A method for preparing silicon nitride ceramic material
Fourier transform infrared spectroscopy technology is used to monitor the mixing process of ceramic slurry in real time and control the stirring time, which solves the problem of difficulty in accurately controlling the stirring time of ceramic slurry in the preparation of silicon nitride ceramic materials, and improves the mixing uniformity and mixing accuracy. Reduced production costs.
Patent Information
- Application Number
- CN202410910646.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
In the existing silicon nitride ceramic material preparation method, the stirring time of the ceramic slurry is difficult to accurately control, which may lead to uneven mixing or damage to the powder particles, and increase production costs.
Fourier transform infrared spectroscopy technology is used to monitor the mixing process of ceramic slurry in real time. By analyzing the second-order spectral absorption peak wave number ratio coefficient and mixing coefficient, the stirring time is controlled in real time to ensure uniform mixing of ceramic slurry.
It improves the mixing uniformity and stirring accuracy of ceramic slurry, reduces production costs and equipment wear, and ensures the quality of silicon nitride ceramic materials.
Smart Images

Figure CN118495965B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of silicon nitride ceramic material preparation, and in particular to a method for preparing a silicon nitride ceramic material. Background Art
[0002] Silicon nitride ceramics are a covalent bond compound composed of silicon and nitrogen. They have excellent physical, chemical and mechanical properties such as high strength, high hardness, low density, high temperature resistance and corrosion resistance. Due to these properties, silicon nitride ceramic materials have been widely used in aerospace engines, mechanical industry and electronic packaging fields.
[0003] Ceramic slurry is the core of silicon nitride ceramic material preparation. It is usually necessary to stir the ceramic slurry for a long time to make it mix evenly in order to obtain a fine and uniform ceramic slurry. However, the stirring time of ceramic slurry is often difficult to control accurately. Insufficient stirring time may lead to uneven mixing of the slurry, while too long stirring time may cause the powder particles in the slurry to be damaged or broken due to long-term high shear force stirring, which will also increase equipment wear and increase production costs.
[0004] An invention with patent application number CN107941747A discloses a device and method for detecting the uniformity of a mixture based on MEMS near-infrared technology. The method has the following steps: Step 1: Use a MEMS-based near-infrared spectrometer to detect the mixture in a mixing tank in real time through a window structure, and continuously collect spectra to obtain spectral variables, thereby obtaining multiple absorbances A; Step 2: Calculate and analyze the absorbance A; Step 3: Draw a trend graph based on the analysis results obtained in step 2; Step 4: Analyze the trend graph, and if the curve of the trend graph is lower than the uniformity limit (MBSD value = 0.000035), it is judged that the material has reached a uniform state. Although the method described in the patent document utilizes an advanced near-infrared spectrometer to detect the mixing degree of the mixture in real time to a certain extent, due to the phenomenon of overlapping absorption peaks in the infrared spectrum data between different raw materials during the mixing process of the materials, there is an error in judging the uniform state of the material mixing using infrared spectrum data. Summary of the invention
[0005] In order to solve the above technical problems, the present application provides a method for preparing a silicon nitride ceramic material to solve the existing problems.
[0006] A method for preparing silicon nitride ceramic material in the present application adopts the following technical solution:
[0007] An embodiment of the present application provides a method for preparing a silicon nitride ceramic material, the method comprising the following steps:
[0008] S1: Weigh silicon nitride powder, pore-forming agent, and surfactant according to mass, mix, wet-grind, stir, and dry to obtain raw material powder;
[0009] S2: obtaining a mixture of monomers, a cross-linking agent, deionized water and ethanol, mixing and stirring the raw material powder, the mixture, an initiator and a catalyst according to parts by mass, collecting Fourier transform infrared spectral data of the same position of the slurry at each moment during the mixing and stirring process, and collecting Fourier transform infrared spectral data of various raw materials;
[0010] Analyze the differences in the wavenumbers corresponding to the peak points and the trough points in the second-order derivative spectra of the Fourier transform infrared spectral data of the slurry and various raw materials at each moment, and obtain the wavenumber ratio coefficient of the second-order spectral absorption peak of the slurry in various raw materials at each moment;
[0011] All raw materials are screened by the second-order spectral absorption peak wave number ratio coefficient, and the difference between the quantity of the remaining raw materials after screening and the quantity of all raw materials is analyzed to obtain the ceramic slurry mixing coefficient at each moment;
[0012] Combined with the ceramic slurry mixing coefficient, the overall mixing degree of the ceramic slurry at each moment is analyzed to control the stirring time of the slurry;
[0013] After the stirring is completed, the ceramic slurry is subjected to vacuum defoaming treatment to obtain a ceramic slurry;
[0014] S3: injecting the ceramic slurry into the mold, leaving it to solidify naturally at room temperature, and then taking it out for drying to obtain a green embryo;
[0015] S4: heating and sintering the green body to form pores inside to obtain a silicon nitride ceramic material;
[0016] The process of determining the second-order spectral absorption peak wave number ratio coefficient is as follows:
[0017] The wavenumbers corresponding to all the peak points and all the trough points in the second-order derivative spectrum of the Fourier transform infrared spectrum data of the slurry at each moment are used to form the FT-IR second-order spectrum absorption peak wavenumber set of the slurry at each moment, and the FT-IR second-order spectrum absorption peak wavenumber set of various raw materials is obtained by the same method, and the intersection of the FT-IR second-order spectrum absorption peak wavenumber sets of all raw materials is used as the common absorption peak wavenumber set of raw materials;
[0018] The wavenumbers in the common absorption peak wavenumber set of the raw materials are removed from the FT-IR second-order spectrum absorption peak wavenumber set of various raw materials to obtain the unique absorption peak wavenumber set of various raw materials, and the number of overlapping wavenumbers in the FT-IR second-order spectrum absorption peak wavenumber set of the slurry at each moment is counted, and the ratio of the number of overlapping wavenumbers to the number of wavenumbers in the unique absorption peak wavenumber set is used as the second-order spectrum absorption peak wavenumber ratio coefficient of the slurry in various raw materials at each moment;
[0019] The determination process of the ceramic slurry mixing coefficient is:
[0020] At each moment, all the wavenumbers in the unique absorption peak wavenumber set of the raw material corresponding to the maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient are eliminated from the FT-IR second-order spectrum absorption peak wavenumber set of the slurry, and the raw material corresponding to the maximum value is eliminated at the same time, and the second-order spectrum absorption peak wavenumber ratio coefficient of the FT-IR second-order spectrum absorption peak wavenumber set of the slurry after elimination and the unique absorption peak wavenumber set of various raw materials remaining after elimination are calculated, and all the wavenumbers in the unique absorption peak wavenumber set of the raw material corresponding to the maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient are continued to be eliminated from the FT-IR second-order spectrum absorption peak wavenumber set of the slurry by the same method, and the second-order spectrum absorption peak wavenumber ratio coefficient is repeatedly calculated, and when the calculated maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient is less than a preset threshold, the calculation is stopped;
[0021] Calculate the ratio of the number of remaining raw materials to the total number of raw materials, and obtain the ceramic slurry mixing coefficient at each moment by inverse proportional mapping, wherein the preset threshold is the minimum value of the second-order spectral absorption peak wave number ratio coefficient of the ceramic slurry whose mixing degree meets the production standard among all kinds of raw materials;
[0022] The control of the stirring time of the slurry includes:
[0023] Calculate the coefficient of variation of the ceramic slurry mixing coefficient in the local time period at each moment, and map the coefficient of variation in inverse proportion as the ceramic slurry stirring completion degree at each moment. When the ceramic slurry stirring completion degree is greater than or equal to the ceramic slurry mixing completion threshold, stop stirring. The ceramic slurry mixing completion threshold is the average of the ceramic slurry stirring completion degrees of multiple ceramic slurries whose mixing degrees meet the production standards at the last moment in the stirring process.
[0024] In the above scheme, the second-order spectral absorption peak wavenumber ratio coefficient of the slurry in various raw materials at each moment is constructed by analyzing the distribution of data in the FT-IR spectrum of the ceramic slurry and the FT-IR spectrum of the raw materials of the ceramic slurry. The beneficial effect is that it reduces the absorption peak overlap phenomenon that may appear in the FT-IR spectrum of the ceramic slurry, and the influence that the raw materials of the ceramic slurry may have the same absorption peak characteristics in the FT-IR spectrum of the ceramic slurry, and improves the degree of distinction between the FT-IR spectral characteristics of different raw materials in the ceramic slurry in the FT-IR spectrum of the ceramic slurry. The ceramic slurry mixing coefficient is constructed by analyzing the data distribution in the FT-IR second-order spectral absorption peak wavenumber set and combining the second-order spectral absorption peak wavenumber ratio coefficient. The beneficial effect is that by identifying the distribution of each component in the ceramic slurry, the actual mixing of the raw materials of the ceramic slurry can be monitored in real time without affecting the stirring process of the ceramic slurry, which improves the speed and accuracy of evaluating the mixing degree of the ceramic slurry during the stirring process. By combining the ceramic slurry mixing coefficient, analyzing the overall mixing degree of the ceramic slurry at each moment, and controlling the stirring time of the ceramic slurry, the production cost and the wear on the stirring equipment are reduced while ensuring the quality of the prepared ceramic slurry.
[0025] In one embodiment, the silicon nitride powder is 85-105 parts by weight, the pore former is aluminum hydroxide, which is 11-16 parts by weight, and the surfactant is sodium dodecylbenzene sulfonate, which is 2.0-2.5 parts by weight.
[0026] In one embodiment, the wet grinding condition is to ensure that the powder with a particle size of 4-20 μm accounts for more than 95%.
[0027] In the above scheme, the purpose of wet grinding is to fully mix the particles of different components and reduce the particle size of the particles by mechanical action. The wet-milled mixture is stirred to ensure that all components are evenly distributed throughout the mixture.
[0028] In one embodiment, the raw material powder is 90-110 parts, the monomer is 6-12 parts, the cross-linking agent is 4-5 parts, the initiator is 0.3-0.8 parts, the catalyst is 0.6-1 parts, the deionized water is 30-50 parts, and the ethanol is 30-40 parts.
[0029] In one embodiment, the monomer is acrylamide, the cross-linking agent is hydroxyethyl acrylate, the initiator is ammonium sulfate, and the catalyst is hydroxymethyl acrylamide.
[0030] In the above scheme, the cross-linking agent is added to improve the cross-linking density and mechanical strength of the final product, and the initiator is added to initiate the polymerization reaction of the monomers in the slurry.
[0031] In one embodiment, the natural curing time is 1 to 5 hours.
[0032] In one embodiment, the green embryo heating and sintering comprises:
[0033] First, heat the temperature to 300~600℃ at a heating rate of 1~2℃ / min and keep it warm for 1~3 hours. Then, in a nitrogen atmosphere, continue heating at a heating rate of 1~2℃ / min to 800~1000℃ and keep it warm for 1~2 hours. Finally, continue heating at a heating rate of 5~8℃ / min under a pressure of 0.3~0.5MPa to 1300~1800℃ and keep it warm for 1~6 hours.
[0034] In the above scheme, the first stage is kept warm for 1 to 3 hours, which helps to form pores inside the material. The second stage is kept warm for 1 to 2 hours, which helps to further promote the physical changes of the material and prepare for subsequent high-temperature sintering. The third stage is kept warm for 1 to 6 hours, which helps to complete the densification process of the material while maintaining a certain porosity.
[0035] This application has at least the following beneficial effects:
[0036] The present application constructs the second-order spectral absorption peak wavenumber proportion coefficient of the slurry in various raw materials at each moment by analyzing the distribution of data in the FT-IR spectrum of ceramic slurry and the FT-IR spectrum of the raw materials of ceramic slurry. The beneficial effect is that it reduces the absorption peak overlap that may appear in the FT-IR spectrum of ceramic slurry, and the influence of the raw materials of ceramic slurry that may have the same absorption peak characteristics in the FT-IR spectrum of ceramic slurry, and improves the degree of distinction of FT-IR spectral characteristics of different raw materials in ceramic slurry in the FT-IR spectrum of ceramic slurry.
[0037] The ceramic slurry mixing coefficient is constructed by analyzing the data distribution in the FT-IR second-order spectrum absorption peak wavenumber set and combining the second-order spectrum absorption peak wavenumber proportion coefficient. The beneficial effect is that by identifying the distribution of each component in the ceramic slurry, the actual mixing situation of the raw materials of the ceramic slurry can be monitored in real time without affecting the ceramic slurry stirring process, thereby improving the speed and accuracy of evaluating the mixing degree of the ceramic slurry during the stirring process.
[0038] The ceramic slurry stirring completion degree is constructed based on the distribution of the ceramic slurry mixing coefficient over time. The beneficial effect is that it realizes the control of the stirring time of the ceramic slurry during the preparation process of silicon nitride ceramic material, while ensuring the quality of the prepared ceramic slurry, reducing the production cost and the wear on the stirring equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0040] Figure 1 A flow chart of the steps of a method for preparing a silicon nitride ceramic material provided in this application;
[0041] Figure 2 This is a flow chart for controlling the stirring time of ceramic slurry;
[0042] Figure 3 Schematic diagram of FT-IR spectrum with overlapping peaks;
[0043] Figure 4 It is a schematic diagram of the second derivative spectrum of FT-IR spectrum;
[0044] Figure 5 For Figure 3 Schematic diagram of FT-IR spectra with similar absorption peaks;
[0045] Figure 6 for Figure 5 Schematic diagram of the second derivative spectrum of ;
[0046] Figure 7 for Figure 4 Schematic diagram of the unique absorption peaks;
[0047] Figure 8 for Figure 6 Schematic diagram of the unique absorption peak. DETAILED DESCRIPTION
[0048] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of a method for preparing a silicon nitride ceramic material proposed in the present application, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.
[0049] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.
[0050] The specific scheme of the method for preparing a silicon nitride ceramic material provided by the present application is described in detail below with reference to the accompanying drawings.
[0051] An embodiment of the present application provides a method for preparing a silicon nitride ceramic material. Specifically, the following method for preparing a silicon nitride ceramic material is provided. Figure 1 , the method comprises the following steps:
[0052] S1: Preparation of raw powder
[0053] Weigh silicon nitride powder, pore-forming agent, and surfactant by mass to obtain a mixture, add an appropriate solvent for wet grinding, the appropriate solvent can be water or alcohol, then stir and dry, use a particle size analyzer to check the particle size distribution of the powder in the dried mixture, ensure that the powder with a particle size of 4~20μm accounts for more than 95%, and set aside the mixture after drying and checking the particle size as raw material powder. Among them, aluminum hydroxide is selected as a pore-forming agent in this application, and sodium dodecylbenzene sulfonate is selected as a surfactant. The particle size analyzer used in this application is a laser particle size analyzer. The implementer can choose other particle size analyzers according to actual conditions, and this application is not limited here.
[0054] In Example 1 of the present application, 85 parts of silicon nitride powder, 11 parts of a pore former, and 2.0 parts of a surfactant were weighed, mixed, and then water was added for wet grinding, followed by stirring and drying to obtain a raw material powder.
[0055] In Example 2 of the present application, 95 parts of silicon nitride powder, 14 parts of pore-forming agent, and 2.3 parts of surfactant were weighed, mixed, and then added with alcohol for wet grinding, and then stirred and dried to obtain raw material powder.
[0056] In Example 3 of the present application, 105 parts of silicon nitride powder, 16 parts of a pore former, and 2.5 parts of a surfactant were weighed, mixed, and then water was added for wet grinding, followed by stirring and drying to obtain a raw material powder.
[0057] S2: Preparation of ceramic slurry
[0058] A mixture of monomers, a cross-linking agent, deionized water and ethanol is obtained, and the mixture, the raw material powder in step S1, and the initiator and the catalyst are mixed and stirred according to mass parts until a uniformly mixed slurry is formed, and the slurry is subjected to vacuum defoaming treatment to obtain a ceramic slurry. In this application, acrylamide is selected as the monomer, hydroxyethyl acrylate is selected as the cross-linking agent, ammonium sulfate is selected as the initiator, and hydroxymethyl acrylamide is selected as the catalyst.
[0059] In Example 1 of the present application, the raw material powder is 90 parts, the monomer is 6 parts, the cross-linking agent is 4 parts, the initiator is 0.3 parts, the catalyst is 0.6 parts, the deionized water is 30 parts, and the ethanol is 30 parts.
[0060] In Example 2 of the present application, the raw material powder is 100 parts, the monomer is 9 parts, the cross-linking agent is 4.5 parts, the initiator is 0.5 parts, the catalyst is 0.8 parts, the deionized water is 40 parts, and the ethanol is 35 parts.
[0061] In Example 3 of the present application, the raw material powder is 110 parts, the monomer is 12 parts, the cross-linking agent is 5 parts, the initiator is 0.8 parts, the catalyst is 1 part, the deionized water is 50 parts, and the ethanol is 40 parts.
[0062] Adjust the mixing and stirring time of the ceramic slurry preparation in step S2. The ceramic slurry stirring time control flow chart is as follows: Figure 2 As shown, the specific steps are:
[0063] Step S001, collecting Fourier transform infrared spectral data of the slurry at each moment during the stirring process, and collecting Fourier transform infrared spectral data of various raw materials in step S2.
[0064] In the mixing and stirring process of the ceramic slurry preparation in step S2, a Fourier transform infrared spectrometer connected to an immersed optical fiber probe is used to collect the FT-IR (Fourier transform infrared) spectrum of the ceramic slurry at a fixed position in the mixer every T minutes, and the fixed position is recorded as the sampling position of the FT-IR spectrum data. In one embodiment of the present application, T=5, and the sampling time interval and sampling position of the FT-IR spectrum can be set by the implementer according to the actual situation, and the present application does not limit it here. In addition, the FT-IR spectrum data of each raw material of the ceramic slurry is collected. It should be noted that the raw materials here include silicon nitride powder, pore former, surfactant, monomer, cross-linking agent, deionized water, ethanol, initiator and catalyst.
[0065] All the obtained FT-IR spectra were subjected to baseline correction and spectrum smoothing processing to eliminate the baseline drift phenomenon that may occur in the collected spectra and reduce the interference of noise. The baseline correction and spectrum smoothing processing are existing well-known technologies and will not be described in detail in this application.
[0066] Step S002, analyzing the differences in wavenumbers corresponding to peak points and trough points in the second-order derivative spectra of the Fourier transform infrared spectral data of the slurry and various raw materials at each moment, and obtaining the second-order spectral absorption peak wavenumber ratio coefficient of the slurry in various raw materials at each moment.
[0067] First FT-IR spectrum of ceramic slurry at sampling time For example, since ceramic slurry is a multi-component mixture, this may cause the absorption peaks to overlap in the FT-IR spectrum of the ceramic slurry. The schematic diagram of the FT-IR spectrum with overlapping peaks is shown in Figure 3 As shown, the spectrum is obtained The second derivative spectrum of , in order to improve the spectrum of different components in the ceramic slurry The degree of distinction between the corresponding absorption peaks in the spectrum, wherein the acquisition of the second-order derivative spectrum is a known technique, and the specific process is not described in detail in this application. The schematic diagram of the second-order derivative spectrum of the FT-IR spectrum is as follows Figure 4 As shown. Among them, Figure 3 The horizontal axis is the wave number, and the vertical axis is the reflectivity. Figure 4 The horizontal axis is the wave number and the vertical axis is the second-order derivative.
[0068] Secondly, since the absorption peaks of each component in the ceramic slurry in the FT-IR spectrum, such as the peak intensity, peak width, and peak shape of the absorption peak, will be affected by the concentration of each component in the ceramic slurry and the degree of overlap of the absorption peaks of each component, the spectrum As the input of the peak and valley second-order difference identification algorithm, the output spectrum All the peak points and trough points are identified, wherein the peak and trough second-order difference identification algorithm is a well-known technology, and the specific process is not repeated here. All the peak points and trough points obtained are The set of corresponding wave numbers in is recorded as spectrum FT-IR second-order spectrum absorption peak wave number set , to characterize the spectrum The second derivative spectrum of all components in the ceramic slurry at the sampling position The position distribution of all corresponding absorption peaks in order to improve the different raw materials of ceramic slurry in the spectrum The identification accuracy of the absorption peak in Figure 3 The schematic diagram of FT-IR spectrum with similar absorption peak performance is shown in Figure 5. Figure 5 The schematic diagram of the second derivative spectrum is as follows Figure 6 shown. Figure 5 The horizontal axis is the wave number, and the vertical axis is the reflectivity. Figure 6 The horizontal axis is the wave number and the vertical axis is the second-order derivative.
[0069] The same calculation method as the FT-IR second-order spectrum absorption peak wavenumber set of the ceramic slurry at each moment is used to obtain the FT-IR second-order spectrum absorption peak wavenumber set of various raw materials. The intersection of the FT-IR second-order spectrum absorption peak wavenumber set of all raw materials is used as the common absorption peak wavenumber set of raw materials to characterize the position distribution of all the same absorption peaks of all raw materials of the ceramic slurry in the FT-IR second-order spectrum of the FT-IR spectrum, so as to improve the degree of distinction between the FT-IR spectrum characteristics of different raw materials of the ceramic slurry.
[0070] At any moment, taking the raw material monomer, i.e. acrylamide, as an example, the FT-IR second-order spectrum absorption peak wavenumber set of the raw material acrylamide is taken as the unique absorption peak wavenumber set of the raw material acrylamide after removing all the wavenumbers in the common absorption peak wavenumber set of the raw materials. The number of wavenumbers that overlap between the unique absorption peak wavenumber set of the raw material acrylamide and the FT-IR second-order spectrum absorption peak wavenumber set of the ceramic slurry at the corresponding moment is counted, and the ratio of the number of overlapping wavenumbers to the number of wavenumbers in the unique absorption peak wavenumber set of the raw material acrylamide is taken as the second-order spectrum absorption peak wavenumber ratio coefficient of the ceramic slurry in the raw material acrylamide at the corresponding moment. Using the same method, the unique absorption peak wavenumber set of various raw materials (silicon nitride powder, pore former, surfactant, monomer, cross-linking agent, deionized water, ethanol, initiator and catalyst) at each moment and the second-order spectrum absorption peak wavenumber ratio coefficient of the slurry in various raw materials at each moment can be obtained. Characterize the spectrum The greater the proportion of all absorption peaks in the second-order derivative spectra of various raw material spectra, the greater the possibility that the corresponding raw materials exist in the components of the ceramic slurry at the sampling position. Figure 4 The schematic diagram of the unique absorption peak is as follows Figure 7 As shown, Figure 6 The schematic diagram of the unique absorption peak is as follows Figure 8 shown. Figure 7 , Figure 8 The horizontal axis is the wave number and the vertical axis is the second-order derivative.
[0071] Step S003, screening all raw materials by the second-order spectral absorption peak wave number ratio coefficient, analyzing the difference between the quantity of remaining raw materials after screening and the quantity of all raw materials, and obtaining the ceramic slurry mixing coefficient at each moment.
[0072] For each moment, after obtaining the second-order spectral absorption peak wavenumber ratio coefficient of the ceramic slurry in various raw materials, the unique absorption peak wavenumber set of the raw material corresponding to the maximum value of the second-order spectral absorption peak wavenumber ratio coefficient is obtained. For each wavenumber in the unique absorption peak wavenumber set, if it exists in the FT-IR second-order spectral absorption peak wavenumber set of the slurry at the corresponding moment, the wavenumber is removed from the FT-IR second-order spectral absorption peak wavenumber set of the slurry at the corresponding moment. At the same time, the raw material corresponding to the maximum value of the second-order spectral absorption peak wavenumber ratio coefficient is removed from all raw materials, and then the FT-IR second-order spectral absorption of the slurry after removal is calculated. The second-order spectrum absorption peak wave number ratio coefficient of the peak wave number set and the unique absorption peak wave number set of various raw materials remaining after elimination is collected. The same method is used to remove all wave numbers in the unique absorption peak wave number set of the raw material corresponding to the maximum value of the second-order spectrum absorption peak wave number ratio coefficient from the FT-IR second-order spectrum absorption peak wave number set of the slurry, and the second-order spectrum absorption peak wave number ratio coefficient is repeatedly calculated until all raw materials are eliminated, or the maximum value of the calculated second-order spectrum absorption peak wave number ratio coefficient is less than the second-order spectrum absorption peak wave number ratio coefficient threshold, and the number of remaining raw materials after the raw materials are finally eliminated is counted. The threshold value of the second-order spectrum absorption peak wave number ratio coefficient is recorded as the preset threshold value.
[0073] The method for obtaining the threshold value of the second-order spectral absorption peak wavenumber proportion coefficient is as follows: the same method as that for obtaining the FT-IR second-order spectral absorption peak wavenumber set of the above-mentioned slurry is used to obtain the FT-IR second-order spectral absorption peak wavenumber set of the ceramic slurry whose mixing degree meets the production standards, and the second-order spectral absorption peak wavenumber proportion coefficient of the ceramic slurry whose mixing degree meets the production standards in various raw materials is calculated, and the minimum value of all the second-order spectral absorption peak wavenumber proportion coefficients obtained is used as the threshold value of the second-order spectral absorption peak wavenumber proportion coefficient.
[0074] After the above conditions are met, the ratio of the number of the remaining raw materials to the total number of raw materials is calculated, and the ceramic slurry mixing coefficient at each moment is obtained by inverse proportional mapping.
[0075] It should be noted that the inverse proportional mapping indicates that there is a negative correlation between variables. The dependent variable will decrease as the independent variable increases, and the dependent variable will increase as the independent variable decreases. Specifically, it can be a subtraction relationship, a division relationship, etc.
[0076] As an embodiment of the present application, the ratio of the number of the remaining raw materials to the total number of raw materials is calculated, and the difference between 1 and the ratio is determined as the ceramic slurry mixing coefficient at the corresponding moment.
[0077] At each moment, the greater the proportion of raw material types present in the ceramic slurry at the sampling position, the greater the ceramic slurry mixing coefficient, the more comprehensive the distribution of raw material types in the ceramic slurry at the sampling position, and the better the ceramic slurry is mixed at the sampling position.
[0078] Step S004, combining the ceramic slurry mixing coefficient, analyzing the overall mixing degree of the ceramic slurry at each moment, and completing the control of the slurry stirring time.
[0079] First As an example, in one embodiment of the present application, the first To The ceramic slurry mixing coefficient at each time during the time period, where , in this application =5, implementers can set it according to actual conditions, this application does not limit it, and will start from Time to The time elapsed is taken as the The local time period at time . Calculate the To The coefficient of variation of all ceramic slurry mixing coefficients during the time period is inversely mapped to determine the ceramic slurry stirring completion degree at each time. To During the time period, the closer the values of the ceramic slurry mixing coefficients at each time are, and the larger the value of the ceramic slurry mixing coefficient is, the greater the value of the ceramic slurry mixing coefficient is. At a certain moment, the better the overall mixing degree of the ceramic slurry is, the more it is necessary to stop stirring at this time, and the greater the value of the ceramic slurry stirring completion degree is.
[0080] As an embodiment of the present application, the sum of the coefficient of variation and the preset adjustment factor at each moment is calculated, and the reciprocal of the sum is used as the degree of completion of the ceramic slurry stirring at each moment, wherein the preset adjustment factor is set to prevent the denominator from being 0, resulting in an inability to calculate. In the present application, the adjustment factor is artificially set to 0.01, and the implementer can set it according to the actual situation, and the present application does not impose any restrictions on this.
[0081] The same calculation method as the above-mentioned ceramic slurry stirring completion degree is used to obtain the ceramic slurry stirring completion degree of m ceramic slurries whose mixing degree meets the production standard at the last moment of the stirring process, and the average of the obtained m ceramic slurry stirring completion degrees is used as the ceramic slurry mixing completion threshold. When the ceramic slurry stirring completion degree of the ceramic slurry is greater than or equal to the ceramic slurry mixing completion threshold, it means that the mixing degree of the ceramic slurry meets the production standard at the corresponding moment, and the stirring of the ceramic slurry can be stopped. In this application, m=3, and the implementer can set it according to the actual situation, and this application does not limit it.
[0082] S3: Preparation of raw embryos
[0083] In Example 1 of the present application, a ceramic slurry is injected into a mold, and the introduction of bubbles should be avoided during injection, and it is ensured that the slurry evenly fills every corner of the mold; the mold after injection is placed at room temperature for natural curing, and the curing time is 1 hour; the formed green embryo is taken out from the cured mold, and is dried to remove residual moisture inside the green embryo, and the dried green embryo is set aside to obtain a green embryo.
[0084] In Example 2 of the present application, the ceramic slurry is injected into the mold, and the introduction of bubbles should be avoided during the injection, and it is ensured that the slurry evenly fills every corner of the mold; the mold after injection is placed at room temperature for natural curing, and the curing time is 3 hours; the molded green embryo is taken out from the cured mold, and is dried to remove residual moisture inside the green embryo, and the dried green embryo is set aside to obtain a green embryo.
[0085] In Example 3 of the present application, the ceramic slurry is injected into the mold, and the introduction of bubbles should be avoided during the injection, and it is ensured that the slurry evenly fills every corner of the mold; the mold after injection is placed at room temperature for natural curing, and the curing time is 5 hours; the formed green embryo is taken out from the cured mold, and is dried to remove residual moisture inside the green embryo, and the dried green embryo is set aside to obtain a green embryo.
[0086] S4: Preparation of silicon nitride ceramic materials
[0087] In Example 1 of the present application, the green embryo is placed in a sintering furnace and gradually heated at a heating rate of 1°C / minute. When the temperature rises to 300°C, it is kept warm for 1 hour. After the insulation is completed, heating is continued at a heating rate of 1°C / minute in a nitrogen atmosphere. When the temperature rises to 800°C, it is kept warm for 1 hour. After the insulation is completed, heating is continued at a heating rate of 5°C / minute under a pressure of 0.3MPa. When the temperature reaches 1300°C, it is kept warm for 1 hour. After the insulation is completed, the temperature in the sintering furnace is cooled to room temperature and the sintered silicon nitride ceramic material is taken out.
[0088] In Example 2 of the present application, the green embryo is placed in a sintering furnace and gradually heated at a heating rate of 1.5°C / minute. When the temperature rises to 450°C, it is kept warm for 2 hours. After the insulation is completed, heating is continued at a heating rate of 1.5°C / minute in a nitrogen atmosphere. When the temperature rises to 900°C, it is kept warm for 1.5 hours. After the insulation is completed, heating is continued at a heating rate of 6.5°C / minute under a pressure of 0.4MPa. When the temperature reaches 1500°C, it is kept warm for 4 hours. After the insulation is completed, the temperature in the sintering furnace is cooled to room temperature and the sintered silicon nitride ceramic material is taken out.
[0089] In Example 3 of the present application, the green embryo is placed in a sintering furnace and gradually heated at a heating rate of 2°C / minute. When the temperature rises to 600°C, it is kept warm for 3 hours. After the insulation is completed, heating is continued at a heating rate of 2°C / minute in a nitrogen atmosphere. When the temperature rises to 1000°C, it is kept warm for 2 hours. After the insulation is completed, heating is continued at a heating rate of 8°C / minute under a pressure of 0.5MPa. When the temperature reaches 1800°C, it is kept warm for 6 hours. After the insulation is completed, the temperature in the sintering furnace is cooled to room temperature and the sintered silicon nitride ceramic material is taken out.
[0090] It should be noted that the above sequence of the embodiments of the present application is for description only and does not represent the advantages and disadvantages of the embodiments. The above is a description of a specific embodiment of this specification. In addition, the processes depicted in the accompanying drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.
[0091] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0092] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Modifications to the technical solutions recorded in the aforementioned embodiments, or equivalent replacement of some of the technical features therein, do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for preparing a silicon nitride ceramic material, characterized in that: The method comprises the following steps: S1: Weigh silicon nitride powder, pore-forming agent, and surfactant according to mass, mix, wet-grind, stir, and dry to obtain raw material powder; S2: obtaining a mixture of monomers, a cross-linking agent, deionized water and ethanol, mixing and stirring the raw material powder, the mixture, an initiator and a catalyst according to parts by mass, collecting Fourier transform infrared spectral data of the same position of the slurry at each moment during the mixing and stirring process, and collecting Fourier transform infrared spectral data of various raw materials; Analyze the differences in the wavenumbers corresponding to the peak points and the trough points in the second-order derivative spectra of the Fourier transform infrared spectral data of the slurry and various raw materials at each moment, and obtain the wavenumber ratio coefficient of the second-order spectral absorption peak of the slurry in various raw materials at each moment; All raw materials are screened by the second-order spectral absorption peak wave number ratio coefficient, and the difference between the quantity of the remaining raw materials after screening and the quantity of all raw materials is analyzed to obtain the ceramic slurry mixing coefficient at each moment; Combined with the ceramic slurry mixing coefficient, the overall mixing degree of the ceramic slurry at each moment is analyzed to control the stirring time of the slurry; After the stirring is completed, the ceramic slurry is subjected to vacuum defoaming treatment to obtain a ceramic slurry; S3: injecting the ceramic slurry into the mold, leaving it to solidify naturally at room temperature, and then taking it out for drying to obtain a green embryo; S4: heating and sintering the green body to form pores inside to obtain a silicon nitride ceramic material; The process of determining the second-order spectral absorption peak wave number ratio coefficient is as follows: The wavenumbers corresponding to all the peak points and all the trough points in the second-order derivative spectrum of the Fourier transform infrared spectrum data of the slurry at each moment are used to form the FT-IR second-order spectrum absorption peak wavenumber set of the slurry at each moment, and the FT-IR second-order spectrum absorption peak wavenumber set of various raw materials is obtained by the same method, and the intersection of the FT-IR second-order spectrum absorption peak wavenumber sets of all raw materials is used as the common absorption peak wavenumber set of raw materials; The wavenumbers in the common absorption peak wavenumber set of the raw materials are removed from the FT-IR second-order spectrum absorption peak wavenumber set of various raw materials to obtain the unique absorption peak wavenumber set of various raw materials, and the number of overlapping wavenumbers in the FT-IR second-order spectrum absorption peak wavenumber set of the slurry at each moment is counted, and the ratio of the number of overlapping wavenumbers to the number of wavenumbers in the unique absorption peak wavenumber set is used as the second-order spectrum absorption peak wavenumber ratio coefficient of the slurry in various raw materials at each moment; The determination process of the ceramic slurry mixing coefficient is: At each moment, all the wavenumbers in the unique absorption peak wavenumber set of the raw material corresponding to the maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient are eliminated from the FT-IR second-order spectrum absorption peak wavenumber set of the slurry, and the raw material corresponding to the maximum value is eliminated at the same time, and the second-order spectrum absorption peak wavenumber ratio coefficient of the FT-IR second-order spectrum absorption peak wavenumber set of the slurry after elimination and the unique absorption peak wavenumber set of various raw materials remaining after elimination are calculated, and all the wavenumbers in the unique absorption peak wavenumber set of the raw material corresponding to the maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient are continued to be eliminated from the FT-IR second-order spectrum absorption peak wavenumber set of the slurry by the same method, and the second-order spectrum absorption peak wavenumber ratio coefficient is repeatedly calculated, and when the calculated maximum value of the second-order spectrum absorption peak wavenumber ratio coefficient is less than a preset threshold, the calculation is stopped; Calculate the ratio of the number of remaining raw materials to the total number of raw materials, and obtain the ceramic slurry mixing coefficient at each moment by inverse proportional mapping, wherein the preset threshold is the minimum value of the second-order spectral absorption peak wave number ratio coefficient of the ceramic slurry whose mixing degree meets the production standard among all kinds of raw materials; The control of the stirring time of the slurry includes: Calculate the coefficient of variation of the ceramic slurry mixing coefficient in the local time period at each moment, and map the coefficient of variation in inverse proportion as the ceramic slurry stirring completion degree at each moment. When the ceramic slurry stirring completion degree is greater than or equal to the ceramic slurry mixing completion threshold, stop stirring. The ceramic slurry mixing completion threshold is the average of the ceramic slurry stirring completion degrees of multiple ceramic slurries whose mixing degrees meet the production standards at the last moment in the stirring process.
2. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The silicon nitride powder accounts for 85 to 105 parts, the pore-forming agent is aluminum hydroxide, which accounts for 11 to 16 parts by weight, and the surfactant is sodium dodecylbenzene sulfonate, which accounts for 2.0 to 2.5 parts by weight.
3. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The wet grinding condition is to ensure that the powder with a particle size of 4 to 20 μm accounts for more than 95%.
4. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The raw material powder is 90-110 parts, the monomer is 6-12 parts, the cross-linking agent is 4-5 parts, the initiator is 0.3-0.8 parts, the catalyst is 0.6-1 parts, the deionized water is 30-50 parts, and the ethanol is 30-40 parts.
5. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The monomer is acrylamide, the cross-linking agent is hydroxyethyl acrylate, the initiator is ammonium sulfate, and the catalyst is hydroxymethyl acrylamide.
6. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The natural curing time is 1 to 5 hours.
7. A method for preparing a silicon nitride ceramic material according to claim 1, characterized in that: The green embryo heating and sintering comprises: First, heat the temperature to 300~600℃ at a heating rate of 1~2℃ / min and keep it warm for 1~3 hours. Then, in a nitrogen atmosphere, continue heating at a heating rate of 1~2℃ / min to 800~1000℃ and keep it warm for 1~2 hours. Finally, continue heating at a heating rate of 5~8℃ / min under a pressure of 0.3~0.5MPa to 1300~1800℃ and keep it warm for 1~6 hours.