A kind of splitting knife coating and preparation method thereof

The microcrystalline chromium oxide coating is formed on the surface of the splitter by radio frequency magnetron sputtering, which solves the problems of increased surface roughness and insufficient binding force caused by CVD method, significantly extends the service life of the splitter and improves the wire bonding process. stability.

CN118497675BActive Publication Date: 2024-11-15苏州芯合半导体材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979656.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

When the CVD method is used to make chromium oxide coatings in the prior art, the surface roughness of the splitter knife increases, the bonding force between the coating and the substrate is weak, which affects the service life of the splitter knife.

Method used

RF magnetron sputtering method is used to form a chromium oxide coating with a microcrystalline structure on the surface of the splitter base, and the surface roughness is reduced and the binding force is improved through cleaning and pretreatment steps.

Benefits of technology

It significantly reduces the roughness of the surface of the splitter coating, improves the bonding force between the coating and the splitter substrate, extends the service life of the splitter, and improves the stability and consistency during the wire bonding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497675B_ABST
    Figure CN118497675B_ABST
Patent Text Reader

Abstract

The invention provides a splitting knife coating and a preparation method thereof, comprising the following steps: S1 cleaning the surface of a splitting knife substrate; S2 pre-treating the splitting knife substrate after the cleaning; S3 forming a chromium element coating on the surface of the pre-treated splitting knife substrate; S4 using a radio frequency magnetron sputtering method to produce a chromium oxide coating with a microcrystalline structure on the chromium element coating to obtain the splitting knife coating; in this way, the roughness of the surface of the splitting knife coating is reduced, the bonding force between the coating and the splitting knife substrate is improved, and the service life of the splitting knife is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wedge coatings, and in particular to a wedge coating and a preparation method thereof. Background Art

[0002] During the bonding process, as the number of times the splitter is used to bond wires increases, dirt will accumulate on the surface of the ceramic splitter. This is mainly because during the bonding process, the splitter will come into contact with the frame, the chip substrate, and the wire for lead bonding. These materials are all made of metal, such as aluminum, silver, copper and other non-ferrous metals. During the bonding process, due to the energy of ultrasound, the surface of the splitter will rub against these metals, thereby accumulating metal dirt on the surface of the splitter. As the number of bonding increases, the accumulation will also increase, ultimately affecting the quality of the chip after bonding. At the same time, during the wire bonding process, due to the effect of ultrasound, there is high-frequency vibration and friction between the surface of the splitter and the wire frame, and its surface will gradually wear out (such as Figure 1 As shown in the figure), the original surface morphology and structure cannot be maintained, which affects the number of wire bonding times of the splitter. The life of the splitter is determined based on the maximum number of wire bonding times before the chip lead bonding fails.

[0003] The existing technology uses CVD (chemical vapor deposition) to make chromium oxide coating to solve the technical problem of gradual wear of the wedge during the wire bonding process. However, the chromium oxide produced by CVD tends to grow into a columnar crystal structure of {1,1,1} plane, resulting in the following technical problems in actual application:

[0004] The columnar crystal structure of the {1,1,1} plane means that the chromium oxide coating is composed of many columnar crystals perpendicular to the substrate. These crystals may form an uneven surface during the growth process because the growth rate and direction of the crystals may be inconsistent; due to the growth characteristics and possible unevenness of the columnar crystals, the coating surface will appear uneven, resulting in increased surface roughness of the splitter. This increase in roughness may affect the performance and life of the splitter. In the actual wire bonding process, the phenomenon of grain pulling out occurs, and the life improvement is not obvious.

[0005] The bond between the chromium oxide coating and the cutter substrate may be weak, especially at the grain boundaries or the interface between the grain and the substrate. This may be due to factors such as temperature gradients, stress distribution or material mismatch during the coating preparation process. During the wire bonding process, the cutter is subjected to mechanical stresses such as stretching, bending, etc. If the bond between the coating and the substrate is weak, these mechanical stresses may cause the grains to pull out of the substrate, affecting the performance and life of the cutter.

[0006] Although the CVD method can produce high-quality chromium oxide coatings, the columnar crystal structure in the coating may lead to defects or stress concentration points inside the coating. These defects or stress concentration points may become the starting point of coating failure, thereby reducing the service life of the splitting tool.

[0007] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application, nor does it necessarily provide technical guidance. In the absence of clear evidence that the above content has been disclosed before the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention

[0008] In order to solve the technical problems of the prior art of using CVD (chemical vapor deposition) to make chromium oxide coating to solve the problems of increased surface roughness of the splitting knife, weak bonding force between the coating and the substrate, and reduced service life of the splitting knife during the wire bonding process, the present invention proposes a splitting knife coating and a preparation method thereof, which reduces the roughness of the surface of the splitting knife coating, improves the bonding force between the coating and the splitting knife substrate, and thus improves the service life of the splitting knife.

[0009] In order to achieve the above object, the technical solution of the present invention is as follows:

[0010] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0011] S1 cleans the surface of the splitting cutter base;

[0012] S2 pre-treats the cleaned splitter substrate;

[0013] S3 forms a chromium coating on the surface of the pre-treated splitter substrate;

[0014] S4 uses radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a splitter coating.

[0015] The present invention provides a splitting knife coating and a preparation method thereof, which reduces the roughness of the splitting knife coating surface, improves the bonding force between the coating and the splitting knife substrate, and thus improves the service life of the splitting knife.

[0016] As a preferred technical solution, step S3 forms a chromium coating on the surface of the pretreated splitter substrate, which specifically includes the following steps:

[0017] S301 evacuates the cavity and heats the wedge substrate to above 500° C. to form a vacuum chamber;

[0018] S302 injects argon gas into the vacuum chamber;

[0019] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias on the chromium target. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating.

[0020] As a preferred technical solution, step S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating, which specifically includes the following steps:

[0021] S401 continues to evacuate the cavity, and at the same time heats the wedge substrate to above 500° C. to form a vacuum chamber;

[0022] S402 injects argon gas into the vacuum chamber;

[0023] S403 uses CrO3 target as cathode, attracting ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules detach from CrO3 target, and decompose under the heating temperature of splitter substrate to generate Cr2O3 and O2. RF power is used to form negative bias on CrO3 target, and at the same time, Cr2O3 is deposited on the surface of chromium coating to form chromium oxide coating under the micro-oxygen atmosphere formed by O2.

[0024] As a preferred technical solution, the air pressure in the vacuum chamber is ≤10 -5 Bar, the pressure flow rate of argon gas injected into the vacuum chamber is greater than 150ml / min, the negative bias voltage formed on the chromium target is -100~-200V, and the negative bias voltage formed on the CrO3 target is -100~-200V.

[0025] As a preferred technical solution, step S1 cleans the surface of the cleaver substrate, including the following steps:

[0026] S101 uses ultrasonic cleaning on the surface of the splitter substrate;

[0027] S102 performs high-pressure water washing on the surface of the splitter substrate after ultrasonic cleaning;

[0028] S103: soaking the surface of the splitting cutter base body after high-pressure water washing in a hydrocarbon cleaning agent;

[0029] S104 spin-drying the surface of the soaked splitter base;

[0030] S105 packages the dried splitting knife substrate in a dust-free environment.

[0031] As a preferred technical solution, the hydrocarbon cleaning agent includes the following components in weight percentage:

[0032] n-Dodecane or isododecane 60-80%;

[0033] 1,1,1,2,3-pentafluoropropane or 1,1,1,3,3-pentafluoropropane 10-20%;

[0034] Oxalic acid 10%~20%.

[0035] As a preferred technical solution, the temperature of the hydrocarbon cleaning agent is 60-80° C., and the immersion time of the hydrocarbon cleaning agent is more than 3 hours.

[0036] As a preferred technical solution, step S2 pre-treats the cleaned splitting knife, including the following steps:

[0037] After the cavity is evacuated in step S201, argon gas is introduced into the cavity;

[0038] After the chamber is further evacuated in step S202 and the DC power supply is turned on, the argon gas forms a plasma state, and the ionized argon ions bombard the surface of the splitting cutter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitting cutter substrate is ≤Ra0.05μm.

[0039] In another aspect, the present invention provides a wedge coating, which is prepared according to the preparation method of the wedge coating as described in any one of the above items.

[0040] As a preferred technical solution, it includes: a splitting knife substrate, the surface of which is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating presents a microcrystalline structure, and the thickness of the chromium oxide coating is 200nm to 1200nm.

[0041] The present invention provides a wedge coating and a preparation method thereof, which have the following beneficial effects:

[0042] 1) The roughness of the coating surface of the splitter is reduced, the bonding force between the coating and the splitter substrate is improved, and the service life of the splitter is increased;

[0043] 2) The present application purposefully selects to clean the surface of the splitting knife substrate in step S1 to prevent the dirt on the surface of the splitting knife substrate from affecting the effect of the coating, which not only avoids the reaction between some dirt and the coating, but also improves the bonding strength and thickness uniformity of the subsequent coating;

[0044] The present application purposefully selects to pre-treat the cleaned splitter substrate in step S2, which not only removes gas impurities adsorbed on the splitter surface, presents molecular-level cleanliness, reduces the roughness of the splitter substrate surface, but also helps to enhance the bonding strength of the chromium coating subsequently formed on its surface;

[0045] The present application intentionally selects to form a chromium coating on the surface of the splitting cutter substrate after pretreatment in step S3, which is conducive to improving the bonding strength of the chromium oxide coating formed on its surface later. Chromium is an inactive metal element, and its oxide (such as chromium trioxide) has high chemical stability. When the chromium element is deposited on the surface of the splitting cutter in the form of a coating, a stable chemical bond or interface reaction layer is formed between the coating and the substrate, which helps to enhance the bonding strength between the coating and the splitting cutter substrate;

[0046] The present application purposefully selects step S4 to produce a chromium oxide coating with a microcrystalline structure on the chromium element coating by a radio frequency magnetron sputtering method to obtain a splitter coating. The radio frequency magnetron sputtering method can achieve fine regulation of the deposition process by accurately controlling sputtering parameters (such as gas flow, gas pressure, substrate temperature, negative bias voltage, etc.). This high degree of controllability helps to obtain a uniform and dense chromium oxide coating, avoids the problems of uneven coating and columnar crystal structure that may occur in the CVD method, reduces the roughness of the splitter coating surface, and improves the bonding force between the coating and the splitter substrate, so that the service life of the splitter is improved;

[0047] The present application purposefully selects chromium coatings with excellent hardness, wear resistance, corrosion resistance and good electrical conductivity; forming a chromium coating on the cleaver substrate can significantly improve the service life and performance stability of the cleaver, and at the same time, the chromium coating can also serve as the bottom layer of the subsequent chromium oxide coating to improve the bonding strength and overall performance between the chromium oxide coating and the substrate;

[0048] The present application purposefully selects chromium oxide coatings for their excellent hardness, wear resistance, corrosion resistance, and optical properties, etc. The chromium oxide coatings prepared by radio frequency magnetron sputtering methods can further improve these properties and meet the needs of specific applications;

[0049] The present application purposefully selects the chromium oxide coating to have a microcrystalline structure. The microcrystalline structure makes the surface of the chromium oxide coating denser, reduces the contact area between the corrosive medium and the substrate, and thus improves the corrosion resistance of the coating. The chromium oxide coating with a microcrystalline structure has high hardness and can effectively resist wear and scratches from external forces. This property enables the coating to maintain good performance for a long time in a friction and wear environment, which is better reflected in the microcrystalline structure, so that the coating has a better protective effect in a high-temperature oxidation environment. The chromium oxide coating with a microcrystalline structure has a stronger interface bonding force with the substrate, which can effectively prevent the coating from falling off or peeling off when subjected to external forces.

[0050] 3) RF magnetron sputtering mainly relies on the bombardment of high-energy argon ions on the target material, so that the target molecules or atoms are detached and deposited on the substrate; this is a physical process, which is different from the chemical vapor reaction process of the CVD method; the physical deposition process is easier to control the growth morphology and structure of the coating, reducing the possibility of forming a columnar crystal structure;

[0051] During the RF magnetron sputtering process, the negative bias voltage formed on the target helps to attract ionized argon ions and accelerate their bombardment of the target, thereby increasing the sputtering yield of the target; at the same time, in the micro-oxygen atmosphere formed by O2, CrO3 molecules decompose on the heated substrate to generate Cr2O3, which can be quickly deposited on the substrate surface to form a uniform chromium oxide coating. This micro-oxygen atmosphere and the control of substrate temperature help to inhibit the growth of columnar crystals; at the same time, the micro-oxygen atmosphere avoids the appearance of oxygen vacancies in the chromium oxide coating to affect the density, thereby obtaining a uniform and dense chromium oxide coating.

[0052] 4) The negative bias voltage formed on the CrO3 target will change the speed and angle of chromium oxide atoms entering the surface of the splitter. The negative bias voltage formed on the CrO3 target using a radio frequency power supply will directly affect the surface roughness and grain size of the chromium oxide coating. The present application purposefully selects a negative bias voltage of -100 to -200 V formed on the CrO3 target using a radio frequency power supply to effectively improve the roughness of the splitter surface.

[0053] 5) The present application purposefully selects hydrocarbon cleaning agents, and the hydrocarbon cleaning agent formula purposefully selects the following components in weight percentage: 60-80% n-dodecane or isododecane; 10-20% 1,1,1,2,3-pentafluoropropane or 1,1,1,3,3-pentafluoropropane; 10%-20% oxalic acid. The hydrocarbon cleaning agent formula selects the above components to be compounded, which can dissolve many substances, remove grease, dust and other stains through strong dissolving action, has strong activity and inertness, and forms stable compounds with other elements, thereby better exerting the role of the hydrocarbon cleaning agent, and for metal-type dirt, generates new substances through chemical reactions to achieve the purpose of removing metal dirt.

[0054] 6) After the chamber is further evacuated, the DC power supply is turned on, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate, which removes gas impurities adsorbed on the surface of the splitter, presenting molecular-level cleanliness, which is beneficial to the bonding strength of the subsequent chromium coating. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is ≤Ra0.05μm, which is further beneficial to the bonding strength of the subsequent chromium coating;

[0055] 7) The present application purposefully selects the thickness of the chromium oxide coating to be 200nm to 1200nm, thereby improving the bonding strength of the wedge coating and also improving the service life of the wedge coating;

[0056] Due to the increase in the service life of the splitting knife coating, the alarm rate of the product in the actual wire welding process is reduced. At the same time, the morphological characteristics of the first and second welding points of the product are maintained for a longer time, so the quality is more stable and the consistency is better. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 SEM image of the surface of the wedge substrate provided as background technology;

[0058] Figure 2 The SEM image of the surface of the splitting cutter substrate in step S1 provided by the present invention;

[0059] Figure 3 The XRD pattern of the chromium oxide coating provided in Example 1 of the present invention;

[0060] Figure 4 SEM image of chromium oxide coating produced by CVD (chemical vapor deposition) method provided as background technology;

[0061] Figure 5 This is a SEM image of a chromium oxide coating produced by the radio frequency magnetron sputtering method provided in Example 1 of the present invention;

[0062] Figure 6 A schematic diagram of a flattened standard sample block in a thickness test step of a wedge anti-fouling coating is provided for the present invention. DETAILED DESCRIPTION

[0063] The preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0064] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0065] S1 cleans the surface of the splitting cutter base;

[0066] S2 pre-treats the cleaned splitter substrate;

[0067] S3 forms a chromium coating on the surface of the pre-treated splitter substrate;

[0068] S4 uses radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a splitter coating.

[0069] The present invention provides a method for preparing a splitting knife coating, which reduces the roughness of the surface of the splitting knife coating, improves the bonding force between the coating and the splitting knife substrate, and thus improves the service life of the splitting knife.

[0070] The present application purposefully selects step S1 to clean the surface of the splitting knife substrate to prevent dirt on the surface of the splitting knife substrate from affecting the effect of the coating, which not only avoids the reaction between some dirt and the coating, but also improves the bonding strength and thickness uniformity of the subsequent coating;

[0071] The present application purposefully selects to pre-treat the cleaned splitter substrate in step S2, which not only removes gas impurities adsorbed on the splitter surface, presents molecular-level cleanliness, reduces the roughness of the splitter substrate surface, but also helps to enhance the bonding strength of the chromium coating subsequently formed on its surface;

[0072] The present application intentionally selects to form a chromium coating on the surface of the pre-treated splitter substrate in step S3, which is beneficial to improve the bonding strength of the chromium oxide coating formed on its surface later;

[0073] The present application purposefully selects step S4 to produce a chromium oxide coating with a microcrystalline structure on the chromium element coating by a radio frequency magnetron sputtering method to obtain a splitter coating. The radio frequency magnetron sputtering method can achieve fine regulation of the deposition process by accurately controlling sputtering parameters (such as gas flow, gas pressure, substrate temperature, negative bias voltage, etc.). This high degree of controllability helps to obtain a uniform and dense chromium oxide coating, avoids the problems of uneven coating and columnar crystal structure that may occur in the CVD method, reduces the roughness of the splitter coating surface, and improves the bonding force between the coating and the splitter substrate, so that the service life of the splitter is improved;

[0074] The present application purposefully selects chromium coatings with excellent hardness, wear resistance, corrosion resistance and good electrical conductivity; forming a chromium coating on the cleaver substrate can significantly improve the service life and performance stability of the cleaver, and at the same time, the chromium coating can also serve as the bottom layer of the subsequent chromium oxide coating to improve the bonding strength and overall performance between the chromium oxide coating and the substrate;

[0075] The present application purposefully selects chromium oxide coatings for their excellent hardness, wear resistance, corrosion resistance, and optical properties, etc. The chromium oxide coatings prepared by radio frequency magnetron sputtering methods can further improve these properties and meet the needs of specific applications;

[0076] The present application purposefully selects the chromium oxide coating to have a microcrystalline structure. The microcrystalline structure makes the surface of the chromium oxide coating denser, reduces the contact area between the corrosive medium and the substrate, and thus improves the corrosion resistance of the coating. The chromium oxide coating with a microcrystalline structure has high hardness and can effectively resist wear and scratches from external forces. This property enables the coating to maintain good performance for a long time in a friction and wear environment, which is better reflected in the microcrystalline structure, so that the coating has a better protective effect in a high-temperature oxidation environment. The chromium oxide coating with a microcrystalline structure has a stronger interface bonding force with the substrate, which can effectively prevent the coating from falling off or peeling off when subjected to external forces.

[0077] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0078] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0079] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40 to 80 KHZ;

[0080] S102: performing high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is ≥10 Bar, and the time of the high-pressure water washing is >20 minutes;

[0081] S103: soaking the surface of the splitting cutter base body after high-pressure water washing in a hydrocarbon cleaning agent at 60 to 80° C. for more than 3 hours;

[0082] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM, and the drying time is ≥15 minutes;

[0083] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0084] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0085] S201 evacuates the chamber and when the pressure inside the chamber reaches 10 -2 Bar below, argon gas is introduced into the chamber;

[0086] S202 continues to evacuate the chamber. When the pressure in the chamber reaches 10 -3 Bar, after turning on the DC power supply to 500V, the argon gas forms a plasma state, and the ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is ≤Ra0.05μm;

[0087] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0088] S301 continues to evacuate the chamber to 10 -5 Below Bar, the wedge substrate is heated to above 500 degrees at the same time to form a vacuum chamber;

[0089] S302: injecting argon gas into the vacuum chamber, wherein the flow rate of the argon gas pressure injected into the vacuum chamber is greater than 150 ml / min;

[0090] The S303 chromium target is used as a cathode to attract ionized argon ions to bombard the chromium target at high speed, and the chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -100 to -200V. Under the action of the electric field, the chromium atoms are deposited on the surface of the pre-treated splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 50 to 100nm.

[0091] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0092] S401 Move the CrO3 target to the opposite side of the splitter substrate, and keep the distance from the splitter substrate at 50mm to 150mm. Continue to evacuate the chamber until the pressure is ≤10 -5 Bar, while heating the wedge substrate to above 500°C to form a vacuum chamber;

[0093] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber are greater than 150 ml / min;

[0094] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed at the heating temperature of the splitter substrate (above 500°C) to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias on the CrO3 target. The negative bias formed on the CrO3 target is -100 to -200V. At the same time, in the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of the chromium element coating to form a chromium oxide coating. The chromium oxide coating has a microcrystalline structure and a thickness of 200nm to 1200nm.

[0095] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0096] Preferably, the hydrocarbon cleaning agent comprises the following components in weight percentage: 60-80% n-dodecane or isododecane; 10-20% 1,1,1,2,3-pentafluoropropane or 1,1,1,3,3-pentafluoropropane; 10%-20% oxalic acid; the hydrocarbon cleaning agent formula is selected from the above components, which can dissolve many substances, remove grease, dust and other stains through strong dissolving effect, has strong activity and inertness, and can form stable compounds with other elements, so as to better play the role of the hydrocarbon cleaning agent. For metal type dirt, new substances are generated through chemical reactions to achieve the purpose of removing metal dirt.

[0097] Preferably, the negative bias voltage generated by the RF power supply is calculated by the following formula:

[0098] V = k(W / P)^1 / 2;

[0099] Where V is the negative bias voltage generated by the RF power supply;

[0100] k is a factor that depends on the electrode area;

[0101] W is the RF power;

[0102] P is the gas pressure.

[0103] The present invention provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any one of the above items. The splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating presents a microcrystalline structure, the thickness of the chromium oxide coating is 200nm to 1200nm, and the thickness of the chromium element coating is 50 to 100nm.

[0104] Example 1

[0105] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0106] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0107] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40KHZ;

[0108] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 10 Bar, and the time of the high-pressure water washing is 21 minutes;

[0109] S103: soaking the surface of the splitter substrate after high-pressure water washing in a 60° C. three-dimensional hydrocarbon cleaning agent for 3.1 hours;

[0110] The hydrocarbon cleaning agent is composed of the following components in weight percentage: 60% n-dodecane, 20% 1,1,1,2,3-pentafluoropropane and 20% oxalic acid;

[0111] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 15 minutes;

[0112] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0113] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0114] S201 evacuates the chamber and when the pressure inside the chamber reaches 10 -2 Bar below, argon gas is introduced into the chamber;

[0115] S202 continues to evacuate the chamber. When the pressure in the chamber reaches 10 -3 Bar, after turning on the DC power supply to 500V, the argon gas forms a plasma state, and the ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.05μm;

[0116] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0117] S301 continues to evacuate the chamber to 10 -5 Below Bar, the wedge substrate is heated to above 500 degrees at the same time to form a vacuum chamber;

[0118] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0119] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -100V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 50nm.

[0120] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0121] S401 Move the CrO3 target to the opposite side of the splitter substrate and keep it 50mm away from the splitter substrate. Continue to evacuate the chamber until the pressure is ≤10-5 Bar, while heating the wedge substrate to above 500°C to form a vacuum chamber;

[0122] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0123] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed under the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on CrO3 target, and the negative bias voltage formed on CrO3 target is -100V. At the same time, under the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium element coating to form chromium oxide coating, and the chromium oxide coating has a microcrystalline structure and a thickness of 200nm.

[0124] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0125] The present invention provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any one of the above items, and the splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating presents a microcrystalline structure, the thickness of the chromium oxide coating is 200nm, and the thickness of the chromium element coating is 50nm.

[0126] Example 2

[0127] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0128] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0129] S101 uses ultrasonic cleaning on the surface of the splitter substrate, and the frequency of the ultrasonic cleaning is 80KHZ;

[0130] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 12 Bar, and the time of the high-pressure water washing is 22 minutes;

[0131] S103: soaking the surface of the splitter base body after high-pressure water washing in a hydrocarbon cleaning agent at 80° C. for 3.2 hours;

[0132] The hydrocarbon cleaning agent is composed of the following components in weight percentage: 80% n-dodecane, 10% 1,1,1,2,3-pentafluoropropane and 10% oxalic acid;

[0133] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 16 minutes;

[0134] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0135] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0136] S201 evacuates the chamber, and when the pressure in the chamber reaches below 10-2Bar, argon gas is introduced into the chamber;

[0137] S202: Continue to evacuate the chamber. When the pressure in the chamber reaches below 10-3 Bar, turn on the DC power supply to 500 V, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.04μm.

[0138] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0139] S301: continue to evacuate the cavity to below 10-5 Bar, and heat the wedge substrate to above 500 degrees to form a vacuum chamber;

[0140] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 153 ml / min;

[0141] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -150V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 75nm.

[0142] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0143] S401: Move the CrO3 target to the opposite side of the splitter substrate, and keep it 75mm away from the splitter substrate. Continue to evacuate the cavity to a pressure of ≤10-5Bar. Meanwhile, heat the splitter substrate to above 500℃ to form a vacuum chamber.

[0144] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 153 ml / min;

[0145] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed under the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on CrO3 target, and the negative bias voltage formed on CrO3 target is -150V. At the same time, under the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium element coating to form chromium oxide coating, and the chromium oxide coating has a microcrystalline structure and a thickness of 750nm;

[0146] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0147] The present invention provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any one of the above items, and the splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating presents a microcrystalline structure, the thickness of the chromium oxide coating is 750nm, and the thickness of the chromium element coating is 75nm.

[0148] Example 3

[0149] The present invention provides a method for preparing a wedge coating, comprising the following steps:

[0150] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0151] S101 uses ultrasonic cleaning on the surface of the splitting cutter substrate, and the frequency of the ultrasonic cleaning is 60KHZ;

[0152] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 13 Bar, and the time of the high-pressure water washing is 23 minutes;

[0153] S103: soaking the surface of the splitter substrate after high-pressure water washing in a hydrocarbon cleaning agent at 70° C. for 3.3 hours;

[0154] The hydrocarbon cleaning agent is composed of the following components in weight percentage: 70% isododecane, 15% 1,1,1,3,3-pentafluoropropane and 15% oxalic acid;

[0155] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 17 minutes;

[0156] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0157] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0158] S201 evacuates the chamber, and when the pressure in the chamber reaches below 10-2Bar, argon gas is introduced into the chamber;

[0159] S202: Continue to evacuate the chamber. When the pressure in the chamber reaches below 10-3 Bar, turn on the DC power supply to 500 V, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.03μm.

[0160] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0161] S301: continue to evacuate the cavity to below 10-5 Bar, and heat the wedge substrate to above 500 degrees to form a vacuum chamber;

[0162] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 155 ml / min;

[0163] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -200V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 100nm.

[0164] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0165] S401: Move the CrO3 target to the opposite side of the splitter substrate, 150 mm away from the splitter substrate, continue to evacuate the chamber to a pressure of ≤10-5Bar, and heat the splitter substrate to above 500°C to form a vacuum chamber;

[0166] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 155 ml / min;

[0167] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed under the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on CrO3 target, and the negative bias voltage formed on CrO3 target is -200V. At the same time, in the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium element coating to form chromium oxide coating, and the chromium oxide coating has a microcrystalline structure, and the thickness of the chromium oxide coating is 1200nm;

[0168] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0169] The present invention provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any one of the above items, and the splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating presents a microcrystalline structure, the thickness of the chromium oxide coating is 1200nm, and the thickness of the chromium element coating is 100nm.

[0170] Comparative Example 1

[0171] Comparative Example 1 provides a method for preparing a wedge coating, comprising the following steps:

[0172] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0173] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40KHZ;

[0174] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 10 Bar, and the time of the high-pressure water washing is 21 minutes;

[0175] S103: soaking the surface of the splitter substrate after high-pressure water washing in a 60° C. hydrocarbon cleaning agent for 3.1 hours;

[0176] The hydrocarbon cleaning agent is composed of the following components in weight percentage: 60% n-dodecane, 20% 1,1,1,2,3-pentafluoropropane and 20% oxalic acid;

[0177] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 15 minutes;

[0178] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0179] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0180] S201 evacuates the chamber, and when the pressure in the chamber reaches below 10-2Bar, argon gas is introduced into the chamber;

[0181] S202 continues to evacuate the chamber. When the pressure in the chamber reaches 10 -3 Bar, after turning on the DC power supply to 500V, the argon gas forms a plasma state, and the ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.05μm;

[0182] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0183] S301: continue to evacuate the cavity to below 10-5 Bar, and heat the wedge substrate to above 500 degrees to form a vacuum chamber;

[0184] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0185] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -100V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 50nm.

[0186] After the S4 chromium element coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0187] Comparative Example 1 provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any one of the above items, and the splitting knife coating comprises: a splitting knife substrate, and a chromium element coating is provided on the surface of the splitting knife substrate, and the thickness of the chromium element coating is 50nm.

[0188] Comparative Example 2

[0189] Comparative Example 2 provides a method for preparing a wedge coating, comprising the following steps:

[0190] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0191] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40KHZ;

[0192] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 10 Bar, and the time of the high-pressure water washing is 21 minutes;

[0193] S103: soaking the surface of the splitter substrate after high-pressure water washing in a 60° C. hydrocarbon cleaning agent for 3.1 hours;

[0194] Preferably, the hydrocarbon cleaning agent is composed of the following components in weight percentage: 60% n-dodecane, 20% 1,1,1,2,3-pentafluoropropane and 20% oxalic acid;

[0195] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 15 minutes;

[0196] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0197] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0198] S201 evacuates the chamber and when the pressure inside the chamber reaches 10 -2 Bar below, argon gas is introduced into the chamber;

[0199] S202: Continue to evacuate the chamber. When the pressure in the chamber reaches below 10-3 Bar, turn on the DC power supply to 500 V, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.05μm.

[0200] S3 uses radio frequency magnetron sputtering to produce a microcrystalline chromium oxide coating to obtain a wedge coating, which specifically includes the following steps:

[0201] S301 Move the CrO3 target to the opposite side of the splitter substrate and keep it 50mm away from the splitter substrate. Continue to evacuate the chamber until the pressure is ≤10 -5 Bar, while heating the wedge substrate to above 500°C to form a vacuum chamber;

[0202] S302 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0203] S303 uses a CrO3 target as a cathode to attract ionized argon ions to bombard the CrO3 target at high speed, and the CrO3 molecules are separated from the CrO3 target. At the heating temperature of the splitting knife substrate, the CrO3 molecules will decompose to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on the CrO3 target. The negative bias voltage formed on the CrO3 target is -100V. At the same time, in the presence of a micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of the pre-treated splitting knife substrate to form a chromium oxide coating. The chromium oxide coating has a microcrystalline structure and a thickness of 200nm.

[0204] After the S4 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0205] Comparative Example 2 provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any of the above items, and the splitting knife coating comprises: a splitting knife substrate, a chromium oxide coating is provided on the surface of the splitting knife substrate, the chromium oxide coating has a microcrystalline structure, and the thickness of the chromium oxide coating is 200nm.

[0206] Comparative Example 3

[0207] Comparative Example 3 provides a method for preparing a wedge coating, comprising the following steps:

[0208] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0209] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40KHZ;

[0210] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 10 Bar, and the time of the high-pressure water washing is 21 minutes;

[0211] S103: soaking the surface of the splitter substrate after high-pressure water washing in a 60° C. hydrocarbon cleaning agent for 3.1 hours;

[0212] Preferably, the hydrocarbon cleaning agent is composed of the following components in weight percentage: 60% n-dodecane, 20% 1,1,1,2,3-pentafluoropropane and 20% oxalic acid;

[0213] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 15 minutes;

[0214] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0215] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0216] S201 evacuates the chamber, and when the pressure in the chamber reaches below 10-2Bar, argon gas is introduced into the chamber;

[0217] S202: Continue to evacuate the chamber. When the pressure in the chamber reaches below 10-3 Bar, turn on the DC power supply to 500 V, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.05μm.

[0218] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0219] S301 continues to evacuate the chamber to 10 -5 Below Bar, the wedge substrate is heated to above 500 degrees at the same time to form a vacuum chamber;

[0220] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0221] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -100V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 50nm.

[0222] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0223] S401 Move the CrO3 target to the opposite side of the splitter substrate and keep it 50mm away from the splitter substrate. Continue to evacuate the chamber until the pressure is ≤10 -5 Bar, while heating the wedge substrate to above 500°C to form a vacuum chamber;

[0224] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0225] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed under the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on CrO3 target, and the negative bias voltage formed on CrO3 target is -100V. At the same time, in the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium element coating to form chromium oxide coating, and the chromium oxide coating has a microcrystalline structure and a thickness of 100nm;

[0226] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0227] Comparative Example 3 provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any of the above items, and the splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating in sequence from the inside to the outside, the chromium oxide coating has a microcrystalline structure, the thickness of the chromium oxide coating is 100nm, and the thickness of the chromium element coating is 50nm.

[0228] Comparative Example 4

[0229] Comparative Example 4 provides a method for preparing a wedge coating, comprising the following steps:

[0230] S1 cleans the surface of the riving cutter substrate, specifically comprising the following steps:

[0231] S101 uses ultrasonic cleaning on the surface of the splitting knife substrate, and the frequency of the ultrasonic cleaning is 40KHZ;

[0232] S102 performs high-pressure water washing on the surface of the splitting cutter substrate after ultrasonic cleaning, wherein the water pressure of the high-pressure water washing is 10 Bar, and the time of the high-pressure water washing is 21 minutes;

[0233] S103: soaking the surface of the splitter substrate after high-pressure water washing in a 60° C. hydrocarbon cleaning agent for 3.1 hours;

[0234] Preferably, the hydrocarbon cleaning agent is composed of the following components in weight percentage: 60% n-dodecane, 20% 1,1,1,2,3-pentafluoropropane and 20% oxalic acid;

[0235] S104: drying the surface of the soaked splitter substrate in a centrifuge, wherein the rotation speed of the centrifuge is 10000 RPM and the drying time is 15 minutes;

[0236] S105 packages the dried splitting knife substrate in a dust-free environment, and the dust-free environment level is within 10,000 levels;

[0237] S2 pre-treats the cleaned splitter substrate, specifically comprising the following steps:

[0238] S201 evacuates the chamber, and when the pressure in the chamber reaches below 10-2Bar, argon gas is introduced into the chamber;

[0239] S202: Continue to evacuate the chamber. When the pressure in the chamber reaches below 10-3 Bar, turn on the DC power supply to 500 V, and the argon gas forms a plasma state. The ionized argon ions bombard the surface of the splitter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitter substrate is Ra0.05μm.

[0240] S3 forms a chromium coating on the surface of the pretreated splitter substrate, specifically comprising the following steps:

[0241] S301: continue to evacuate the cavity to below 10-5 Bar, and heat the wedge substrate to above 500 degrees to form a vacuum chamber;

[0242] S302: injecting argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0243] The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias voltage on the chromium target. The negative bias voltage formed on the chromium target is -100V. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating. The thickness of the chromium element coating is controlled at 50nm.

[0244] S4 uses a radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating to obtain a wedge coating, which specifically includes the following steps:

[0245] S401 Move the CrO3 target to the opposite side of the splitter substrate and keep it 50mm away from the splitter substrate. Continue to evacuate the chamber until the pressure is ≤10 -5 Bar, while heating the wedge substrate to above 500°C to form a vacuum chamber;

[0246] S402 injects argon gas into the vacuum chamber, and the pressure and flow rate of the argon gas injected into the vacuum chamber is 151 ml / min;

[0247] S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed under the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias voltage on CrO3 target, and the negative bias voltage formed on CrO3 target is -100V. At the same time, in the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium element coating to form chromium oxide coating, and the chromium oxide coating has a microcrystalline structure, and the thickness of the chromium oxide coating is 1500nm;

[0248] After the S5 wedge coating is deposited, wait for the vacuum chamber to cool down, release the air pressure, and close the vacuum chamber.

[0249] Comparative Example 4 provides a splitting knife coating, which is prepared according to the preparation method of the splitting knife coating as described in any of the above items, and the splitting knife coating comprises: a splitting knife substrate, the surface of the splitting knife substrate is provided with a chromium element coating and a chromium oxide coating from the inside to the outside, the chromium oxide coating has a microcrystalline structure, the thickness of the chromium oxide coating is 1500nm, and the thickness of the chromium element coating is 50nm.

[0250] Experimental means of experimental data testing

[0251] The wedge coatings of Examples 1-3 and Comparative Examples 1-4 were tested by the following experimental means:

[0252] The thickness of the coating on the splitter is tested using the following steps:

[0253] 1. Standard sample for film thickness test, made of the same material as the base material of the splitter in this application, ground into a flat surface (such as Figure 6 As shown), the flat surface is for subsequent deposition of coatings;

[0254] 2. The deposited coating is placed into a flattened standard sample block and placed together with the splitter substrate of the present application, and the same process of preparing the splitter coating is followed;

[0255] 3. After the completion, use the film peeling method to remove part of the cleaver coating;

[0256] 4. Use KEYENCE's 3D laser scanning microscope VK-3000 to measure the height difference, which is the thickness of the coating on the part of the splitter.

[0257] The bonding strength of the splitter coating can be confirmed by whether the splitter coating on the surface peels off after wire bonding.

[0258] The roughness of the coating surface of the wedge is quantitatively measured by a 3D laser profile scanner;

[0259] The maximum number of wire bonding times for the wedge coating is determined by the actual bonding of the wire bonding machine. The parameters of the wire bonding machine are shown in Table 1. The final judgment is based on the morphology and size of the first and second welding points after bonding and the wire tension. If it exceeds the specification requirements, it is unqualified.

[0260] Table 1 Parameters of wire bonding machine

[0261]

[0262] The experimental data of the wedge coatings of Examples 1-3 and Comparative Examples 1-4 after testing by the above experimental means are as follows in Table 2:

[0263] Table 2 Experimental data of the wedge coating of Examples 1-3 and Comparative Examples 1-4

[0264]

[0265] From Table 1, we can observe that the splitting knife coatings prepared in Examples 1-3 reduce the roughness of the surface of the splitting knife coatings, improve the bonding force between the coatings and the splitting knife substrate, and thus improve the service life of the splitting knife; the splitting knife coatings prepared in Comparative Example 1 lack the chromium oxide coating compared to the splitting knife coatings prepared in Example 1. Although the bonding force between the coatings and the splitting knife substrate is maintained, the roughness of the surface of the splitting knife coating is increased to 0.25 μm, which increases the roughness of the surface of the splitting knife coating. The maximum number of wire bonding applications of the splitting knife coating is reduced to 1,300 thousand times, which reduces the service life of the splitting knife coating; the splitting knife coatings prepared in Comparative Example 2 lack the chromium element coating compared to the splitting knife coatings prepared in Example 1. The splitting knife coatings on the surface of the splitting knife substrate peel off, resulting in the coating and the splitting knife. The bonding force between the substrates is poor; the splitting knife coating prepared in Comparative Example 3 is that the thickness of the chromium oxide coating is reduced to 100nm compared to the splitting knife coating prepared in Example 1. Although the bonding force between the coating and the splitting knife substrate and the roughness of the surface of the splitting knife coating are maintained, the maximum number of application wire bonding times of the splitting knife coating is reduced to 1500 thousand times, which reduces the service life of the splitting knife coating; the splitting knife coating prepared in Comparative Example 4 is that the thickness of the chromium oxide coating is increased to 1500nm compared to the splitting knife coating prepared in Example 1. Although the bonding force between the coating and the splitting knife substrate is maintained, the roughness of the surface of the splitting knife coating is increased to 0.15μm, which increases the roughness of the surface of the splitting knife coating. At the same time, the maximum number of application wire bonding times of the splitting knife coating is reduced to 1350 thousand times, which reduces the service life of the splitting knife.

[0266] like Figure 3 As shown, from the XRD diagram of the chromium oxide coating provided in Example 1 of the present invention, we can observe that the four circled peaks in the figure are consistent with chromium oxide, proving that the chromium oxide coating is prepared in this application.

[0267] like Figure 4 As shown in the SEM image of the chromium oxide coating produced by the CVD (chemical vapor deposition) method provided by the background technology, we can observe that since the chromium oxide produced by CVD easily grows into a columnar crystal structure of the {1,1,1} plane, the coating surface will appear uneven, the grain morphology is sharp and cracked, the grain morphology is uneven, and there are fractures between the grains, resulting in an increase in the surface roughness of the splitter.

[0268] like Figure 5 As shown, from the SEM image of the chromium oxide coating produced by the RF magnetron sputtering method provided in Example 1 of the present invention, we can observe that the coating surface does not appear uneven, the grain morphology surface is smooth and has no cracks, the grain morphology is uniform, and the grains are continuous and dense, which reduces the roughness of the surface of the splitting knife coating.

[0269] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all various changes or equivalent substitutions falling within the scope of the claims of the present application are included. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of the present application are within the scope protected by the present invention.

Claims

1. A method for preparing a wedge coating, characterized in that: The following steps are involved: S1 cleans the surface of the splitting cutter base; S2 pre-treats the cleaned splitter substrate; S3 forms a chromium coating on the surface of the pre-treated splitter substrate; S4 uses radio frequency magnetron sputtering method to produce a microcrystalline chromium oxide coating on the chromium element coating, which specifically includes the following steps: S401 continues to evacuate the cavity, and at the same time heats the wedge substrate to above 500° C. to form a vacuum chamber; S402 injects argon gas into the vacuum chamber; S403 uses CrO3 target as cathode, attracts ionized argon ions to bombard CrO3 target at high speed, CrO3 molecules are separated from CrO3 target, and CrO3 molecules are decomposed at the heating temperature of splitter substrate to generate Cr2O3 and O2. A radio frequency power supply is used to form a negative bias on CrO3 target. At the same time, in the micro-oxygen atmosphere formed by O2, Cr2O3 is deposited on the surface of chromium coating to form chromium oxide coating, thus obtaining splitter coating; The air pressure in the vacuum chamber is ≤10 -5 Bar, the pressure flow rate of argon gas injected into the vacuum chamber is greater than 150ml / min, and the negative bias voltage formed on the CrO3 target is -100~-200 V.

2. The method for preparing a wedge coating according to claim 1, characterized in that: Step S3 forms a chromium coating on the surface of the pretreated splitter substrate, which specifically includes the following steps: S301 evacuates the cavity and heats the wedge substrate to above 500° C. to form a vacuum chamber; S302 injects argon gas into the vacuum chamber; The S303 chromium target is used as the cathode to attract ionized argon ions to bombard the chromium target at high speed. The chromium atoms are separated from the chromium target. A radio frequency power supply is used to form a negative bias on the chromium target. Under the action of the electric field, the chromium atoms are deposited on the pre-treated surface of the splitter to form a chromium element coating.

3. The method for preparing a wedge coating according to claim 2, characterized in that: The air pressure in the vacuum chamber is ≤10 -5 Bar, the pressure flow rate of argon gas injected into the vacuum chamber is greater than 150ml / min, and the negative bias voltage formed on the chromium target is -100~-200V.

4. The method for preparing a wedge coating according to claim 1, characterized in that: Step S1 is to clean the surface of the riving cutter base, comprising the following steps: S101 uses ultrasonic cleaning on the surface of the splitter substrate; S102 performs high-pressure water washing on the surface of the splitter substrate after ultrasonic cleaning; S103: soaking the surface of the splitting cutter base body after high-pressure water washing in a hydrocarbon cleaning agent; S104 spin-drying the surface of the soaked splitter base; S105 packages the dried splitting knife substrate in a dust-free environment.

5. The method for preparing a wedge coating according to claim 4, characterized in that: The hydrocarbon cleaning agent comprises the following components in percentage by weight: n-Dodecane or isododecane 60-80%; 1,1,1,2,3-pentafluoropropane or 1,1,1,3,3-pentafluoropropane 10-20%; Oxalic acid 10%~20%.

6. The method for preparing a wedge coating according to claim 4 or 5, characterized in that: The temperature of the hydrocarbon cleaning agent is 60-80° C., and the immersion time of the hydrocarbon cleaning agent is more than 3 hours.

7. The method for preparing a wedge coating according to claim 1, characterized in that: Step S2 pre-processes the cleaned splitting knife, including the following steps: After the cavity is evacuated in step S201, argon gas is introduced into the cavity; After the chamber is further evacuated in step S202 and the DC power supply is turned on, the argon gas forms a plasma state, and the ionized argon ions bombard the surface of the splitting cutter substrate. This process lasts for more than 30 minutes. After pretreatment, the roughness of the surface of the splitting cutter substrate is ≤Ra0.05μm.

8. A cleaver coating, characterized in that: The coating is prepared according to the method for preparing the splitting knife coating according to any one of claims 1 to 7.

9. The wedge coating according to claim 8, characterized in that: include: The splitting knife substrate has a chromium element coating and a chromium oxide coating arranged on its surface from the inside to the outside, the chromium oxide coating has a microcrystalline structure, and the thickness of the chromium oxide coating is 200nm to 1200nm.