A porous covalent organic framework nanofiber membrane and preparation method thereof
The preparation of porous COF nanofiber membranes through electrospinning technology has solved the problem of poor continuity and uniformity in the preparation of COF nanofiber membranes in the prior art, achieved efficient adsorption and high-throughput applications of materials, and was suitable for water treatment, etc. field.
Patent Information
- Application Number
- CN202410948115.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing COF nanofiber membrane preparation methods have problems such as poor continuity and uniformity, blockage of channels, long reaction time, and complex operation, which limit their large-scale production applications.
Using electrospinning technology, functional COF is mixed with dispersant and solubilizer and spinned evenly. Porous COF nanofiber membrane is prepared by regulating the spinning process parameters to ensure 100% COF content and macroscopic continuity, and reduce mass transfer resistance. , improve adsorption rate and capacity.
The high specific surface area and porosity of COF nanofiber membranes are achieved, giving material flexibility and macroscopic continuity, and are suitable for efficient applications in water treatment and other fields, simplifying the production process.
Smart Images

Figure CN118497980B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanofiber materials, and in particular to a porous covalent organic framework nanofiber membrane and a preparation method thereof. Background Art
[0002] Covalent Organic Framework (COF) is a porous polymer material with both chemical stability and crystallinity. Its structural characteristics are: a regular geometric framework composed of repeating structural units connected by covalent bonds. COF materials not only show ultra-high specific surface area, but also have rich nanopore structures, which makes them have broad application prospects in adsorption, separation, water treatment and other aspects.
[0003] Since traditional COF exists in powder form and is difficult to dissolve and melt, it is difficult to process, the separation procedure after use is complicated, and the recovery rate is low, which limits its practical application. Therefore, COF materials with macroscopic continuity can effectively solve the above problems. Among them, electrospun nanofibers have the characteristics of small fiber diameter, large specific surface area, and high porosity, and have broad application prospects in the field of water treatment.
[0004] Nowadays, the preparation methods of COF nanofiber membranes mainly include physical co-spinning of polymer and COF, in-situ growth of COF on the surface of polymer nanofibers, etc. Among them, the physical blending method is prone to microphase separation and agglomeration of polymer and COF in the system, resulting in poor continuity and uniformity of COF fibers. At the same time, the polymer will seriously block the active sites and pores of COF, resulting in pore blockage, which significantly reduces the specific surface area of the material. The COF fiber membrane prepared by the in-situ growth method has a dense structure and good crystallinity, but it has the disadvantages of long reaction time, complex operation, and low grafting efficiency. The above preparation methods of COF nanofiber membranes have high requirements on equipment and synthesis conditions, and the performance of the obtained products is poor, which seriously hinders the large-scale production and application of COF nanofiber membranes. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a porous covalent organic framework nanofiber membrane and a preparation method thereof.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] The invention discloses a method for preparing a porous covalent organic framework nanofiber membrane. Functional COF, a dispersant and a solubilizer are mixed in a solvent, and a uniform spinning solution is obtained after homogenization; the uniform spinning solution is subjected to electrostatic spinning to obtain a porous COF nanofiber membrane.
[0008] Preferably, the functional COF is functional COF-2, and the preparation method of the functional COF-2 is as follows: COF-1 is treated in an aqueous solution of hydroxylamine, and then filtered, washed, and dried to obtain functional COF-2; the preparation process of the COF-1 is as follows: a polyaldehyde monomer and a polyamine monomer are dissolved in a solvent, a catalyst is added, nitrogen is introduced, and then a reaction is carried out; after the reaction is completed, the precipitate is filtered, washed, and dried to obtain COF-1.
[0009] Preferably, the concentration of the functional COF is 10.0 to 35.0 wt%, the concentration of the dispersant is 0.5 to 5.0 wt%, and the concentration of the solubilizer is 1.0 to 10.0 wt%; the homogenization method includes one or more of ultrasound, magnetic stirring, mechanical stirring, high and low temperature treatment, the homogenization time is 10 to 360 min, and the temperature range of the high and low temperature treatment is -20 to 100 ° C.
[0010] Preferably, the dispersant is any one or more of toluene, benzene, naphthalene ring, polyether, polyurethane, PPA, citric acid, and triacylglycerol; the solubilizer is any one or more of urea, sodium alkylbenzene sulfonate, tert-butanol, Tween 80, polysorbate, and polyoxyethylene fatty acid ester; and the solvent in which the functional COF is mixed with the dispersant and the solubilizer is any one or more of deionized water, methanol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, chloroform, chloroform, N,N-dimethylformamide, N-methylpyrrolidone, 1,4-dioxane, N,N-dimethylacetamide, dimethyl sulfoxide, and acetone.
[0011] Preferably, the electrospinning parameters are voltage 15-30 kV, liquid supply rate 0.2-5.0 mL / min, receiving distance 10-40 cm, drum speed 30-80 r / min, spinning temperature 20-28 ° C, humidity 20-80%, and the material for receiving the fiber membrane is one of oil-absorbing paper, tin foil, aluminum foil, and non-woven fabric.
[0012] Preferably, the polyaldehyde monomer is 2,4,6-triformylphloroglucinol, trimesic acid, 1,3,5-tri(p-formylphenyl)benzene, 5''-(4-formylphenyl)-[1,1':4',1'':3'', 1''':4''',1''''-pentaphenyl]-4,4''''-dicarboxaldehyde, 5',5''''-(anthracene-9,10-diyl)bis(([1,1':3',1''-terphenyl]-4,4''-dicarboxaldehyde)), 5',5''''-bis(4-formylphenyl)-[1,1':3',1'':4'',1''':4''',1'''':3'''',1'''''-hexaphenyl]-4, The polyamino monomer is one or more of p-diaminoazobenzene, 2,6-diaminoanthraquinone, 2,5-diaminobenzonitrile, 4,4''-diamino-5'-(4-aminophenyl)-[1,1':3',1''-terphenyl]-3-carbonitrile, 2-amino-5-((4-aminophenyl)azo)benzonitrile, 2,6-diamino-9,10-dioxo-9,10-dihydroanthracene-1-carbonitrile, 2,5-diamino-1,4-benzoquinone, 4,4'-diamino-[1,1'-biphenyl]-3,3'-dicarbonitrile, and 4,4'-diamino-[1,1'-biphenyl]-3-carbonitrile;
[0013] The solvent for dissolving the polyaldehyde monomer and the polyamine monomer is any one or more of mesitylene, methanol, chloroform, benzyl alcohol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, 1,4-dioxane, acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and acetone;
[0014] The catalyst is one or more of acetic acid, toluenesulfonic acid, diglycolic acid, phosphoric acid, and sulfonic acid;
[0015] The detergent used in the washing process is one or more of DMAc, deionized water, methanol, ethanol, DMF, and acetone.
[0016] Preferably, the concentration of the catalyst is 20-100wt%, the concentrations of the polyaldehyde monomer and the polyamine monomer are 0.36-1.00mM respectively, the molar ratio of the polyaldehyde monomer to the polyamine monomer is 0.66-1.5:1, and the concentration of the hydroxylamine aqueous solution is 5-20%.
[0017] Preferably, the nitrogen introduction time is 8 to 20 minutes, the reaction time is 24 to 120 hours, the reaction temperature is 80 to 160°C, the product drying temperature is -100°C to -50°C, and the drying time is 12 to 24 hours.
[0018] Preferably, the COF-1 is treated in the hydroxylamine aqueous solution for 12 to 72 hours, the treatment temperature is 50 to 120° C., the product drying temperature is -120° C. to -60° C., and the drying time is 8 to 48 hours.
[0019] Correspondingly, a porous covalent organic framework nanofiber membrane prepared by the above preparation method has a porous size including macropores, mesopores and micropores.
[0020] The present invention has the following beneficial effects:
[0021] 1. The present invention adopts electrostatic direct spinning technology to prepare COF nanofiber self-supporting membrane, which not only retains the intrinsic high specific surface area and porosity of COF, but also gives the material excellent macroscopic continuity and flexibility, which helps to achieve its special effects in the fields of water pollutant treatment, uranium extraction from seawater, lithium extraction from salt lakes, etc.
[0022] 2. The present invention prepares the synthesized functional COF, dispersant and solubilizer into a uniform spinning solution, and directly obtains a COF nanofiber membrane with a porous structure by adjusting the parameters of the electrospinning process. The preparation method disclosed in the present invention can obtain a new porous COF nanofiber membrane with a COF content of 100% and no linear polymer support. In addition, the pore structure of the fiber membrane (including macropores, mesopores, and micropores) can effectively reduce the mass transfer resistance while ensuring that the material has a high adsorption rate and adsorption capacity, so as to achieve its special effects in the fields of adsorption and filtration.
[0023] 3. The preparation method disclosed in the present invention can ensure that the COF content in the porous nanofiber membrane reaches 100%, which gives the material macroscopic continuity and flexibility on the basis of maintaining the high specific surface area and nanopore structure of COF itself. The macropores on the porous COF nanofiber membrane can effectively reduce the mass transfer resistance, and the micro / mesopores can provide a high specific surface area and a large number of adsorption sites, achieving the high-throughput and high-efficiency requirements that need to be met in water treatment technology. The electrostatic direct spinning preparation method is simple to operate and easy to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The specific surface area and nitrogen adsorption-desorption curve of the porous COF nanofiber membrane of Example 1;
[0025] Figure 2 The porosity and pore size distribution diagram of the porous COF nanofiber membrane of Example 1;
[0026] Figure 3 is a cross-sectional SEM image of the porous COF nanofiber of Example 1;
[0027] Figure 4 This is a diagram showing the flexibility of the porous COF nanofiber membrane in Example 1. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0030] The present invention discloses a method for preparing a porous covalent organic framework nanofiber membrane, comprising the following steps:
[0031] S1: Synthesis of functional COF. Dissolve the polyaldehyde monomer and the polyamine monomer in a solvent, add them to a reactor, add a catalyst, introduce nitrogen, and react; after the reaction is completed, filter, wash, and freeze-dry the precipitate to obtain COF-1.
[0032] Benefits of COF functionalization: Although existing COF has general characteristics such as high porosity, large specific surface area, high crystallinity, and good stability, it does not have the characteristics of selective adsorption, which greatly limits its use scenarios. Therefore, in order to improve the performance of COF, this patent introduces a photosensitive structure to give COF photosensitivity, which generates photogenerated electrons and holes by absorbing photons. The generated electrons and holes can drive redox reactions and convert light energy into chemical energy. Photocatalysis, as a method that can break through adsorption equilibrium, has a larger adsorption capacity and adsorption rate than traditional adsorption.
[0033] The concentration of the catalyst is 20-100 wt %, the concentrations of the polyaldehyde monomer and the polyamine monomer are 0.36-1.00 mM, respectively, and the molar ratio of the polyaldehyde monomer to the polyamine monomer is 0.66-1.5: 1. The nitrogen introduction time is 8-20 min, the reaction time is 24-120 h, the reaction temperature is 80-160 ° C, the product drying temperature is -100 ° C to -50 ° C, and the drying time is 12-24 h.
[0034] S2: Further functional modification of COF-1: COF-1 is treated in a hydroxylamine aqueous solution, and then filtered, washed, and freeze-dried to obtain functional COF-2.
[0035] The obtained functional COF-2 has the following characteristics: it has both photosensitivity and amidoxime groups. The amidoxime-functionalized COF has a highly selective adsorption capacity for uranium in seawater; the photosensitivity drives the redox reaction to effectively improve the adsorption performance. Its selective adsorption, multiple active sites, excellent light capture ability, and efficient electron and hole separation performance break the single performance application of traditional COF and have excellent performance.
[0036] The concentration of the hydroxylamine aqueous solution is 5-20%, the modification time of the COF-1 in the hydroxylamine aqueous solution is 12-72 hours, the modification temperature is 50-120°C, the product drying temperature is -120°C--60°C, and the drying time is 8-48 hours.
[0037] S3: preparing a uniform spinning solution. The prepared functional COF (functional COF-2) is mixed with a dispersant and a solubilizer in a specific solvent, and a uniform spinning solution is obtained by a variety of homogenization methods.
[0038] Among them, the concentration of the functional COF is 10.0-35.0wt%, the concentration of the dispersant is 0.5-5.0wt%, and the concentration of the solubilizer is 1.0-10.0wt%; the homogenization method includes one or more of ultrasound, magnetic stirring, mechanical stirring, high and low temperature treatment, the homogenization time is 10-360min, and the temperature range of the high and low temperature treatment is -20-100°C.
[0039] S4: Electrospinning: The uniform spinning solution prepared in S3 is electrospun, the spinning condition parameters are set, and the fiber membrane receiving substrate is determined to obtain a porous COF nanofiber membrane.
[0040] Among them, the electrospinning parameters are voltage 15-30kV, liquid supply rate 0.2-5.0mL / min, receiving distance 10-40cm, drum speed 30-80r / min, spinning temperature 20-28°C, humidity 20-80%, and the material for receiving the fiber membrane is one of oil-absorbing paper, tin foil, aluminum foil, and non-woven fabric.
[0041] Further, in step S1, the polyaldehyde monomers are 2,4,6-triformyl phloroglucinol (Tp), trimesaldehyde (Tb), 1,3,5-tris(p-formylphenyl)benzene (BFPB), 5''-(4-formylphenyl)-[1,1':4',1'':3'',1''':4''',1''''-pentaphenyl]-4,4''''-dicarboxaldehyde (FQD), 5' ,5''''-(anthracene-9,10-diyl)bis(([1,1':3',1''-terphenyl]-4,4''-dicarboxaldehyde)) (ADBTD), 5',5''''-bis(4-formylphenyl)-[1,1':3',1'':4'',1''':4''',1'''':3'''',1'''''-hexaphenyl]-4,4'''''-dicarboxaldehyde ( The polyamino monomer is one or more of p-diaminoazobenzene (AZO-NH2), 2,6-diaminoanthraquinone (DAAQ), 2,5-diaminobenzonitrile (PDA-CN), 4,4''-diamino-5'-(4-aminophenyl)-[1,1':3',1''-terphenyl]-3-carbonitrile (TAPB-CN), 2-amino-5-((4-aminophenyl)azo)benzonitrile (AZO-CN), 2,6-diamino-9,10-dioxo-9,10-dihydroanthracene-1-carbonitrile (DAAQ-CN), 2,5-diamino-1,4-benzoquinone (DB), 4,4'-diamino-[1,1'-biphenyl]-3,3'-dicarbonitrile (DBD), and 4,4'-diamino-[1,1'-biphenyl]-3-carbonitrile (DBC).
[0042] The solvent for dissolving the polyaldehyde monomer and the polyamine monomer is any one or more of mesitylene, methanol, chloroform, benzyl alcohol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, 1,4-dioxane, acetonitrile, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and acetone; the catalyst is one or more of acetic acid, toluenesulfonic acid, diglycolic acid, phosphoric acid, and sulfonic acid. As a preferred solution, the concentration of acetic acid is 50-100wt%, the concentration of toluenesulfonic acid is 60-90wt%, the concentration of diglycolic acid is 30-80wt%, the concentration of phosphoric acid is 50-80wt%, and the concentration of sulfonic acid is 20-70wt%; the detergent used in the washing process is one or more of DMAc, deionized water, methanol, ethanol, DMF, and acetone. The detergent used in steps S1 and S2 is the same.
[0043] Furthermore, in step S3, the dispersant is any one or more of toluene, benzene, naphthalene ring, polyether, polyurethane, PPA polyphosphate, citric acid, and triacylglycerol; the solubilizer is any one or more of urea, sodium alkylbenzene sulfonate, tert-butyl alcohol, Tween 80, polysorbate, and polyoxyethylene fatty acid ester; the solvent in which the functional COF is mixed with the dispersant and the solubilizer is any one or more of deionized water, methanol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, chloroform, chloroform, N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), 1,4-dioxane, N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and acetone.
[0044] Furthermore, in electrospinning, the spinning solution uses dichloromethane, chloroform, dimethyl sulfoxide, DMAc, and DMF as good solvents, and deionized water, methanol, ethanol, n-butanol, and 1,4-dioxane as non-solvents, and the good solvent / non-solvent is mixed in a volume ratio of 5:5 to 9:1.
[0045] The present invention will be further described below in conjunction with specific embodiments.
[0046] Embodiment 1
[0047] A method for preparing a porous COF nanofiber membrane comprises the following steps:
[0048] S1: Synthesis of functional COF. Weigh 2,4,6-triformylphloroglucinol (Tp, 0.075 g, 0.36 mmol) and p-diaminoazobenzene (AZO-NH2, 0.114 g, 0.54 mmol) and dissolve them in 25 mL of a mixed solvent of mesitylene and DMAc (1:1, v / v), respectively. Mix 25 mL of the monomer solution in a reactor (a total of 50 mL of the solution), add catalyst acetic acid (80 wt%, 0.3 mL), pass nitrogen for 10 min, and synthesize at 120 ° C for 24 h. The precipitate after the reaction was filtered, washed with mesitylene / DMAc (1:1, v / v), deionized water, and methanol in turn, and freeze-dried at -69 ° C for 12 h to obtain COF-1.
[0049] S2: Further functional modification of COF-1. The COF-1 was treated with 14% hydroxylamine aqueous solution at 80°C for 28 h, filtered, washed with deionized water and acetone in sequence, and freeze-dried at -80°C for 13 h to obtain functional COF-2.
[0050] S3: Preparation of uniform spinning solution. The prepared functional COF-2 was mixed with 1wt% toluene and 2wt% urea in chloroform / ethanol (6:4, v / v) solvent at 20wt%, totaling 10mL, and the system was ultrasonically homogenized for 15min to obtain a uniform spinning solution.
[0051] S4: Electrospinning. The uniform spinning solution prepared in S3 was electrospun at a voltage of 15 kV, a liquid supply rate of 1.0 mL / min, a receiving distance of 15 cm, a drum speed of 40 r / min, an oil-absorbing paper as the receiving fiber membrane, a spinning temperature of 24 °C, and a humidity of 55%. After spinning, a functional porous COF nanofiber membrane was obtained.
[0052] The specific surface area, porosity and flexibility of the obtained functional porous COF nanofiber membrane were measured, and the fiber cross section was observed by scanning electron microscopy (SEM), showing that the porous ( Figure 1 , Figure 2 )、Cross-sectional morphology( Figure 3 ) and flexibility ( Figure 4 ).
[0053] Embodiment 2
[0054] A method for preparing a porous COF nanofiber membrane comprises the following steps:
[0055] S1: Synthesis of functional COF. Weigh trimesaldehyde (Tb, 0.162 g, 1.00 mmol) and 2,6-diaminoanthraquinone (DAAQ, 0.238 g, 1.00 mmol) and dissolve them in 25 mL of mesitylene solvent, mix 25 mL of monomer solution in a reactor (a total of 50 mL of solution), add catalyst acetic acid (60 wt%, 0.4 mL), pass nitrogen for 15 min, and synthesize at 130 ° C for 30 h. The precipitate after the reaction was filtered, washed with mesitylene, deionized water, and ethanol in turn, and freeze-dried at -75 ° C for 15 h to obtain COF-1.
[0056] S2: Further functional modification of COF-1. A 16% hydroxylamine aqueous solution was used for treatment at 110°C for 45 h, and then filtered, washed with deionized water and acetone in sequence, and freeze-dried at -100°C for 16 h to obtain functional COF-2.
[0057] S3: Preparation of uniform spinning solution. The prepared functional COF-2 was mixed with 0.8wt% benzene and 1.5wt% sodium alkylbenzene sulfonate in DMF / methanol (7:3, v / v) solvent at 15wt%, totaling 10mL, and the system was magnetically stirred for 90min to obtain a uniform spinning solution.
[0058] S4: Electrospinning. The uniform spinning solution prepared in S3 was electrospun at a voltage of 18 kV, a liquid supply rate of 1.5 mL / min, a receiving distance of 17 cm, a drum speed of 50 r / min, a receiving fiber membrane material of tin foil, a spinning temperature of 26 ° C, and a humidity of 57%. After spinning, a functional porous COF nanofiber membrane was obtained.
[0059] The test results of the obtained functional porous COF nanofiber membrane are the same as those in Example 1, with no significant difference.
[0060] Embodiment 3
[0061] A method for preparing a porous COF nanofiber membrane comprises the following steps:
[0062] S1: Synthesis of functional COF. Weigh 1,3,5-tri(p-formylphenyl)benzene (BFPB, 0.195 g, 0.50 mmol) and 2,5-diaminobenzonitrile (PDA-CN, 0.133 g, 1.0 mmol) and dissolve them in 25 mL of DMAc solvent respectively. Mix 25 mL of monomer solution in a reactor (a total of 50 mL of solution), add catalyst toluenesulfonic acid (70 wt%, 0.5 mL), pass nitrogen for 12 min, and synthesize at 140 ° C for 36 h. The precipitate after the reaction was filtered, washed with DMAc, deionized water, and methanol in turn, and freeze-dried at -72 ° C for 15 h to obtain COF-1.
[0063] S2: Further functional modification of COF-1. 18% hydroxylamine aqueous solution was used for treatment at 90°C for 33 h, and then filtered, washed with deionized water and acetone in sequence, and freeze-dried at -85°C for 14 h to obtain functional COF-2.
[0064] S3: Preparation of uniform spinning solution. The prepared functional COF-2 was mixed with 22wt% naphthalene ring, 1.3wt% tert-butyl alcohol in a solvent of dimethyl sulfoxide / deionized water (8:3, v / v), a total of 10mL, and the system was ultrasonically homogenized for 20min to obtain a uniform spinning solution.
[0065] S4: Electrospinning. The uniform spinning solution prepared in S3 was electrospun at a voltage of 20 kV, a liquid supply rate of 1.5 mL / min, a receiving distance of 20 cm, a drum speed of 65 r / min, a non-woven fabric as the receiving fiber membrane material, a spinning temperature of 25 °C, and a humidity of 58%. After spinning, a functional porous COF nanofiber membrane was obtained.
[0066] The test results of the obtained functional porous COF nanofiber membrane are the same as those in Example 1, with no significant difference.
[0067] Embodiment 4
[0068] A method for preparing a porous COF nanofiber membrane comprises the following steps:
[0069] S1: Synthesis of functional COF. Weigh trimesic acid (Tb, 0.162 g, 1.00 mmol) and 2,5-diamino-1,4-benzoquinone (DB, 0.138 g, 1.00 mmol) and dissolve them in 25 mL of DMF / 1,4-dioxane (2:1, v / v) mixed solvent, mix 25 mL of monomer solution in a reactor (a total of 50 mL of solution), add catalyst diglycolic acid (50 wt%, 0.6 mL), pass nitrogen for 20 min, and synthesize at 160 ° C for 40 h. The precipitate after the reaction was filtered, washed with DMF / 1,4-dioxane (2:1, v / v), deionized water, and acetone in turn, and freeze-dried at -80 ° C for 20 h to obtain COF-1.
[0070] S2: Further functional modification of COF-1. A 20% hydroxylamine aqueous solution was used for treatment at 100°C for 40 h, and then filtered, washed with deionized water and acetone in sequence, and freeze-dried at -95°C for 15 h to obtain functional COF-2.
[0071] S3: Preparation of uniform spinning solution. The prepared functional COF-2 was mixed with 1.5wt% citric acid and 5.0wt% Tween 80 in a dichloromethane / 1,4-dioxane (8:2, v / v) solvent at 24wt%, totaling 10mL, and the system was ultrasonically homogenized for 30min to obtain a uniform spinning solution.
[0072] S4: Electrospinning. The uniform spinning solution prepared in S3 was electrospun at a voltage of 25 kV, a liquid supply rate of 2.0 mL / min, a receiving distance of 30 cm, a drum speed of 75 r / min, an aluminum foil as the receiving fiber membrane, a spinning temperature of 22 °C, and a humidity of 62%. After spinning, a functional porous COF nanofiber membrane was obtained.
[0073] The test results of the obtained functional porous COF nanofiber membrane are the same as those in Example 1, with no significant difference.
[0074] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a porous covalent organic framework nanofiber membrane, characterized in that: The functional COF is mixed with a dispersant and a solubilizer in a solvent, and a uniform spinning solution is obtained by homogenization; the uniform spinning solution is electrospun to obtain a porous COF nanofiber membrane; The functional COF is functional COF-2. The preparation method of the functional COF-2 is as follows: COF-1 is treated in a hydroxylamine aqueous solution, and then filtered, washed, and dried to obtain functional COF-2; the preparation process of COF-1 is as follows: polyaldehyde monomers and polyamine monomers are dissolved in a solvent, a catalyst is added, nitrogen is introduced, and then reacted; after the reaction is completed, the precipitate is filtered, washed, and dried to obtain COF-1; The concentration of the functional COF is 10.0-35.0wt%, the concentration of the dispersant is 0.5-5.0wt%, and the concentration of the solubilizer is 1.0-10.0wt%; the homogenization method includes one or more of ultrasound, magnetic stirring, mechanical stirring, high and low temperature treatment, the homogenization time is 10-360min, and the temperature range of the high and low temperature treatment is -20-100°C; The dispersant is any one or more of toluene, benzene, naphthalene ring, polyether, polyurethane, PPA, citric acid, and triacylglycerol; the solubilizer is any one or more of urea, sodium alkylbenzene sulfonate, tert-butyl alcohol, Tween 80, polysorbate, and polyoxyethylene fatty acid ester; the solvent in which the functional COF is mixed with the dispersant and the solubilizer is any one or more of deionized water, methanol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, chloroform, chloroform, N,N-dimethylformamide, N-methylpyrrolidone, 1,4-dioxane, N,N-dimethylacetamide, dimethyl sulfoxide, and acetone; The polyaldehyde monomer is any one or more of 2,4,6-triformylphloroglucinol, trimesaldehyde, 1,3,5-tris(p-formylphenyl)benzene, 5''-(4-formylphenyl)-[1,1':4',1'':3'',1''':4''',1''''-pentaphenyl]-4,4''''-dicarbaldehyde, 5',5''''-(anthracene-9,10-diyl)bis(([1,1':3',1''-terphenyl]-4,4''-dicarbaldehyde)), and 5',5''''-bis(4-formylphenyl)-[1,1':3',1'':4'',1''':4''',1'''':3'''',1''''-hexaphenyl]-4,4'''''-dicarbaldehyde; The polyamino monomer is one or more of p-diaminoazobenzene, 2,6-diaminoanthraquinone, 2,5-diaminobenzonitrile, 4,4''-diamino-5'-(4-aminophenyl)-[1,1':3',1''-terphenyl]-3-carbonitrile, 2-amino-5-((4-aminophenyl)azo)benzonitrile, 2,6-diamino-9,10-dioxo-9,10-dihydroanthracene-1-carbonitrile, 2,5-diamino-1,4-benzoquinone, 4,4'-diamino-[1,1'-biphenyl]-3,3'-dicarbonitrile, and 4,4'-diamino-[1,1'-biphenyl]-3-carbonitrile; The solvent for dissolving the polyaldehyde monomer and the polyamine monomer is any one or more of mesitylene, methanol, chloroform, benzyl alcohol, ethanol, n-butanol, dichloromethane, tetrahydrofuran, 1,4-dioxane, acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and acetone; The catalyst is one or more of acetic acid, toluenesulfonic acid, diglycolic acid, phosphoric acid, and sulfonic acid; The detergent used in the washing process is one or more of DMAc, deionized water, methanol, ethanol, DMF, and acetone; The concentration of the catalyst is 20-100 wt %, the concentrations of the polyaldehyde monomer and the polyamine monomer are 0.36-1.00 mM respectively, the molar ratio of the polyaldehyde monomer to the polyamine monomer is 0.66-1.5:1, and the concentration of the hydroxylamine aqueous solution is 5-20%; In the preparation process of the COF-1, the nitrogen introduction time is 8 to 20 minutes, the reaction time is 24 to 120 hours, the reaction temperature is 80 to 160°C, the product drying temperature is -100°C to -50°C, and the drying time is 12 to 24 hours; the COF-1 is treated in a hydroxylamine aqueous solution for 12 to 72 hours, the treatment temperature is 50 to 120°C, the product drying temperature is -120°C to -60°C, and the drying time is 8 to 48 hours.
2. The preparation method according to claim 1, characterized in that: The electrospinning parameters are voltage of 15-30 kV, liquid supply rate of 0.2-5.0 mL / min, receiving distance of 10-40 cm, drum speed of 30-80 r / min, spinning temperature of 20-28° C., humidity of 20-80%, and the material for receiving the fiber membrane is one of oil-absorbing paper, tin foil, aluminum foil, and non-woven fabric.
3. A porous covalent organic framework nanofiber membrane prepared by the preparation method according to any one of claims 1 to 2, characterized in that: The porous size of the nanofiber membrane includes macropores, mesopores and micropores.
Citation Information
Patent Citations
Preparation method of fiber containing porous covalent organic framework compound
CN103741243A
Flexible carbon fiber / COF film and preparation method thereof
CN115075013A
Flexible covalent organic framework-based composite fiber as well as preparation method and application thereof
CN115304730A
Covalent organic framework composite nanofiber electrochromic film and preparation and application thereof
CN116479583A
Covalent organic framework membranes, methods and uses thereof
WO2023009072A2