A water injection point corrosion inhibitor and preparation method thereof

By using 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine ​​at the oil field water injection point to form a long helical chain-like inclusion structure, combined with biological regulators and inorganic salts, which solves the corrosion problems caused by high salinity, dissolved oxygen and sulfide ions at water injection points in oil fields, and achieves efficient corrosion inhibition and scale removal effects.

CN118496831BActive Publication Date: 2024-10-22KARAMAY HUAYOU FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973357.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Oilfield water injection points have corrosion problems caused by high salinity, dissolved oxygen and sulfide ions. Existing chemicals use large amounts and are not effective, making it difficult to effectively inhibit scaling and corrosion.

Method used

A long spiral chain formed by 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine ​​through disulfide bonds is used, combined with biological regulators and inorganic salts. Microwave heating and constant temperature treatment, adding triethylsilane and p-bromomethylbenzoic acid to form a corrosion inhibitor with a chain inclusion structure, using covalent bonds, hydrogen bonds and hydrophobic interactions to form a stable structure, slowly releasing biological regulators to Inhibit corrosion.

Benefits of technology

It significantly reduces the corrosion rate at the water injection point, improves the scale removal and corrosion inhibition effect, achieves good scaling and corrosion prevention effects, and is administered at a lower dose to extend the service life of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of chemical corrosion protection, and specifically relates to a water injection point corrosion inhibitor and a preparation method thereof. The method comprises: 1) taking raw materials and solvents for thermal reaction, dripping acid solution, filtering, washing, and drying to obtain a precipitate, adding a silane compound and an organic solvent to mix evenly, and purifying and freeze-drying to obtain a substrate after removing the solvent by rotary evaporation; 2) taking a carboxylic acid compound and an acyclic polyamine to condense to obtain an intermediate, mixing the substrate, a hydrocarbon halide, and the intermediate evenly, and subjecting the substrate to constant temperature treatment and filtering to obtain a modified substrate; 3) taking a biological regulator and an inorganic salt to mix evenly, and cultivating to obtain a bacterial liquid, and mixing the modified substrate and the bacterial liquid evenly to obtain a corrosion inhibitor. The inhibitor of the present invention can achieve a good effect of preventing scaling and corrosion at the water injection point by being added at a relatively low dosage, significantly reducing the corrosion rate of the water injection point, extending the service life of the equipment, and having a good descaling and corrosion inhibition effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical anticorrosion, and in particular relates to a water injection point corrosion inhibitor and a preparation method thereof. Background Art

[0002] At present, most oil fields in my country have entered the stage of water injection and exploitation. The injected water mainly comes from the produced water of the oil field. After treatment, the injected water is reinjected into the formation to meet the production needs of the oil field. However, the produced water of the oil field has a high water temperature and high mineralization. It is rich in metal elements such as magnesium, barium, calcium and their scaling products, and also produces highly corrosive gases such as hydrogen sulfide and oxygen. The produced water of the oil field is rich in dissolved oxygen, and the system is acidic. At the same time, the high content of sulfur ions will aggravate the corrosion phenomenon. Dissolved oxygen and sulfur ions are the main causes of metal corrosion. Moreover, dissolved oxygen and sulfur ions react slowly and can coexist for a long time. These factors can easily lead to scaling and corrosion of water treatment equipment, water injection pumps and other equipment, resulting in increased pressure of reinjection water and reduced water injection efficiency. If the water pipeline is perforated, the oil field will not be able to produce normally.

[0003] In order to solve the scaling and corrosion problems, chemicals are usually added to the produced water treatment system. However, the current dosage of chemicals used in oilfield produced water treatment systems is relatively large, generally greater than 50 mg / L. Summary of the invention

[0004] Based on the above content, in order to solve the problem that the economic benefits of the chemicals added to the water injection points in oil fields are poor and the corrosion inhibition effect is not ideal, the present invention proposes a water injection point corrosion inhibitor and a preparation method thereof.

[0005] The purpose of the present invention is to provide a water injection point corrosion inhibitor to reduce the corrosion rate of the water injection point, improve the descaling and corrosion inhibition effect of the corrosion inhibitor, and ensure that a small amount of injection can achieve a good effect of preventing scaling and corrosion at the water injection point.

[0006] To achieve the above objectives, the present invention adopts the following technical solutions.

[0007] A method for preparing a water injection point corrosion inhibitor comprises: 1) taking raw materials and solvents for thermal reaction, dropping acid solution, filtering, washing and drying to obtain a precipitate, adding a silane compound and an organic solvent to mix evenly, rotary evaporating to remove the solvent, purifying, and freeze-drying to obtain a base material.

[0008] 2) A carboxylic acid compound and an acyclic polyamine are condensed to obtain an intermediate, and the substrate, a hydrocarbon halide and the intermediate are evenly mixed, and the modified substrate is obtained by constant temperature treatment and filtration.

[0009] 3) Mix the bioregulator and the inorganic salt evenly, cultivate a bacterial solution, and mix the modified substrate and the bacterial solution evenly to obtain a corrosion inhibitor; Step 1) The raw materials are 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine; the 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine ​​are prepared as raw materials in a mass ratio of 1:(2.6-2.8).

[0010] Preferably, the solvent is anhydrous DMF and triethylamine, and the amount thereof is 15-25 mL / g of raw material. Anhydrous DMF and triethylamine are prepared in a volume ratio of 1: (0.3-0.5).

[0011] Preferably, the thermal reaction in step 1) is carried out at 100-105°C with a microwave at 700-1200 W for 5-10 min.

[0012] Preferably, the acid solution in step 1) is hydrochloric acid with a concentration of 1 to 1.5 mol / L, and its dosage is 0.5 to 0.8 mL / g raw material.

[0013] Step 1) The silane compound is triethylsilane, and 4 to 6 mL of the silane compound is added per gram of precipitate.

[0014] Step 1) The organic solvent is trifluoroacetic acid and dichloromethane. 30-40 mL of solvent is added per gram of precipitate. The trifluoroacetic acid and dichloromethane are prepared in a volume ratio of 1: (0.8-1).

[0015] Preferably, the purification process after the solvent removal by rotary evaporation in step 1) is: after the solid is precipitated by rotary evaporation, the solid is dissolved in acetonitrile and purified by C18 reverse phase preparative column.

[0016] The freeze drying in step 1) is carried out at a constant temperature of -10 to 0°C for 2 to 4 hours.

[0017] Preferably, in step 2), the carboxylic acid compound is p-bromomethylbenzoic acid, and 1.5 to 2 g of the carboxylic acid compound is taken per gram of substrate.

[0018] Step 2) The acyclic polyamine is propylenediamine, and 0.35-0.4 mL of the acyclic polyamine is taken per gram of substrate.

[0019] Step 2) The condensation is carried out at a constant temperature of 140-160°C for 3-4 hours.

[0020] Preferably, in step 2), the hydrocarbon halide is 4-bromo-2-nitrotrifluoromethoxybenzene, and 0.05-0.15 mL of the hydrocarbon halide is added per gram of substrate.

[0021] Step 2) The constant temperature treatment is carried out at 60-80°C for 25-35 min.

[0022] Preferably, in step 3), the bioregulator is a mixed solution of CPB carboxypeptidase B and JSHD-4 Geobacillus, wherein the concentration of CPB carboxypeptidase B is 0.5-2.0 mg / mL, and the spore concentration of JSHD-4 Geobacillus is 1.5×10 8 ~2×10 11 cfu / mL.

[0023] Step 3) The inorganic salt is sodium dihydrogen phosphate, and its dosage is 1-3 mg / mL bioregulator.

[0024] Step 3) After the mixed solution is prepared, it is cultured for 5 to 7 days.

[0025] Preferably, the amount of the bioregulator in step 3) is 3-8 mL / g modified substrate.

[0026] The water injection pitting corrosion inhibitor prepared by the above method has the effect of inhibiting water injection pitting corrosion.

[0027] The oilfield reinjection water contains trace amounts of elemental sulfur, free sulfur, and organic sulfur compounds, such as pentan-2-thiol, methyl sulfide, ethyl cyclohexyl sulfide, and phenylthiophene, as well as a large amount of dissolved oxygen. The suspended solids content in the oilfield produced water exceeds the standard, the total mineralization and dissolved oxygen mass concentration are high, and the composition is relatively complex. In an environment with a high dissolved oxygen mass concentration, although dissolved oxygen will inhibit the activity of anaerobic bacteria, it will also oxidize and decompose the polymer in the corrosion inhibitor. In order to avoid severe metal corrosion caused by a large amount of dissolved oxygen and sulfide ions, the present invention combines fungi and chain inclusion structures to prepare a water injection point corrosion inhibitor. The chain inclusion structure prepared by the present invention forms a stable structure through covalent bonds, hydrogen bonds, aromatic structure interactions, hydrophobic effects, etc., and forms a composite biological regulator in a spirally wound manner until the long chain is cut into broken short peptides and amino acids.

[0028] However, the strength of the bond is related to the relative position between the functional groups, and the position of the key amino acid in the long chain is difficult to adjust. To solve this problem, the present invention uses the electron-deficient aromatic compound 1,4,5,8-naphthalenetetracarboxylic anhydride to connect the aliphatic amino acid (S)-trityl-L-cysteine, and forms a helical long chain through disulfide bonds and thiol exchange reactions. There are strong intermolecular π-π interactions on the helical long chain. Compared with the (S)-trityl-L-cysteine ​​monomer, the helical structure of the product tends to be stable, and the hydrolysis resistance of the material is significantly improved. Among them, due to the dynamic characteristics of the disulfide bond, the helical long chain tends to be rigid. In an endogenous reducing environment, the disulfide bond is stimulated to break, releasing the endogenous biological regulator. If 4-4'-dibromomethylbiphenyl is used to connect the thiol group, the resulting product has a shorter connection bond. Although the material has a strong rigid structure and excellent hydrophobicity, 4-4'-dibromomethylbiphenyl forms a hydrophobic interaction force with the hydrophobic amino acid, the product yield is low, and the material hydrolysis resistance is significantly reduced. The release rate of the bioregulator is fast, and the corrosion inhibition effect is good in a short time. Compared with the product of the present invention, the product has a small rigid plane and does not form a gap structure surrounded by cations, and the adsorption effect on divalent metal ions is reduced. If a polypeptide aromatic ring amino acid, such as (S)-2-amino-3-(4-hydroxyphenyl) propionic acid, is used instead, the active molecule is on the opposite side of the helix of the aromatic amino acid. However, the coiled coil mainly relies on the combined action of hydrophobic interaction and electrostatic attraction. It is difficult to form π-π interaction due to the long distance. In the absence of non-covalent bond force, the molecular chain has almost no helical structure and poor hydrolysis resistance. Most importantly, the substrate prepared by the present invention exhibits excellent electron-deficient properties, while the material prepared from this aromatic amino acid exhibits obvious electron-rich properties. Its inclusion space volume is small, and it is obvious that the amount of bioregulatory agents that can be released after being put into use is small, resulting in a poor corrosion inhibition effect.

[0029] After microwave heating and hydrochloric acid treatment, the present invention adds triethylsilane to modify the surface of the precipitate, and the steric protective agent can provide a good support for the substrate and improve its structural stability. At the same time, triethylsilane has a certain effect on bacterial adhesion, and silanization of the precipitate can improve bacterial adhesion, which is conducive to the adhesion of microorganisms such as thiobacillus contained in the produced water itself, and is conducive to the formation of larger flocs after the competition is completed. It should be noted that trifluoroacetic acid is used as a solvent, and dichloromethane needs to be added, otherwise trifluoroacetic acid is difficult to remove by rotary evaporation. After purification, it can be measured that the target product yield is high.

[0030] Further, the present invention uses p-bromomethylbenzoic acid and propylene diamine to condense to obtain an intermediate of a reactive halogen group ·Br, which is used as a connecting bond, which is beneficial to improve the stability of the α-helical secondary structure. The length of the connecting bond has a certain influence on the secondary structure of the polypeptide. After SPR characterization, it is found that the short bond length is conducive to the dynamic binding and dissociation of the helical structure, and enhances the ability of binding peptides and inclusion bioregulators. After the connecting bond is bound, the product has rigidity and will not twist and fold, and its action interface is protected. At the same time, the product has little effect on the specific effects of releasing bioregulators and adsorbing microorganisms. If the rigid connecting bond length is extended, its structure is obviously not an α-helix. Although this helical form is more typical, the extension of the bond length does not increase the helical tendency of the molecule, and it also causes more molecules to be disordered. Obviously, if the intermediate is prepared with an alkane long chain, the connecting bond is too flexible and cannot provide sufficient support for the molecule, which will cause molecular deformation, that is, the stability of the molecular spatial structure decreases, thereby causing the corrosion inhibitor to have a poor complexing ability for heavy metal ions.

[0031] Based on the main body of the substrate, the present invention has a high molecular helicity and connects 4-bromo-2-nitrotrifluoromethoxybenzene to the outside of the substrate. This crown ether fluoride provides a complexing center for the substrate and also provides a trifluoromethyl peptidomimetic structure. Bacteria can strongly hydrophobically bind to the trifluoromethyl group. The two modified helical molecules can combine to form a cavity ring that can encapsulate small mineral molecules. Depending on the size of the ring, it can preferentially bind to Al 3+ , Fe 3+ , Fe 2+ , Ca 2+ Mg 2+ The metal cations form stable complexes with remarkable selectivity. However, 4-bromo-2-nitrotrifluoromethoxybenzene makes the molecule lipophilic. In this case, a large amount of 4-bromo-2-nitrotrifluoromethoxybenzene is used to modify the molecule. When the molecules are intercalated, free F - Competitive complexation occurs with bacteria, thereby inhibiting the bacterial agent. Therefore, the present invention regulates the amount of 4-bromo-2-nitrotrifluoromethoxybenzene.

[0032] At the same time, the produced water of the oil field contains a large number of anaerobic bacteria, which will decompose the polymer, seriously reduce the viscosity of the polymer, and lead to a decrease in the effect of inhibitor flooding. Generally, the produced water is treated by aeration, but the polymer molecular chain is easy to break, and the higher the oxygen content in the water sample, the easier it is to cause pipeline corrosion. Among them, the carbon source combines with the sulfate ions in the water sample, and after catalysis by sulfate-reducing bacteria, a large amount of hydrogen sulfide, carbon dioxide, and water are produced, which cause corrosion and promote the growth and reproduction of other bacteria, thereby causing pipeline corrosion and scaling. The technical solution of the present invention uses sodium dihydrogen phosphate as a nutrient base, uses denitrifying anaerobic bacteria to cultivate sulfur removal bacteria, and CPB carboxypeptidase B and JSHD-4 Bacillus (purchased from the cooperative unit, Xinjiang Petroleum Branch of China Petrochemical Corporation) are compounded to enable JSHD-4 Bacillus to grow in an environment with an oxygen concentration of less than 0.1 mg / mL, and can become spores in an unsuitable environment and still survive. At the standard reinjection water temperature (45-55 ℃), the bacterial agent is tolerant and grows well. The temperature effectively distributes the ecological sites of the bacterial agent, ensuring that the target bacterial agent grows and reproduces under its own suitable temperature conditions, forming a dominant bacterial community and competitively inhibiting the reproduction of sulfate-reducing bacteria. After 5-7 days of cultivation experiments, it was found that the sulfate-reducing bacteria removal rate of the compound biological regulator was higher than that of the uncompounded single bacterial agent used alone. At a certain ratio, the synergistic inhibition of sulfate-reducing bacteria is the best.

[0033] When the corrosion inhibitor is added to the produced water of the oil field, the disulfide bond breaks, and the biological regulator composed of CPB carboxypeptidase B and JSHD-4 Geobacillus is continuously and slowly released, so that the injected water maintains a low dissolved oxygen state for a long time, effectively improving its corrosion inhibition effect. When used, if it is made into a colloid, the surface adsorption energy generated by the colloid is also greater due to its larger surface area, and the adsorption performance of the colloid is stronger. During the adsorption process, the colloid adsorbs a part of Mg 2+ , Ca 2+ The same amount of cations are released at the same time, so that the ionic compounds are adsorbed on the surface of the same charge. At the same time, the stable colloidal ions condense to form flocs with small particle size, and the chain polypeptide bridges these small flocs to form large flocs, which accelerates sedimentation and has a better descaling effect. In addition, the corrosion inhibition effect increases with the increase of the dosage of the corrosion inhibitor. When the dosage increases to a certain value, the corrosion inhibition effect of the corrosion inhibitor slows down and tends to balance. The comprehensive economic benefits determine the dosage of the corrosion inhibitor of the present invention.

[0034] The beneficial effects of the present invention are as follows: the corrosion inhibitor of the present invention is added at a relatively low dosage, which can achieve a good effect of preventing scaling and corrosion at the water injection point, significantly reduce the corrosion rate of the water injection point, extend the service life of the equipment, have a good descaling and corrosion inhibition effect, and can obtain a relatively clear oilfield produced water sample through sedimentation and filtration. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0036] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0037] Example 1: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, removing the solvent by rotary evaporation, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column and keeping it at -10 °C for 2 h to obtain a substrate.

[0038] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.05 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0039] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0040] The performance of the corrosion inhibitor prepared in this example was tested.

[0041] Take 45 ℃ oilfield produced water in a stainless steel kettle (the stainless steel kettle complies with the standard GB / T9711-2017), add 100 mg of the corrosion inhibitor prepared in this example per liter of oilfield produced water, and add it within 2 hours. After 10 days, the oilfield produced water samples and the oilfield produced water samples treated with the corrosion inhibitor of the present invention are characterized by suspended solid content, average particle size, ferrous content, sulfide content, sulfate-reducing bacteria concentration, average corrosion rate, and dissolved oxygen removal performance test.

[0042] The results are as follows.

[0043]

[0044] Since the corrosion inhibition effect increases with the increase of the dosage of the corrosion inhibitor, when the dosage increases to a certain value, the growth rate of the corrosion inhibition effect of the corrosion inhibitor slows down and tends to balance. The dosage of the corrosion inhibitor of the present invention is determined based on comprehensive economic benefits.

[0045] According to the results in the table, it can be seen that the suspended solid content is significantly reduced, forming a large volume of floccules, which can be removed by physical sedimentation. At the same time, the present invention puts in a corrosion inhibitor at an input amount of 20 mg / L, which is much lower than the commercially available corrosion inhibitors and has high economic benefits. Before treatment, the average corrosion rate of oil field produced water far exceeds the injection water standard (0.076 mm / a), the oxygen content is high, a large number of bacteria grow on the inner wall of the equipment, a large number of particles are suspended on the surface of the produced water, the mineralization exceeds 840 mg / mL, and the scaling is serious. After treatment, it can be observed with the naked eye that the dirt in the water sample is reduced. Analysis shows that the ferrous content, sulfide and hydrogen sulfide content are significantly reduced. The total sterilization rate of the corrosion inhibitor in this example is 96.0% (including the remaining native bacteria in addition to SRB), the corrosion inhibition rate is high, and the dissolved oxygen content in the reinjection water meets the requirements of SY / T5329-2012 "Water Quality Indicators and Analysis Methods for Injection Water in Clastic Reservoirs". It can be seen that the corrosion inhibitor in this example has a good corrosion inhibition effect and can be put into use.

[0046] After characterization of the enzyme cleavage sites, it can be known that only the amide bond on the carboxyl side is broken. The corrosion inhibitor in this example not only successfully releases the bioregulator, but also protects the active site of the electron-deficient structure. This analysis is consistent with the results in the table, indicating that the corrosion inhibitor in this example has strong anti-hydrolysis performance.

[0047] Example 2: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, removing the solvent by rotary evaporation, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column and keeping it at -10 °C for 2 h to obtain a substrate.

[0048] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0049] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0050] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0051]

[0052] According to the results in the table, more 4-bromo-2-nitrotrifluoromethoxybenzene was used in this case, and the suspended solids content was significantly reduced, indicating that 4-bromo-2-nitrotrifluoromethoxybenzene can provide complexing centers for the substrate, especially it can preferentially bind to Fe 3+ , Fe 2+ At the same time, the corrosion inhibitor in this example contains more trifluoromethyl peptidomimetic structures, and bacteria can have a strong hydrophobic binding with the trifluoromethyl group.

[0053] Example 3: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of precipitate and mixing evenly, removing the solvent by rotary evaporation, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10 °C, and keeping the temperature for 2 h to obtain a substrate.

[0054] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.15 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0055] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0056] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0057]

[0058] Since 4-bromo-2-nitrotrifluoromethoxybenzene makes the molecule lipophilic, a large amount of 4-bromo-2-nitrotrifluoromethoxybenzene is used to modify the molecule. When the molecules are interlaced, free F - Competitive complexation occurs with bacteria, thereby inhibiting the bioregulator, resulting in a slight decrease in the total sterilization rate. Therefore, regulating the amount of 4-bromo-2-nitrotrifluoromethoxybenzene in the present invention will have a significant impact on product performance.

[0059] Comparative Example 1: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 36 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100°C, dropping 18 mL of 1.5 mol / L hydrochloric acid, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, rotary evaporation to remove the solvent, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10°C, and keeping the temperature for 2 h to obtain a substrate.

[0060] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0061] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0062] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0063]

[0064] According to the results in the table, in order to ensure that a strongly bonded chain inclusion structure is obtained, the present invention uses an electron-deficient aromatic compound 1,4,5,8-naphthalenetetracarboxylic anhydride to connect the aliphatic amino acid (S)-trityl-L-cysteine, and forms a long spiral chain through disulfide bonds and sulfhydryl exchange reactions. There is a strong intermolecular π-π interaction on the long spiral chain. Compared with Example 2, the spiral structure obtained by using (S)-trityl-L-cysteine ​​monomer as a raw material in this example is not stable enough, the material has poor hydrolysis resistance, and it quickly complexes metal ions, inhibits bacterial growth, and includes small molecules in water, but its long-term effect is poor, and the flocs are broken and dispersed.

[0065] Comparative Example 2: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 4-4'-dibromomethylbiphenyl, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100°C, dropping 18 mL of 1.5 mol / L hydrochloric acid, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, rotary evaporation to remove the solvent, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10°C, and keeping the temperature for 2 h to obtain a substrate.

[0066] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0067] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0068] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0069]

[0070] According to the results in the table, this example uses 4-4'-dibromomethylbiphenyl to connect the thiol group, and the resulting product has a short connection bond. Although the material has a strong rigid structure and excellent hydrophobicity, 4-4'-dibromomethylbiphenyl forms a hydrophobic interaction force with the hydrophobic amino acid, the product yield is low, and the material's hydrolysis resistance is significantly reduced. The bioregulator release rate is fast, and the corrosion inhibition effect is good in a short time. Compared with the product of the present invention, the product has a small rigid plane, does not form a gap structure surrounded by cations, and the adsorption effect on divalent metal ions is reduced.

[0071] Comparative Example 3: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-2-amino-3-(4-hydroxyphenyl)propionic acid, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, rotary evaporation to remove the solvent, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10 °C, and keeping the temperature for 2 h to obtain a substrate.

[0072] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0073] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0074] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0075]

[0076] According to the results in the table, this example uses a polypeptide aromatic ring amino acid (S)-2-amino-3-(4-hydroxyphenyl) propionic acid for preparation, and the active molecule is on the opposite side of the helix of the aromatic amino acid. However, the coiled coil mainly relies on the combined effects of hydrophobic interaction and electrostatic attraction. Due to the long distance between them, it is difficult to form π-π interactions. In the absence of non-covalent bond forces, the molecular chain has almost no helical structure and poor hydrolysis resistance. Most importantly, the substrate prepared by the present invention shows excellent electron deficiency, while the material prepared by this aromatic amino acid shows obvious electron richness, and its inclusion space volume is small. Obviously, the amount of biological regulator that can be released after being put into use is small, which leads to poor corrosion inhibition effect.

[0077] Comparative Example 4: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100°C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, dissolving the precipitate in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10°C, and keeping the temperature for 2 h to obtain a substrate.

[0078] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0079] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0080] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0081]

[0082] According to the results in the table, the product prepared from 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine ​​was not structurally reinforced in this example, and the structural stability of the substrate deteriorated. At the same time, the bacterial adhesion of the corrosion inhibitor deteriorated, and the produced water still contained a large number of microorganisms such as Thiobacillus. After the competition was completed, the flocs had a small particle size and were dispersed in a broken state.

[0083] Comparative Example 5: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of the precipitate and mixing evenly, rotary evaporation to remove the solvent, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10 °C, and keeping the temperature for 2 h to obtain a substrate.

[0084] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of 1,5-diaminopentane per gram of substrate, keep the mixture at 150 °C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70 °C for 35 min, and then filter to obtain a modified substrate.

[0085] 3) Prepare the bioregulator at a ratio of 3 mL / g modified substrate, and the spore concentration of JSHD-4 Bacillus in the bioregulator is 2×10 11 cfu / mL, CPB carboxypeptidase B concentration is 1.0 mg / mL, 1 mg of sodium dihydrogen phosphate is added to each milliliter of biological regulator and mixed evenly, and the bacterial solution is obtained by incubating for 7 days. The modified substrate and the bacterial solution are mixed evenly to obtain the corrosion inhibitor.

[0086] The corrosion inhibitor prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0087]

[0088] According to the results in the table, this example uses p-bromomethylbenzoic acid and 1,5-diaminopentane to condense to obtain an intermediate with a reactive halogen group ·Br. This intermediate acts as a connecting bond, but the rigid connecting bond length is extended, and its structure is obviously not an α-helix. Although this helical form is more typical, the extension of the bond length does not increase the helical tendency of the molecule, but also causes more molecules to bind disorderly. The dynamic binding-dissociation process of the helical structure is affected to a certain extent, and the effect of the inclusion bioregulator is poor, and it will lose its effectiveness too quickly after being administered.

[0089] If the chain length of acyclic polyamine is increased, the connecting bonds are too flexible to provide sufficient support for the molecules, which will cause molecular deformation, that is, the stability of the molecular spatial structure will decrease, and the ability of corrosion inhibitors to complex metal ions will also deteriorate.

[0090] Comparative Example 6: A method for preparing a water injection point corrosion inhibitor, the method comprising: 1) taking 10 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 26 g of (S)-trityl-L-cysteine, 15 mL of anhydrous DMF, and 5 mL of triethylamine, treating them with a microwave at 800 W for 10 min at 100 °C, adding 18 mL of 1.5 mol / L hydrochloric acid dropwise, filtering, washing, and drying to obtain a precipitate, adding 4 mL of triethylsilane, 17 mL of trifluoroacetic acid, and 13.6 mL of dichloromethane per gram of precipitate and mixing evenly, rotary evaporation to remove the solvent, dissolving the solid obtained by rotary evaporation in acetonitrile, purifying it with a C18 reverse phase preparative column, collecting the liquid phase purified by the C18 reverse phase preparative column at -10 °C, and keeping the temperature for 2 h to obtain a substrate.

[0091] 2) Take 1.5 g of p-bromomethylbenzoic acid and 0.35 mL of propylenediamine per gram of substrate, keep the mixture at 150°C for 3.5 h to obtain an intermediate, mix the substrate and the intermediate evenly, add 0.11 mL of 4-bromo-2-nitrotrifluoromethoxybenzene per gram of substrate and mix evenly, keep the mixture at 70°C for 35 min, and then filter to obtain a modified substrate.

[0092] 3) Prepare 3 mL of spores with a concentration of 2×10 11 cfu / mL of JSHD-4 Geobacillus, 1 mg of sodium dihydrogen phosphate was added per milliliter of bacterial agent and mixed evenly, and the bacterial solution was obtained by culturing for 7 days. The modified substrate and the bacterial solution were mixed evenly to obtain a corrosion inhibitor.

[0093] The corrosion inhibitor prepared in this example (6-1) was subjected to the same performance test as in Example 1, and the results are as follows.

[0094]

[0095] Only step 3) is adjusted as follows: prepare 3 mL of 0.5 mg / mL CPB carboxypeptidase B as an enzyme per gram of modified substrate, add 1 mg of sodium dihydrogen phosphate per milliliter of enzyme and mix evenly, let stand for 7 days to obtain an enzyme solution, and mix the modified substrate and the enzyme solution evenly to obtain a corrosion inhibitor.

[0096] The corrosion inhibitor prepared in this example (6-2) was subjected to the same performance test as in Example 1, and the results are as follows.

[0097]

[0098] According to the results in the tables of Example 6-1 and Example 6-2, the effect of corrosion inhibitors prepared by using only bacterial agents or enzyme agents is significantly reduced. Although JSHD-4 Geobacillus can grow in an environment with an oxygen concentration lower than 0.1 mg / mL, can become spores in an unsuitable environment, can still survive, and tolerate the standard reinjection water temperature (45-55 ℃), different temperatures have a certain impact on the ecological site of the bacterial agent. Due to the lack of competitive inhibition caused by another enzyme agent, the effect of inhibiting sulfate-reducing bacteria alone is poor.

Claims

1. A method for preparing a water injection point corrosion inhibitor, characterized in that: The method comprises: 1) Take the raw materials and solvent for thermal reaction, add acid solution, filter, wash and dry to obtain a precipitate, add a silane compound and an organic solvent to mix evenly, remove the solvent by rotary evaporation, purify and freeze-dry to obtain a substrate; 2) Carboxylic acid compounds and acyclic polyamines are condensed to obtain an intermediate, and the substrate, hydrocarbon halide and the intermediate are uniformly mixed, and the modified substrate is obtained by constant temperature treatment and filtration; 3) Mix the bioregulator and inorganic salt evenly, cultivate the bacterial solution, and mix the modified substrate and the bacterial solution evenly to obtain the corrosion inhibitor; Step 1) The raw materials are 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine; The 1,4,5,8-naphthalenetetracarboxylic anhydride and (S)-trityl-L-cysteine ​​are prepared as raw materials in a mass ratio of 1:(2.6-2.8); Step 1) The solvent is anhydrous DMF and triethylamine, and the amount thereof is 15-25 mL / g of raw material. Anhydrous DMF and triethylamine are prepared in a volume ratio of 1: (0.3-0.5); Step 1) The thermal reaction is carried out at 100-105°C and 700-1200 W microwave for 5-10 min; Step 1) The acid solution is hydrochloric acid with a concentration of 1 to 1.5 mol / L, and its dosage is 0.5 to 0.8 mL / g raw material; Step 1) the silane compound is triethylsilane, and 4 to 6 mL of the silane compound is added per gram of precipitate; Step 1) The organic solvent is trifluoroacetic acid and dichloromethane, and 30-40 mL of the solvent is added per gram of precipitate, and the trifluoroacetic acid and dichloromethane are prepared in a volume ratio of 1: (0.8-1); Step 2) the carboxylic acid compound is p-bromomethylbenzoic acid, and 1.5 to 2 g of the carboxylic acid compound is taken per gram of substrate; Step 2) the acyclic polyamine is propylenediamine, and 0.35-0.4 mL of acyclic polyamine is taken per gram of substrate; Step 2) the condensation is carried out at 140-160°C for 3-4 hours; Step 2) the hydrocarbon halide is 4-bromo-2-nitrotrifluoromethoxybenzene, and 0.05-0.15 mL of the hydrocarbon halide is added per gram of substrate; Step 2) the constant temperature treatment is carried out at 60 to 80°C for 25 to 35 minutes; Step 3) The bioregulator is a mixed solution of CPB carboxypeptidase B and JSHD-4 Geobacillus, wherein the concentration of CPB carboxypeptidase B is 0.5-2.0 mg / mL, and the spore concentration of JSHD-4 Geobacillus is 1.5×10 8 ~2×10 11 cfu / mL; Step 3) the inorganic salt is sodium dihydrogen phosphate, and the amount thereof is 1 to 3 mg / mL bioregulator; Step 3) After the mixed solution is prepared, it is cultured for 5 to 7 days.

2. The method for preparing a water injection point corrosion inhibitor according to claim 1, characterized in that: Step 1) The purification process after the solvent is removed by rotary evaporation is as follows: After the solid was precipitated by rotary evaporation, it was dissolved in acetonitrile and purified by C18 reverse phase preparative column; The freeze drying in step 1) is carried out at a constant temperature of -10 to 0°C for 2 to 4 hours.

3. The method for preparing a water injection point corrosion inhibitor according to claim 1, characterized in that: Step 3) The amount of the bioregulator is 3-8 mL / g modified substrate.

4. A water injection point corrosion inhibitor prepared by the method according to any one of claims 1 to 3.