Corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank and preparation method thereof
By using materials such as self-healing modified fillers and chelated graft-modified carbon fibers to prepare modified polytetrafluoroethylene coatings in steel-lined PTFE storage tanks, the problem of poor bonding strength between polytetrafluoroethylene and steel plates is solved and improved Improves the corrosion resistance, high temperature resistance and service life of the storage tank.
Patent Information
- Application Number
- CN202410484296.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-22
AI Technical Summary
During the use of existing steel-lined PTFE storage tanks, due to the poor bonding force between PTFE and the steel plate base material, the coating peels off and the service life is difficult to meet expectations.
Self-healing modified fillers, chelated grafted modified carbon fiber and epoxy resin are used to prepare modified polytetrafluoroethylene coatings, which are sprayed on the inside of the steel lining to form a modified polytetrafluoroethylene coating to improve coating performance. The bonding strength and corrosion resistance and high temperature resistance between the layer and the steel lining base material.
It significantly improves the bonding strength and service life of the coating, prevents the coating from falling off, enhances the high temperature resistance and corrosion resistance of the coating, and gives it self-healing capabilities.
Smart Images

Figure BDA0004803253400000021 
Figure BDA0004803253400000061 
Figure BDA0004803253400000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of storage tank equipment, and in particular to a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank and a preparation method thereof. Background Art
[0002] Steel-lined PTFE storage tanks (i.e., steel-lined polytetrafluoroethylene storage tanks) are generally composed of two layers of materials: the inner layer is polytetrafluoroethylene (PTFE) and the outer layer is carbon steel. PTFE is a material with excellent corrosion resistance and high temperature stability, which can play an excellent anti-corrosion role in harsh chemical media; while the carbon steel layer has high strength and stability, which can ensure the structural stability and safety of the entire storage tank. Therefore, this type of storage tank has both the strength of steel and the corrosion resistance of polytetrafluoroethylene plastic, with a flat appearance, smooth inner wall, impact resistance, high and low temperature resistance, high strength, anti-aging, no leakage, non-toxicity, acid and alkali resistance, resistance to various organic acids, inorganic acids, various solutions, and long service life; making this type of storage tank widely used in industry, such as for the storage and transportation of chemical substances such as acids, alkalis, and salts. For example, CN114313670B discloses a steel-lined polytetrafluoroethylene high temperature resistant storage tank.
[0003] However, polytetrafluoroethylene has strong chemical inertness, low surface energy and poor bonding with the steel plate substrate. The coating solution separates during use, resulting in the actual use effect and service life of the PTFE coating often failing to meet expectations.
[0004] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank and a preparation method thereof in view of the deficiencies in the above-mentioned prior art.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, comprising the following steps:
[0007] Step 1: Process the steel plate into a steel-lined tank body;
[0008] Step 2: pre-treat the inner wall of the steel-lined tank;
[0009] Step 3: spraying a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, and then heating and curing the coating to form a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, thereby obtaining a storage tank blank;
[0010] Step 4: Processing the storage tank blank into a storage tank product, that is, obtaining the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank.
[0011] Preferably, the modified reinforced polytetrafluoroethylene coating comprises the following raw material components in parts by weight:
[0012]
[0013] Preferably, the self-healing modified filler is prepared by the following method:
[0014] S1-1. Preparation of carbon spheres:
[0015] Glucose and citric acid are added to deionized water, ultrasonically dispersed, and the resulting mixture is transferred to a reactor, heated for reaction, cooled to room temperature after the reaction is completed, filtered with a filter membrane, and the resulting solid product is calcined to obtain carbon spheres;
[0016] S1-2. Preparation of mesoporous hollow alumina:
[0017] Add Tween-80 to a mixed solution of ethanol and deionized water, then add Al(NO3)3, stir, then add the carbon spheres prepared in step S1-1, stir, filter, wash the solid product with deionized water, then dry, calcine, and cool to room temperature to obtain mesoporous hollow alumina;
[0018] S1-3. Preparation of modified mesoporous hollow alumina:
[0019] The mesoporous hollow alumina was added to ethanol for ultrasonic dispersion, and then KH570 was added, the mixture was sealed and stirred, filtered, the product was washed with ethanol, and vacuum dried to obtain modified mesoporous hollow alumina;
[0020] S1-4. Preparation of loaded modified mesoporous hollow alumina:
[0021] The modified mesoporous hollow alumina is added to ethanol, ultrasonically dispersed, and then tung oil formate is added dropwise under continuous stirring. After the addition, the mixture is shaken on a shaker, impregnated, filtered, and the solid product is washed with deionized water and vacuum dried to obtain the loaded modified mesoporous hollow alumina.
[0022] S1-5, heating and blending the acrylic acid-maleic acid copolymer and the loaded modified mesoporous hollow alumina to prepare a self-healing modified filler.
[0023] Preferably, the self-healing modified filler is prepared by the following method:
[0024] S1-1. Preparation of carbon spheres:
[0025] 1-4 g of glucose and 0.65-2.6 g of citric acid are added to 50-200 mL of deionized water, and ultrasonically dispersed for 15-60 min. The resulting mixed solution is transferred to a reactor, and reacted at 170-190 ° C for 4-12 h. After the reaction is completed, the mixture is cooled to room temperature and filtered with a 1-3 μm filter membrane. The resulting solid product is heated to 550-700 ° C at a heating rate of 5-20 ° C / min and kept warm for 1-4 h to obtain carbon spheres;
[0026] S1-2. Preparation of mesoporous hollow alumina:
[0027] 1.1-4.4 g of Tween-80 is added to a mixed solution consisting of 10-40 mL of ethanol and 2-8 mL of deionized water, and then 10-40 mmol of Al(NO3)3 is added, stirred for 2-10 min, and then 0.4-1.7 g of the carbon spheres prepared in step S1-1 are added, stirred for 3-10 h, filtered, the solid product is washed with deionized water, and then dried at 65-80 ° C for 3-12 h, heated to 600-700 ° C at a heating rate of 5-20 ° C / min, kept warm for 1-4 h, and cooled to room temperature to obtain mesoporous hollow alumina;
[0028] S1-3. Preparation of modified mesoporous hollow alumina:
[0029] 1-4 g of mesoporous hollow alumina was added to 25-100 mL of ethanol and ultrasonically dispersed for 10-40 min, then 0.16-0.7 g of KH570 was added, and the mixture was sealed and stirred at 35-45° C. for 2-8 h, filtered, and the product was washed with ethanol, and vacuum dried at 60-80° C. for 3-12 h to obtain modified mesoporous hollow alumina;
[0030] S1-4. Preparation of loaded modified mesoporous hollow alumina:
[0031] Take 1-4g of modified mesoporous hollow alumina and add it to 50-200mL of ethanol, ultrasonically disperse it for 5-30min, then add 0.75-3g of tung oil formate dropwise under continuous stirring within 5-20min, shake on a shaker for 1-4h, then soak at 25-35°C for 6-24h, filter, wash the solid product with deionized water, and vacuum dry at 40-60°C for 4-12h to obtain loaded modified mesoporous hollow alumina;
[0032] S1-5, 32-128 mg of acrylic acid maleic acid copolymer and 18-72 mg of loaded modified mesoporous hollow alumina are mixed, and then blended at a rotation speed of 50-200 rpm and 130-150° C. for 5-30 min, and cooled to room temperature to obtain a self-healing modified filler.
[0033] Preferably, the chelate grafted modified carbon fiber is prepared by the following method:
[0034] S2-1, adding carbon fiber powder into acetone, and ultrasonically dispersing the mixture to obtain a carbon fiber dispersion;
[0035] S2-2, adding acrylonitrile to acetone and stirring; then adding carbon fiber dispersion under continuous stirring, sealing and ultrasonically oscillating, and then irradiating. After irradiation, filtering, soaking the solid product with acetone, filtering, washing the solid product with ethanol, and then vacuum drying to obtain a modified carbon fiber intermediate;
[0036] S2-3. Take the modified carbon fiber intermediate, diethylenetriamine and aluminum chloride, add them into acetone, stir, and then react under heating. After the reaction is completed, cool to room temperature, filter, wash the solid product with ethanol, and then vacuum dry to obtain chelated grafted modified carbon fiber.
[0037] Preferably, the chelate grafted modified carbon fiber is prepared by the following method:
[0038] S2-1, adding 4-16 g of carbon fiber powder to 30-120 g of acetone, and ultrasonically dispersing for 15-60 min to obtain a carbon fiber dispersion;
[0039] S2-2, add 7.5-30g acrylonitrile to 50-200g acetone, stir for 2-15min; then add carbon fiber dispersion under continuous stirring, ultrasonically oscillate for 2-8h under sealing, and then irradiate, control the irradiation dose to 50-200KGy, filter after irradiation, soak the solid product with acetone for 1-4h, filter, wash the solid product with ethanol, and then vacuum dry at 70-90°C for 2-8h to obtain a modified carbon fiber intermediate;
[0040] S2-3, take 5-20g of modified carbon fiber intermediate, 0.9-3.6g of diethylenetriamine, and 0.18-0.74g of aluminum chloride, add them to 50-200g of acetone, stir at 150-600rpm for 15-60min, then react at 115-140℃ for 1-4h, cool to room temperature, filter, wash the solid product with ethanol, and then vacuum dry at 70-90℃ for 6-24h to obtain chelated grafted modified carbon fiber.
[0041] Preferably, the epoxy resin is a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin in a mass ratio of 3:2.
[0042] Preferably, the preparation method of the modified reinforced polytetrafluoroethylene coating is: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin, and polyamide wax powder are mixed in proportion by weight, and stirred at 800-3000 rpm for 5-15 minutes to obtain the modified polytetrafluoroethylene coating.
[0043] Preferably, the method for preparing the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank comprises the following steps:
[0044] Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding;
[0045] Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 20-200g / m 2 After spraying, let it stand for 2-15 minutes, then rinse with deionized water, repeat 2-8 times, and then blow dry to complete the pretreatment;
[0046] Wherein, the mixed acid is a mixed solution of H2O2 and H2SO4, the mass fraction of H2O2 is 0.5-10%, and the mass fraction of H2SO4 is 5-45%;
[0047] Step 3: spraying a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, and then curing it at 180-220° C. for 5-20 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 3-8 mm on the inner surface of the steel plate to obtain a storage tank blank;
[0048] Step 4: Processing the storage tank blank into a storage tank product, that is, obtaining the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank.
[0049] The present invention also provides a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, which is prepared by the method as described above.
[0050] The beneficial effects of the present invention are:
[0051] The present invention provides a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank and a preparation method thereof. A modified polytetrafluoroethylene coating is prepared by compounding self-healing modified filler, chelate grafted modified carbon fiber, epoxy resin, polyamide wax powder and polytetrafluoroethylene. The modified polytetrafluoroethylene coating is used to arrange a modified polytetrafluoroethylene coating on the inner side of the steel lining, thereby giving the steel lining excellent corrosion resistance and high-temperature resistance.
[0052] In the present invention, the polytetrafluoroethylene is subjected to multi-effect modification treatment by using self-healing modified filler and chelated grafted modified carbon fiber, which can greatly improve the bonding strength between the formed coating and the steel lining substrate, effectively prevent the coating from falling off, and improve the use effect of the coating;
[0053] In the present invention, the self-healing modified filler can not only improve the high temperature resistance and strength of the coating, and give the coating a certain self-repairing ability, but also improve the bonding strength between the coating and the steel plate substrate, thereby improving the effect of the coating and extending its service life;
[0054] In the present invention, the chelate grafting modification of the carbon fiber can not only overcome the problem of poor compatibility of the carbon fiber in polytetrafluoroethylene, but also improve the bonding strength between the coating and the steel plate substrate. DETAILED DESCRIPTION
[0055] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0056] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0057] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0058] The present invention provides a method for preparing a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, comprising the following steps:
[0059] Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding;
[0060] Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 20-200g / m 2 After spraying, let it stand for 2-15 minutes, then rinse with deionized water, repeat 2-8 times, and then blow dry to complete the pretreatment;
[0061] The mixed acid is a mixed solution of H2O2 and H2SO4, the mass fraction of H2O2 is 0.5-10%, and the mass fraction of H2SO4 is 5-45%;
[0062] The mixed acid corrosion on the steel plate surface forms a rough surface structure that is conducive to the adhesion of the coating, and the acid can produce metal ions (mainly iron ions) on the surface, so that the modified and enhanced polytetrafluoroethylene coating can be used to achieve better adhesion in the future;
[0063] Step 3: spraying a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, and then curing it at 180-220° C. for 5-20 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 3-8 mm on the inner surface of the steel plate to obtain a storage tank blank;
[0064] Step 4: Process the tank blank into a tank product (assemble the cover plate and other accessories according to the specific purpose), and obtain a corrosion-resistant and high-temperature resistant steel-lined PTFE tank.
[0065] It should be understood that the outer wall of the storage tank can also be sprayed with conventional anti-corrosion coatings, such as epoxy resin coatings, etc. as needed, and this is not limited in the present invention.
[0066] In a preferred embodiment, the modified reinforced polytetrafluoroethylene coating comprises the following raw material components in parts by weight:
[0067]
[0068]
[0069] In a preferred embodiment, the self-healing modified filler is prepared by the following method:
[0070] S1-1. Preparation of carbon spheres:
[0071] 1-4 g of glucose and 0.65-2.6 g of citric acid are added to 50-200 mL of deionized water, and ultrasonically dispersed for 15-60 min. The resulting mixed solution is transferred to a reactor, and reacted at 170-190 ° C for 4-12 h. After the reaction is completed, the mixture is cooled to room temperature and filtered with a 1-3 μm filter membrane. The resulting solid product is heated to 550-700 ° C at a heating rate of 5-20 ° C / min and kept warm for 1-4 h to obtain carbon spheres;
[0072] S1-2. Preparation of mesoporous hollow alumina:
[0073] 1.1-4.4 g of Tween-80 is added to a mixed solution consisting of 10-40 mL of ethanol and 2-8 mL of deionized water, and then 10-40 mmol of Al(NO3)3 is added, stirred for 2-10 min, and then 0.4-1.7 g of the carbon spheres prepared in step S1-1 are added, stirred for 3-10 h, filtered, the solid product is washed with deionized water, and then dried at 65-80 ° C for 3-12 h, heated to 600-700 ° C at a heating rate of 5-20 ° C / min, kept warm for 1-4 h, and cooled to room temperature to obtain mesoporous hollow alumina;
[0074] S1-3. Preparation of modified mesoporous hollow alumina:
[0075] 1-4 g of mesoporous hollow alumina was added to 25-100 mL of ethanol and ultrasonically dispersed for 10-40 min, then 0.16-0.7 g of KH570 (silane coupling agent, γ-(methacryloyloxy)propyltrimethoxysilane) was added, and the mixture was sealed and stirred at 35-45° C. for 2-8 h, filtered, and the product was washed with ethanol, and vacuum dried at 60-80° C. for 3-12 h to obtain modified mesoporous hollow alumina;
[0076] S1-4. Preparation of loaded modified mesoporous hollow alumina:
[0077] Take 1-4g of modified mesoporous hollow alumina and add it to 50-200mL of ethanol, ultrasonically disperse it for 5-30min, then add 0.75-3g of tung oil formate dropwise under continuous stirring within 5-20min, shake on a shaker for 1-4h, then soak at 25-35°C for 6-24h, filter, wash the solid product with deionized water, and vacuum dry at 40-60°C for 4-12h to obtain loaded modified mesoporous hollow alumina;
[0078] S1-5, 32-128 mg of acrylic acid maleic acid copolymer and 18-72 mg of loaded modified mesoporous hollow alumina are mixed, and then blended at a rotation speed of 50-200 rpm and 130-150° C. for 5-30 min, and cooled to room temperature to obtain a self-healing modified filler.
[0079] In a preferred embodiment, the chelate grafted modified carbon fiber is prepared by the following method:
[0080] S2-1, adding 4-16 g of carbon fiber powder into 30-120 g of acetone, and ultrasonically dispersing for 15-60 min to obtain a carbon fiber dispersion;
[0081] S2-2, add 7.5-30g acrylonitrile to 50-200g acetone, stir for 2-15min; then add carbon fiber dispersion under continuous stirring, ultrasonically oscillate for 2-8h under sealing, and then irradiate, control the irradiation dose to 50-200KGy, filter after irradiation, soak the solid product with acetone for 1-4h, filter, wash the solid product with ethanol, and then vacuum dry at 70-90°C for 2-8h to obtain a modified carbon fiber intermediate;
[0082] S2-3, take 5-20g of modified carbon fiber intermediate, 0.9-3.6g of diethylenetriamine, and 0.18-0.74g of aluminum chloride, add them to 50-200g of acetone, stir at 150-600rpm for 15-60min, then react at 115-140℃ for 1-4h, cool to room temperature, filter, wash the solid product with ethanol, and then vacuum dry at 70-90℃ for 6-24h to obtain chelated grafted modified carbon fiber.
[0083] In a preferred embodiment, the epoxy resin is a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin in a mass ratio of 3:2.
[0084] In a preferred embodiment, the preparation method of the modified reinforced polytetrafluoroethylene coating is as follows: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin, and polyamide wax powder are mixed in proportion by weight, and stirred at 800-3000 rpm for 5-15 minutes to obtain the modified polytetrafluoroethylene coating.
[0085] PTFE (polytetrafluoroethylene) is a material with excellent corrosion resistance and high temperature stability. It can effectively resist the erosion of various chemical media and has a wide range of corrosion resistance and high temperature resistance. Forming a coating on a steel plate to prepare a storage tank can theoretically greatly improve the corrosion resistance and high temperature resistance of the storage tank. However, due to the low surface energy and strong inertia of the conventional PTFE, the bonding force between the PTFE coating and the steel plate substrate is poor. The coating solution is separated during use, resulting in the actual use effect and service life of the PTFE coating being difficult to achieve the expected results.
[0086] In the present invention, a modified polytetrafluoroethylene coating is prepared by compounding self-healing modified fillers, chelated grafted modified carbon fibers, epoxy resins, polyamide wax powders and polytetrafluoroethylene, and polytetrafluoroethylene is subjected to multi-effect modification by using self-healing modified fillers and chelated grafted modified carbon fibers, which can greatly improve the bonding strength between the formed coating and the steel substrate, effectively prevent the coating from falling off, improve the use effect of the coating, and also give the coating a certain self-healing property, thereby further improving the corrosion and temperature resistance of the coating and extending its service life. The main mechanism of the modified polytetrafluoroethylene coating is described in detail below in conjunction with a specific preparation method to facilitate understanding of the present invention.
[0087] 1. Self-healing modified filler
[0088] Firstly, mesoporous hollow alumina with rich pore structure was prepared using carbon spheres as templates. Mesoporous hollow alumina as the main filler can improve the high temperature resistance and strength of the coating.
[0089] Then, modified mesoporous hollow alumina was prepared by surface-modifying KH570. The modification of KH570 can improve the dispersibility of mesoporous hollow alumina in organic systems and reduce its agglomeration.
[0090] Then, through the impregnation method, tung oil formate is loaded on its pore structure to obtain loaded modified mesoporous hollow alumina; tung oil formate has abundant unsaturated =CH and C=O bonds, and has active chemical properties. It can undergo cross-linking polymerization under the action of oxygen, thereby playing a role in repairing the coating (Chen Fanshi, Qin Zirun, Yang Yan, et al. Research and Development of Tung Oil-Based Self-Healing Coatings [J]. Electroplating and Finishing, 2021, 40(24): 6.); and loading it in the pore structure of mesoporous hollow alumina can achieve a long-term sustained release effect. By continuously and slowly releasing tung oil formate, it can provide a long-term repair function for the coating; at the same time, because tung oil formate can consume oxygen, it can also play a role in slowing down oxygen aging;
[0091] Finally, acrylic acid-maleic acid copolymer was grafted onto the surface of the loaded modified mesoporous hollow alumina by heating and blending to prepare the final self-healing modified filler.
[0092] The grafting of acrylic acid maleic acid copolymer can further improve the compatibility of mesoporous hollow alumina in the organic coating system, so that it can be evenly dispersed, thereby giving full play to its reinforcing effect; in addition, there are a large number of carboxylic acids in the acrylic acid maleic acid copolymer, and the carboxyl oxygen atom has the ability to form coordination bonds and can form stable chelates with metal ions; the steel plate can form a large number of metal ions (mainly iron ions) on the surface through pretreatment before spraying the paint, and after the acrylic acid maleic acid copolymer forms coordination bonds with the metal ions on the surface of the steel plate, the bonding strength between the coating system and the steel plate substrate is significantly improved.
[0093] Therefore, the self-healing modified filler can not only improve the high temperature resistance and strength of the coating and give the coating a certain self-repair ability, but also improve the bonding strength between the coating and the steel plate substrate, thereby improving the effect of the coating and extending its service life.
[0094] 2. Chelation grafting modified carbon fiber
[0095] Carbon fiber can improve the heat resistance, corrosion resistance and mechanical properties of polytetrafluoroethylene coatings, but carbon fiber has poor compatibility in polytetrafluoroethylene and is easily agglomerated and cannot effectively play its reinforcing role, and even easily has a negative impact on the mechanical properties of the agglomerated area. The chelate grafting modification of carbon fiber in the present invention can overcome the above problems while also improving the bonding strength between the coating and the steel plate substrate.
[0096] In the present invention, acrylonitrile is first modified on the carbon fiber by irradiation treatment, and then an amination treatment is performed to graft rich chelated chains with amino groups on the carbon fiber. These chelated chains can form coordination bonds with metal ions, such as iron ions, formed on the surface of the steel plate, thereby improving the bonding strength between the coating and the steel plate substrate; at the same time, it can also help the carbon fiber to maintain a uniform and stable dispersion state in the coating system, so that its reinforcement effect can be fully exerted.
[0097] Therefore, chelated grafted modified carbon fibers can further enhance the bonding strength between the coating and the steel plate substrate, and can improve the coating's heat resistance, corrosion resistance, and mechanical properties.
[0098] Polyamide wax powder can improve the water resistance, oil resistance, wear resistance and corrosion resistance of coatings.
[0099] The addition of epoxy resin can improve the mechanical properties of polytetrafluoroethylene, and epoxy resin has good adhesion, which can improve the bonding strength between polytetrafluoroethylene and the substrate.
[0100] The above is the general concept of the present invention, and detailed examples and comparative examples are provided below on the basis of the above to further illustrate the present invention. The main raw materials and equipment used in the following examples and comparative examples are from the following sources.
[0101] Polytetrafluoroethylene powder, brand 605XTX, Chemours, USA;
[0102] The epoxy resin is a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin, with a mass ratio of 3:2; bisphenol A epoxy resin E12 Sinopec; bisphenol F epoxy resin Jiangsu Bosite Chemical Technology Co., Ltd.;
[0103] Carbon fiber powder, diameter 5 μm, Zhejiang Yamei Nano Technology Co., Ltd.;
[0104] Polyamide wax powder, model PA-8610, Zhejiang Huate New Materials Co., Ltd.;
[0105] Acrylic acid maleic acid copolymer ((Z)-2-butenedioic acid and 2-acrylic acid polymer), CAS: 29132-58-9, Hubei Watson Chemical Technology Co., Ltd.;
[0106] Acrylonitrile, Shandong Huayu Chemical Technology Co., Ltd.;
[0107] The steel plate is 45 carbon steel;
[0108] Spraying equipment, HXD-882A electrostatic sprayer;
[0109] Irradiation equipment, γ-ray radiation source (60Co), Changchun Institute of Applied Chemistry.
[0110] The preparation methods of the self-healing modified fillers and chelate grafted modified carbon fibers involved in the following examples and comparative examples are the same, and are shown below.
[0111] 1. The self-healing modified filler is prepared by the following method:
[0112] S1-1. Preparation of carbon spheres:
[0113] Add 2g of glucose and 1.3g of citric acid into 100mL of deionized water and disperse ultrasonically for 30min. Transfer the obtained mixed solution into a reactor and react at 180℃ for 8h. After the reaction, return the temperature to room temperature and filter with a 2μm filter membrane. Heat the solid product to 650℃ at a heating rate of 10℃ / min and keep warm for 2h to obtain carbon spheres.
[0114] S1-2. Preparation of mesoporous hollow alumina:
[0115] 2.2 g of Tween-80 was added to a mixed solution consisting of 20 mL of ethanol and 4 mL of deionized water, and then 20 mmol of Al(NO3)3 was added, stirred for 5 min, and then 0.85 g of the carbon spheres prepared in step 1-1-1 were added, stirred for 6 h, filtered, and the solid product was washed with deionized water, then dried at 75 ° C for 6 h, heated to 650 ° C at a heating rate of 10 ° C / min, kept warm for 2 h, and cooled to room temperature to obtain mesoporous hollow alumina; the average particle size was 550 nm, and the BET specific surface area was 172 m 2 / g.
[0116] S1-3. Preparation of modified mesoporous hollow alumina:
[0117] 2 g of mesoporous hollow alumina was added to 50 mL of ethanol and ultrasonically dispersed for 20 min, then 0.35 g of KH570 was added, sealed and stirred at 40° C. for 4 h, filtered, the product was washed with ethanol, and vacuum dried at 70° C. for 6 h to obtain modified mesoporous hollow alumina.
[0118] S1-4. Preparation of loaded modified mesoporous hollow alumina:
[0119] Take 2g of modified mesoporous hollow alumina and add it to 100mL of ethanol, ultrasonically disperse it for 10min, then add 1.5g of tung oil formate dropwise under continuous stirring within 10min, shake it on a shaker for 2h, then immerse it at 30℃ for 12h, filter it, wash the solid product with deionized water, and vacuum dry it at 50℃ for 8h to obtain loaded modified mesoporous hollow alumina;
[0120] Wherein, the preparation method of tung oil formate is:
[0121] 50 g of tung oil was added to a three-necked flask equipped with an electric stirrer and a condenser reflux tube, preheated at 65°C for 25 min, and then a methanol solution of KOH was added (the mass of KOH was 1.1% of tung oil, and the molar ratio of methanol to tung oil was 9:1). The mixture was stirred and refluxed at 70°C and 350 rpm for 1 h, cooled to room temperature, and the product was transferred to a separatory funnel and allowed to stand for stratification. The upper layer of liquid was taken and rotary evaporated to remove methanol to obtain tung oil formate (refer to the literature "Yang Ningning, Yu Yun, Huang Bin, et al. Process optimization study on the preparation of tung oil C18 unsaturated fatty acid methyl ester by urea inclusion method [J]. China Oils and Fats, 2019(6):5. DOI:CNKI:SUN:ZYZZ.0.2019-06-014.").
[0122] S1-5, 64 mg of acrylic acid-maleic acid copolymer and 36 mg of loaded modified mesoporous hollow alumina were mixed, and then blended at a rotation speed of 100 rpm and 140° C. for 15 min, and cooled to room temperature to obtain a self-healing modified filler.
[0123] 2. The chelate grafted modified carbon fiber is prepared by the following method:
[0124] S2-1, adding 8 g of carbon fiber powder into 60 g of acetone, and ultrasonically dispersing for 30 min to obtain a carbon fiber dispersion;
[0125] S2-2, add 15g of acrylonitrile to 100g of acetone and stir for 5min; then add the carbon fiber dispersion under continuous stirring, seal and ultrasonically oscillate for 4h, then irradiate with a γ-ray radiation source (60Co), control the irradiation dose to 120KGy, filter after irradiation, soak the solid product with acetone for 2h, filter, wash the solid product with ethanol, and then vacuum dry at 80°C for 5h to obtain a modified carbon fiber intermediate;
[0126] S2-3, take 10g of modified carbon fiber intermediate, 1.8g of diethylenetriamine, and 0.37g of aluminum chloride, add them into 100g of acetone, stir at 300rpm for 30min, then react at 125℃ for 2h, cool to room temperature, filter, wash the solid product with ethanol, and then vacuum dry at 80℃ for 12h to obtain chelated grafted modified carbon fiber.
[0127] Example 1
[0128] A corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, the preparation method of which comprises the following steps:
[0129] Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding;
[0130] Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 50g / m 2 After spraying, let it stand for 5 minutes, then rinse with deionized water, repeat 4 times, and then blow dry to complete the pretreatment;
[0131] The mixed acid is a mixed solution of H2O2 and H2SO4, with the mass fraction of H2O2 being 3% and the mass fraction of H2SO4 being 20%;
[0132] Step 3: spray the modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body by using a spraying device, and then cure it at 200° C. for 12 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 5 mm on the inner surface of the steel plate to obtain a storage tank blank;
[0133] Step 4: Process the tank blank into a tank product, that is, obtain a corrosion-resistant and high-temperature-resistant steel-lined PTFE tank.
[0134] In this embodiment, the modified reinforced polytetrafluoroethylene coating includes the following raw material components in parts by weight:
[0135]
[0136] The preparation method of the modified reinforced polytetrafluoroethylene coating is as follows: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin, and polyamide wax powder are mixed according to weight proportions, and stirred at 1500 rpm for 8 minutes to obtain the modified polytetrafluoroethylene coating.
[0137] Example 2
[0138] A corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, the preparation method of which comprises the following steps:
[0139] Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding;
[0140] Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 50g / m 2 After spraying, let it stand for 5 minutes, then rinse with deionized water, repeat 4 times, and then blow dry to complete the pretreatment;
[0141] The mixed acid is a mixed solution of H2O2 and H2SO4, with the mass fraction of H2O2 being 3% and the mass fraction of H2SO4 being 20%;
[0142] Step 3: spray the modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body by using a spraying device, and then cure it at 200° C. for 12 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 5 mm on the inner surface of the steel plate to obtain a storage tank blank;
[0143] Step 4: Process the tank blank into a tank product, that is, obtain a corrosion-resistant and high-temperature-resistant steel-lined PTFE tank.
[0144] In this embodiment, the modified reinforced polytetrafluoroethylene coating includes the following raw material components in parts by weight:
[0145]
[0146]
[0147] The preparation method of the modified reinforced polytetrafluoroethylene coating is as follows: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin, and polyamide wax powder are mixed according to weight proportions, and stirred at 1500 rpm for 8 minutes to obtain the modified polytetrafluoroethylene coating.
[0148] Example 3
[0149] A corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, the preparation method of which comprises the following steps:
[0150] Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding;
[0151] Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 50g / m 2 After spraying, let it stand for 5 minutes, then rinse with deionized water, repeat 4 times, and then blow dry to complete the pretreatment;
[0152] The mixed acid is a mixed solution of H2O2 and H2SO4, with the mass fraction of H2O2 being 3% and the mass fraction of H2SO4 being 20%;
[0153] Step 3: spray the modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body by using a spraying device, and then cure it at 200° C. for 12 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 5 mm on the inner surface of the steel plate to obtain a storage tank blank;
[0154] Step 4: Process the tank blank into a tank product, that is, obtain a corrosion-resistant and high-temperature-resistant steel-lined PTFE tank.
[0155] In this embodiment, the modified reinforced polytetrafluoroethylene coating includes the following raw material components in parts by weight:
[0156]
[0157] The preparation method of the modified reinforced polytetrafluoroethylene coating is as follows: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin, and polyamide wax powder are mixed according to weight proportions, and stirred at 1500 rpm for 8 minutes to obtain the modified polytetrafluoroethylene coating.
[0158] Comparative Example 1
[0159] This example is basically the same as Example 1, except that the modified reinforced polytetrafluoroethylene coating in this example includes the following raw material components in parts by weight:
[0160]
[0161] Comparative Example 2
[0162] This example is basically the same as Example 1, except that the modified reinforced polytetrafluoroethylene coating in this example includes the following raw material components in parts by weight:
[0163]
[0164] Comparative Example 3
[0165] This example is basically the same as Example 1, except that the modified reinforced polytetrafluoroethylene coating in this example includes the following raw material components in parts by weight:
[0166] 100 parts of polytetrafluoroethylene powder;
[0167] Epoxy resin 17 parts;
[0168] 5.6 parts of polyamide wax powder.
[0169] Comparative Example 4
[0170] This example is basically the same as Example 1, except that the modified reinforced polytetrafluoroethylene coating in this example includes the following raw material components in parts by weight:
[0171]
[0172] Wherein, the preparation method of mesoporous hollow alumina is:
[0173] S1-1. Preparation of carbon spheres:
[0174] Add 2g of glucose and 1.3g of citric acid into 100mL of deionized water and disperse ultrasonically for 30min. Transfer the obtained mixed solution into a reactor and react at 180℃ for 8h. After the reaction, return the temperature to room temperature and filter with a 2μm filter membrane. Heat the solid product to 650℃ at a heating rate of 10℃ / min and keep warm for 2h to obtain carbon spheres.
[0175] S1-2. Preparation of mesoporous hollow alumina:
[0176] 2.2 g of Tween-80 was added to a mixed solution consisting of 20 mL of ethanol and 4 mL of deionized water, and then 20 mmol of Al(NO3)3 was added, stirred for 5 min, and then 0.85 g of the carbon spheres prepared in step 1-1-1 were added, stirred for 6 h, filtered, and the solid product was washed with deionized water, then dried at 75 ° C for 6 h, heated to 650 ° C at a heating rate of 10 ° C / min, kept warm for 2 h, and cooled to room temperature to obtain mesoporous hollow alumina; the average particle size was 550 nm, and the BET specific surface area was 172 m 2 / g.
[0177] Comparative Example 5
[0178] This example is basically the same as Example 1, except that the modified reinforced polytetrafluoroethylene coating in this example includes the following raw material components in parts by weight:
[0179]
[0180] Performance Testing
[0181] A steel plate (10 cm×4 cm) was taken, and a coating was prepared on the steel plate in the same manner as in Examples 1-3 and Comparative Examples 1-4 to obtain several test samples, which were used to perform the following performance tests:
[0182] 1. Bonding strength test:
[0183] Refer to the standard ASTM C633-79 "Coating Interface Bond Strength Tensile Test Standard" to test the bonding strength between the coating and the steel plate;
[0184] 2. Impact resistance
[0185] Refer to the standard GB / T1865-2009 "Determination of impact resistance of coatings and other organic coatings"
[0186] Use an impact tester with the coating of the sample facing upwards. The weight of the hammer of the impact tester is 1 kg, and the maximum height of the hammer is 50 cm. The hammer falls freely on the punch. After the impact, use a 4x magnifying glass to observe whether there are cracks or damage on the coating.
[0187] 3. High temperature and corrosion resistance test
[0188] (1) High temperature treatment: Place the sample with the coating facing up in a heating device, set the temperature to 150°C, and the treatment time to 3 h;
[0189] (2) Corrosion treatment: A spray device is used to continuously and evenly spray a corrosion solution composed of 5wt% sodium chloride and 20wt% hydrochloric acid onto the coating surface (the spraying amount of the corrosion solution is controlled to be 50g / (m 2 *min), treatment for 3h;
[0190] (3) High temperature treatment and corrosion treatment are carried out alternately for 3 times to complete the high temperature and corrosion resistance test.
[0191] The test results are shown in Table 1 below:
[0192] Table 1
[0193]
[0194] According to the test results in Table 1, it can be seen that the sample coatings prepared in Examples 1-3 have high bonding strength with the substrate, and the coatings have excellent impact resistance, high temperature resistance and corrosion resistance; the overall performance of Comparative Examples 1-3 all declined, which can fully illustrate the improvement effect of the self-healing modified filler and the chelated grafted modified carbon fiber on the coating bonding strength, high temperature resistance and corrosion resistance, and mechanical properties; the overall performance of Comparative Example 4 declined to a certain extent, which was attributed to the fact that the problem of easy aggregation of mesoporous hollow alumina in the coating system was not properly solved and the acrylic acid-maleic acid copolymer on the mesoporous hollow alumina had lost the effect of improving the bonding strength; the overall performance of Comparative Example 5 also declined to a certain extent, which was attributed to the fact that the defect of easy aggregation of carbon fibers in the coating system was not well overcome and the chelated chains on the carbon fibers had lost the effect of improving the bonding strength between the coating and the steel plate substrate.
[0195] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing a corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank, characterized in that: The following steps are involved: Step 1: Process the steel plate into a steel-lined tank body; Step 2: pre-treat the inner wall of the steel-lined tank; Step 3: spraying a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, and then heating and curing the coating to form a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, thereby obtaining a storage tank blank; Step 4: Processing the storage tank blank into a storage tank product, that is, obtaining the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank; The modified reinforced polytetrafluoroethylene coating comprises the following raw material components in parts by weight: 100 parts of polytetrafluoroethylene powder; 3-14 parts of self-healing modified filler; 2.2-8.5 parts of chelated grafted modified carbon fiber; Epoxy resin 9-34 parts; 2.3-12 parts of polyamide wax powder; The self-healing modified filler is prepared by the following method: S1-1. Preparation of carbon spheres: 1-4 g of glucose and 0.65-2.6 g of citric acid are added to 50-200 mL of deionized water, and ultrasonically dispersed for 15-60 min. The resulting mixed solution is transferred to a reactor, and reacted at 170-190 ° C for 4-12 h. After the reaction is completed, the mixture is cooled to room temperature and filtered with a 1-3 μm filter membrane. The resulting solid product is heated to 550-700 ° C at a heating rate of 5-20 ° C / min and kept warm for 1-4 h to obtain carbon spheres; S1-2. Preparation of mesoporous hollow alumina: 1.1-4.4 g of Tween-80 is added to a mixed solution consisting of 10-40 mL of ethanol and 2-8 mL of deionized water, and then 10-40 mmol of Al(NO3)3 is added, stirred for 2-10 min, and then 0.4-1.7 g of the carbon spheres prepared in step S1-1 are added, stirred for 3-10 h, filtered, the solid product is washed with deionized water, and then dried at 65-80 ° C for 3-12 h, heated to 600-700 ° C at a heating rate of 5-20 ° C / min, kept warm for 1-4 h, and cooled to room temperature to obtain mesoporous hollow alumina; S1-3. Preparation of modified mesoporous hollow alumina: 1-4 g of mesoporous hollow alumina was added to 25-100 mL of ethanol and ultrasonically dispersed for 10-40 min, then 0.16-0.7 g of KH570 was added, and the mixture was sealed and stirred at 35-45° C. for 2-8 h, filtered, and the product was washed with ethanol, and vacuum dried at 60-80° C. for 3-12 h to obtain modified mesoporous hollow alumina; S1-4, preparation of loaded modified mesoporous hollow alumina: 1-4 g of modified mesoporous hollow alumina is added to 50-200 mL of ethanol, and ultrasonically dispersed for 5-30 min. Then, 0.75-3 g of tung oil formate is added dropwise under continuous stirring within 5-20 min. The mixture is shaken on a shaker for 1-4 h, and then immersed at 25-35 ° C for 6-24 h. The solid product is filtered and washed with deionized water. The solid product is vacuum dried at 40-60 ° C for 4-12 h to obtain loaded modified mesoporous hollow alumina. S1-5, 32-128 mg of acrylic acid maleic acid copolymer and 18-72 mg of loaded modified mesoporous hollow alumina are mixed, and then blended at a speed of 50-200 rpm and 130-150° C. for 5-30 min, and cooled to room temperature to obtain a self-healing modified filler; The chelate grafted modified carbon fiber is prepared by the following method: S2-1, adding 4-16 g of carbon fiber powder to 30-120 g of acetone, and ultrasonically dispersing for 15-60 min to obtain a carbon fiber dispersion; S2-2, add 7.5-30g acrylonitrile to 50-200g acetone, stir for 2-15min; then add carbon fiber dispersion under continuous stirring, ultrasonically oscillate for 2-8h under sealing, and then irradiate, control the irradiation dose to 50-200KGy, filter after irradiation, soak the solid product with acetone for 1-4h, filter, wash the solid product with ethanol, and then vacuum dry at 70-90°C for 2-8h to obtain a modified carbon fiber intermediate; S2-3, take 5-20g of modified carbon fiber intermediate, 0.9-3.6g of diethylenetriamine, and 0.18-0.74g of aluminum chloride, add them to 50-200g of acetone, stir at 150-600rpm for 15-60min, then react at 115-140℃ for 1-4h, cool to room temperature, filter, wash the solid product with ethanol, and then vacuum dry at 70-90℃ for 6-24h to obtain chelated grafted modified carbon fiber.
2. The method for preparing the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank according to claim 1, characterized in that: The epoxy resin is a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin in a mass ratio of 3:
2.
3. The method for preparing the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank according to any one of claims 1 to 2, characterized in that: The preparation method of the modified reinforced polytetrafluoroethylene coating is as follows: polytetrafluoroethylene powder, self-healing modified filler, chelated grafted modified carbon fiber, epoxy resin and polyamide wax powder are mixed according to weight proportion, and stirred at 800-3000 rpm for 5-15 minutes to obtain the modified polytetrafluoroethylene coating.
4. The method for preparing the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank according to claim 1, characterized in that: The following steps are involved: Step 1: Cut the steel plate into the required shape and size, and then make the steel-lined tank body by bending and welding; Step 2: Pre-treat the inner wall of the steel-lined tank: Use ethanol to spray the inner surface of the steel plate, then blow dry it, and then spray mixed acid on the inner surface of the steel plate. The spraying amount is controlled to 20-200g / m 2 After spraying, let it stand for 2-15 minutes, then rinse with deionized water, repeat 2-8 times, and then blow dry to complete the pretreatment; Wherein, the mixed acid is a mixed solution of H2O2 and H2SO4, the mass fraction of H2O2 is 0.5-10%, and the mass fraction of H2SO4 is 5-45%; Step 3: spraying a modified reinforced polytetrafluoroethylene coating on the inner wall of the steel-lined tank body, and then curing it at 180-220° C. for 5-20 minutes to form a modified reinforced polytetrafluoroethylene coating with a thickness of 3-8 mm on the inner surface of the steel plate to obtain a storage tank blank; Step 4: Processing the storage tank blank into a storage tank product, that is, obtaining the corrosion-resistant and high-temperature-resistant steel-lined polytetrafluoroethylene storage tank.
5. A corrosion-resistant and high-temperature resistant steel-lined polytetrafluoroethylene storage tank, characterized in that: It is prepared by the method according to any one of claims 1 to 4.
Citation Information
Patent Citations
A steel-lined polytetrafluoroethylene high-temperature storage tank
CN114313670B
Thermal insulation energy-saving composite material and preparing method thereof
CN101186467A
Polyethylene powder coating suitable for pipeline and method
CN109679413A