trimesoyl chloride is 0.9% (g / mL), the volume concentration of 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.25% (g / mL), and the volume concentration of 2,2′-diaminobibenzyl diphosphate is 0.04% (g / mL). The buffer layer is a polypropylene film, and the support layer is a cellulose film. This embodiment also discloses a lithium metal battery, which includes the above-mentioned composite film.

[0040] Example 4

[0041] This embodiment discloses a composite membrane, which includes the following two membrane layers: a separation layer with a pore size of 0.9-1 nm, a thickness of 70-75 nm, and a porosity of 33%; a cellulose support layer with a pore size of 0.6 μm, a thickness of 40 μm, and a porosity of 55%. The porosity of the composite membrane is 55%. In this embodiment, the separation layer uses a polyamide anthraquinone modified material, which is prepared from four monomers: piperazine, isophthaloyl chloride, anthraquinone-2,6-disulfonyl chloride, and 2,2′-diaminobibenzyl diphosphate. Specifically, in the interfacial polymerization water phase reaction prepolymer, the volume concentration of piperazine is 1% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of isophthaloyl chloride is 1% (g / mL), the volume concentration of anthraquinone-2,6-disulfonyl chloride monomer is 0.3% (g / mL), and the volume concentration of 2,2′-diaminobibenzyl diphosphate is 0.05% (g / mL). This embodiment also discloses a lithium metal battery, which includes the above-mentioned composite film.

[0042] Example 5

[0043] This embodiment discloses a composite membrane, which includes the following four membrane layers connected in sequence: a separation layer with a pore size of 0.9-1 nm, a thickness of 72-75 nm, and a porosity of 40%; a buffer layer with a pore size of 0.4 μm, a thickness of 20 μm, and a porosity of 50%; a permeation layer with a pore size of 0.6 μm, a thickness of 30 μm, and a porosity of 60%; a support layer with a pore size of 0.8 μm, a thickness of 50 μm, and a porosity of 70%. The porosity of the composite membrane is 63%. In this embodiment, the separation layer uses a polyamide anthraquinone modified material, which is prepared from four monomers of o-phenylenediamine, terephthaloyl chloride, 9,10-anthraquinone-2-sulfonyl chloride and 2,2′-diaminobibenzyl diphosphate. Specifically, in the interfacial polymerization aqueous phase reaction prepolymer, the volume concentration of o-phenylenediamine is 1.2% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of terephthaloyl chloride is 0.7% (g / mL), the volume concentration of 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.3% (g / mL), and the volume concentration of 2,2′-diaminobibenzyl diphosphate is 0.025% (g / mL). The buffer layer is a polyethylene material, the permeation layer is a polyvinylidene fluoride material; and the support layer is a non-woven fabric material. This embodiment also discloses a lithium metal battery, which includes the above-mentioned composite membrane.

[0044] Example 6

[0045] This embodiment discloses a composite membrane, which includes the following three membrane layers: a separation layer with a pore size of about 0.5-0.7nm, a thickness of 60-70nm, and a porosity of 20%; a buffer layer with a pore size of 0.2μm, a thickness of 5μm, and a porosity of 30%; a support layer with a pore size of 0.4μm, a thickness of 20μm, and a porosity of 50%. The porosity of the composite membrane is about 38%. In this embodiment, the separation layer uses a polyamide anthraquinone modified material, which is prepared from three monomers: piperazine, 1,3,5-benzene trimesoyl chloride, and 9,10-anthraquinone-2-sulfonyl chloride. Specifically, in the interfacial polymerization aqueous phase reaction prepolymer, the piperazine volume concentration is 1% (g / mL). In the interfacial polymerization oil phase reaction prepolymer, the volume concentration of 1,3,5-benzene trimesoyl chloride is 0.5% (g / mL), and the volume concentration of 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.04% (g / mL). The buffer layer is a polyethylene film, and the support layer is a cellulose film. This embodiment also discloses a lithium metal battery, which includes the above-mentioned composite film.

[0046] Comparative Example 1

[0047] The difference between the lithium metal battery in this comparative example and Example 1 is that a common diaphragm material is used instead of the composite membrane.

[0048] Comparative Example 2

[0049] The lithium metal battery of this comparative example differs from Example 1 in that it does not include a separation layer.

[0050] Performance Testing

[0051] The cycle performance and safety performance of the lithium metal batteries disclosed in Examples 1 to 6 and Comparative Examples 1 to 2 were tested. The specific test method refers to Section 6.4 of GB31484-2015, where the charge and discharge currents are based on the conditions specified by the enterprise. The calculation and integration are as follows:

[0052] Table 1. Performance test results

[0053] Group 100 cycles capacity retention Hot box test Overcharge test Example 1 83.8% pass pass Example 2 86.3% pass pass Example 3 87.2% pass pass Example 4 80.5% pass pass Example 5 93.1% pass pass Example 6 82.0% pass pass Comparative Example 1 5 cycles to failure Not passed Not passed Comparative Example 2 31 cycles to failure Not passed pass

[0054] By observing the above table, it can be seen that the present application greatly improves the cycle performance and safety factor of lithium metal batteries by providing a separation layer containing anthraquinone functional groups and by means of the synergistic effect between the separation layer and other film layers. Specifically, after 100 charge and discharge cycles, the capacity retention rate of the lithium metal battery of the present application remains above 80%, reflecting the durability of the battery after long-term use. In addition, all lithium metal batteries in the embodiments of the present application have passed the hot box test and overcharge test, demonstrating the excellent operating stability and safety of lithium metal batteries under extreme conditions.

Claims

1. A composite film, characterized in that The composite membrane comprises at least two membrane layers; the membrane layers are provided with pores and ion channels for lithium ions to pass through are formed between the pores of each membrane layer; the pore sizes of each membrane layer are arranged to decrease in a unidirectional manner along the thickness direction of the composite membrane; the membrane layer at the end of the composite membrane with a smaller pore size is a separation layer, the separation layer is used to contact the surface of the lithium metal negative electrode, and the separation layer material is a polyamide anthraquinone modified material; The polyamide anthraquinone modified material is obtained by polymerizing a material comprising a first monomer, a second monomer, a third monomer and a fourth monomer; wherein: the first monomer is selected from piperazine and / or a diamine, and the diamine includes at least one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, xylylenediamine, ethylenediamine, propylenediamine, 1,3-diaminocyclohexane and 1,2-diaminocyclohexane; the second monomer is selected from acyl chlorides, and the acyl chlorides include at least one of isophthaloyl chloride, terephthaloyl chloride and 1,3,5-trimethylbenzene chloride; the third monomer includes anthraquinone-2,6-disulfonyl chloride and 9,10-anthraquinone- At least one of 2-sulfonyl chloride; the fourth monomer is selected from amino phosphates, and the amino phosphates include 2,2'-diaminobibenzyl diphosphate; the membrane layer also includes a buffer layer and a support layer sequentially arranged on one side of the separation layer; the pore size of the separation layer is 0.5~1nm; the pore size of the buffer layer is 0.2~0.4μm; the pore size of the support layer is 0.4~0.8μm.

2. A composite membrane according to claim 1, characterized in that: The thickness of the separation layer is 60-75 nm, the thickness of the buffer layer is 5-20 μm; and the thickness of the support layer is 20-50 μm.

3. A composite membrane according to claim 1, characterized in that: The porosity of the composite membrane is 38-63%, wherein the porosity of the separation layer is 20-40%, the porosity of the buffer layer is 30-50%, and the porosity of the support layer is 50-70%.

4. Use of the composite membrane according to any one of claims 1 to 3 in a lithium metal battery.

5. A lithium metal battery, characterized in that: A composite film according to any one of claims 1 to 3 is arranged between the positive and negative electrodes of the lithium metal battery.