Bending-insensitive butterfly cable and preparation method thereof
By adding elastic rubber and carbon fiber reinforced porous titanium dioxide materials to the sheath of the optical fiber butterfly cable, combined with the coating technology of imidazole ionic liquid and chitosan, the attenuation and bending problems in optical fiber transmission are solved, and the mechanical strength and use are improved. life, achieves decomposition of pollutants, and improves the performance of optical fiber butterfly cables.
Patent Information
- Application Number
- CN202410949426.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The attenuation loss and nonlinear effects of optical fibers in existing optical fiber communication networks limit the improvement of system transmission performance, and bending in the transmission environment has a great impact on optical fibers, resulting in a decrease in transmission performance.
Adopting a butterfly cable structure, elastic rubber materials and carbon fiber reinforced modified porous titanium dioxide materials are added to the sheath to improve mechanical strength and bending properties, and a cross-linked coating layer is formed through imidazole ionic liquids, chitosan, and glutaraldehyde. , enhance the bonding degree between filler and sheath and the photocatalytic ability.
It achieves low attenuation and bend-insensitive optical fiber butterfly cables, improves mechanical strength and service life, and effectively decomposes contaminants on the sheath surface to keep it clean.
Smart Images

Figure CN118502046B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of communication optical cable manufacturing, and in particular relates to a bending-insensitive butterfly cable and a preparation method thereof. Background Art
[0002] With the continuous evolution of optical fiber transmission networks and the rapid growth of 5G communication networks, people's requirements for information transmission are getting higher and higher, and operators' demand for network transmission capacity is increasing. The attenuation loss and nonlinear effect of optical fiber have become the main factors restricting the improvement of system transmission performance. It is necessary to develop a low-attenuation and bend-insensitive optical fiber. Summary of the invention
[0003] The present invention provides a bending-insensitive butterfly cable and a preparation method thereof, comprising a butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by weight, 85-90 parts of polyethylene, 50-55 parts of EPDM rubber, 35-40 parts of polyamide, 15-20 parts of ethylene-vinyl acetate copolymer, 20-25 parts of carbon fiber reinforced modified porous titanium dioxide material, 4-8 parts of plasticizer, 5-8 parts of maleic anhydride grafted EPDM rubber, 3-6 parts of stearic acid, 2-5 parts of antioxidant, and 1-2 parts of polymethylvinylsiloxane. The butterfly cable adds elastic rubber material to the sheath to increase the elasticity of the sheath, thereby obtaining good bending performance, and at the same time adds modified carbon fiber reinforced modified porous titanium dioxide material to enhance the mechanical properties of the sheath, thereby obtaining a butterfly cable with excellent mechanical strength and capable of multiple bends.
[0004] The specific plan is as follows:
[0005] A bending-insensitive butterfly cable comprises a butterfly-shaped protective cover 1, an optical fiber 2 is arranged in the middle of the protective cover 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective cover 1 comprises, by weight: 85-90 parts of polyethylene, 50-55 parts of EPDM rubber, 35-40 parts of polyamide, 15-20 parts of ethylene-vinyl acetate copolymer, 20-25 parts of carbon fiber reinforced modified porous titanium dioxide material, 4-8 parts of plasticizer, 5-8 parts of maleic anhydride grafted EPDM rubber, 3-6 parts of stearic acid, 2-5 parts of antioxidant, and 1-2 parts of polymethylvinylsiloxane;
[0006] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0007] 1) Tetraethyl titanate is dispersed in ethanol, and then acetic acid solution is added to react completely to obtain a precursor solution;
[0008] 2) Add polyvinyl pyrrolidone, ethylenediamine and carbon nanofibers to the precursor solution, stir evenly, and dry to obtain a gel;
[0009] 3) soaking the gel in ethanol, drying, calcining, crushing and grinding to obtain a porous titanium dioxide material;
[0010] 4) adding porous titanium dioxide material, surfactant, imidazole ionic liquid, chitosan and glutaraldehyde into acetic acid solution, performing hydrothermal reaction, filtering and drying to obtain carbon fiber reinforced modified porous titanium dioxide material.
[0011] Furthermore, the plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.
[0012] Furthermore, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1790, antioxidant 245, antioxidant 168, antioxidant CA, antioxidant 264, and antioxidant 1076.
[0013] Furthermore, the imidazole ionic liquid is selected from 1-butyl-3-methylimidazole bromide and 1-butyl-3-methylimidazole chloride.
[0014] Furthermore, the surfactant is hexadecyltrimethylammonium bromide.
[0015] Furthermore, the carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0016] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 6-10 hours to obtain a precursor solution;
[0017] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 20-30g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0018] 3) Soaking the gel in ethanol for 30-60 hours, drying, calcining at 500-600° C. in air for 6-8 hours, crushing and grinding;
[0019] 4) Add 50g of the product of step 3, 5g of hexadecyltrimethylammonium bromide, 20-25g of 1-butyl-3-methylimidazole chloride, 2-4g of chitosan, and 1-2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0020] A method for preparing a bending-insensitive butterfly cable comprises the following steps: adding polyethylene, EPDM rubber, polyamide, ethylene-vinyl acetate copolymer, plasticizer, maleic anhydride grafted EPDM rubber, and polymethylvinylsiloxane into a mixer according to a predetermined mass ratio, mixing them evenly, then adding carbon fiber reinforced modified porous titanium dioxide material, stearic acid, and an antioxidant into the mixer, mixing them evenly, thermally dissolving, and granulating to obtain a sheath raw material, and then adding the sheath raw material into a screw extruder, extruding and coating the sheath raw material on the surface of the optical fiber and the reinforcement to obtain the butterfly cable.
[0021] Compared with the prior art, the beneficial effects of the present invention are:
[0022] 1) Elastic rubber material is added to the sheath of the butterfly cable to increase the elasticity of the sheath, thereby obtaining good bending performance;
[0023] 2) The filler is made of carbon fiber reinforced modified porous titanium dioxide material. The porous titanium dioxide material has a higher specific surface area and can improve the bonding degree with polymer macromolecules. At the same time, the carbon fiber reinforced porous titanium dioxide can form a chain structure with a titanium dioxide protrusion structure, which produces an anchoring effect in the polymer, slows down the slippage of the filler in the sheath layer, and increases the mechanical strength of the sheath layer. At the same time, imidazole ionic liquids, chitosan, and glutaraldehyde form a cross-linked coating on the surface of the carbon fiber, which is firmly coated on the carbon surface and not easy to fall off, thereby solidifying the titanium dioxide on the surface of the carbon fiber. Titanium dioxide, as a photocatalyst, can also effectively decompose pollutants on the surface of the sheath, keep the sheath clean, and increase the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a cross-sectional view of the butterfly cable of the present invention. DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with specific implementation methods. In each embodiment and comparative example, the wall thickness of the sheath is 0.3 mm; however, the protection scope of the present invention is not limited to the following embodiments, and any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.
[0026] Example 1
[0027] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 85 parts of polyethylene, 50 parts of EPDM rubber, 35 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 20 parts of carbon fiber reinforced modified porous titanium dioxide material, 4 parts of dioctyl phthalate, 5 parts of maleic anhydride grafted EPDM rubber, 3 parts of stearic acid, 2 parts of antioxidant 1010, and 1 part of polymethylvinylsiloxane;
[0028] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0029] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 6 hours to obtain a precursor solution;
[0030] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine and 20g carbon fiber into 100ml precursor solution, stir evenly and dry to obtain gel;
[0031] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0032] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 20 g of 1-butyl-3-methylimidazole chloride, 2 g of chitosan, and 1 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0033] Example 2
[0034] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 90 parts of polyethylene, 55 parts of EPDM rubber, 40 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 25 parts of carbon fiber reinforced modified porous titanium dioxide material, 8 parts of dioctyl phthalate, 8 parts of maleic anhydride grafted EPDM rubber, 6 parts of stearic acid, 5 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0035] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0036] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0037] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine and 30g carbon fiber into 100ml precursor solution, stir evenly and dry to obtain gel;
[0038] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0039] 4) Add 50g of the product of step 3, 5g of hexadecyltrimethylammonium bromide, 20g of 1-butyl-3-methylimidazole chloride, 4g of chitosan, and 2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0040] Example 3
[0041] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 90 parts of polyethylene, 50 parts of EPDM rubber, 40 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 25 parts of carbon fiber reinforced modified porous titanium dioxide material, 4 parts of dioctyl phthalate, 8 parts of maleic anhydride grafted EPDM rubber, 3 parts of stearic acid, 5 parts of antioxidant 1010, and 1 part of polymethylvinylsiloxane;
[0042] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0043] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0044] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine and 25g carbon fiber into 100ml precursor solution, stir evenly and dry to obtain gel;
[0045] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0046] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 22 g of 1-butyl-3-methylimidazole chloride, 3 g of chitosan, and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0047] Example 4
[0048] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 52 parts of EPDM rubber, 37 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 22 parts of carbon fiber reinforced modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0049] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0050] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0051] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine and 24g carbon fiber into 100ml precursor solution, stir evenly and dry to obtain gel;
[0052] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0053] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 22 g of 1-butyl-3-methylimidazole chloride, 3 g of chitosan, and 1.5 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0054] Example 5
[0055] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of carbon fiber reinforced modified porous titanium dioxide material, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0056] The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method:
[0057] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0058] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0059] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0060] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 24 g of 1-butyl-3-methylimidazole chloride, 3 g of chitosan, and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
[0061] Comparative Example 1
[0062] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of filler, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0063] The filler is prepared by the following method:
[0064] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0065] 2) Add 10g ethylenediamine and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0066] 3) calcining the gel at 600°C for 8 h in air atmosphere, crushing and grinding;
[0067] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 24 g of 1-butyl-3-methylimidazole chloride, 3 g of chitosan, and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a filler.
[0068] Comparative Example 2
[0069] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of filler, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0070] The filler is prepared by the following method:
[0071] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0072] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0073] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0074] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 3 g of chitosan and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter and dry to obtain a filler.
[0075] Comparative Example 3
[0076] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of filler, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0077] The filler is prepared by the following method:
[0078] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0079] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0080] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0081] 4) Add 50 g of the product of step 3, 5 g of hexadecyltrimethylammonium bromide, 24 g of 1-butyl-3-methylimidazole chloride, and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a filler.
[0082] Comparative Example 4
[0083] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of filler, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0084] The filler is prepared by the following method:
[0085] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0086] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0087] 3) Soaking the gel in ethanol for 60 hours, drying it, calcining it at 600°C in air for 8 hours, crushing it, and grinding it;
[0088] 4) Add 50g of the product of step 3, 5g of hexadecyltrimethylammonium bromide, 24g of 1-butyl-3-methylimidazole chloride, and 3g of chitosan to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a filler.
[0089] Comparative Example 5
[0090] A butterfly-shaped protective sleeve 1, an optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing core materials 3 are arranged on both sides of the optical fiber 2. The protective sleeve 1 comprises, by mass, 88 parts of polyethylene, 55 parts of EPDM rubber, 38 parts of polyamide, 18 parts of ethylene-vinyl acetate copolymer, 24 parts of filler, 7 parts of dioctyl phthalate, 7 parts of maleic anhydride grafted EPDM rubber, 4 parts of stearic acid, 4 parts of antioxidant 1010, and 2 parts of polymethylvinylsiloxane;
[0091] The filler is prepared by the following method:
[0092] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 10 hours to obtain a precursor solution;
[0093] 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 26g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel;
[0094] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600° C. for 8 hours in an air atmosphere, crushed, and ground to obtain a filler.
[0095] Experiments and Data
[0096] The tensile strength and environmental stress cracking time of the sheath material are tested in accordance with the national standard GB / T2951.
[0097] According to YD / T1997.1-2022 "Introduction Optical Fiber Cable for Communication Part 1: Butterfly Optical Cable", the optical cable performance was tested and the repeated bending: residual additional attenuation was obtained.
[0098] The results are shown in Table 1.
[0099] Table 1
[0100]
[0101] Tests and Results
[0102] As can be seen from Table 1, in Comparative Example 1, the effect of polyvinyl pyrrolidone can be seen, in Comparative Examples 2-4, the effects of imidazole ionic liquids, chitosan, and glutaraldehyde can be seen, and in Comparative Example 5, the effect of polymer coating modification can be seen; the butterfly cable adds elastic rubber material to the sheath to increase the elasticity of the sheath, thereby obtaining good bending performance; the filler adopts carbon fiber reinforced modified porous titanium dioxide material, the porous titanium dioxide material has a higher specific surface area, and can improve the bonding degree with polymer macromolecules. At the same time, the carbon fiber reinforced porous titanium dioxide can form a process with titanium dioxide, and polyvinyl pyrrolidone and ethylenediamine work together to make the modification effect better; at the same time, through imidazole ionic liquids, chitosan, and glutaraldehyde, a cross-linked coating is formed on the surface of the carbon fiber, and the carbon surface is firmly coated and not easy to fall off, thereby curing titanium dioxide on the surface of the carbon fiber. Titanium dioxide, as a photocatalyst, can also effectively decompose pollutants on the surface of the sheath, keep the sheath clean, and increase the service life. Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A bending-insensitive butterfly cable, comprising a butterfly-shaped protective cover, an optical fiber is arranged in the middle of the protective cover, and reinforcing core materials are arranged on both sides of the optical fiber, and the protective cover comprises, by mass: 85-90 parts of polyethylene, 50-55 parts of EPDM rubber, 35-40 parts of polyamide, 15-20 parts of ethylene-vinyl acetate copolymer, 20-25 parts of carbon fiber reinforced modified porous titanium dioxide material, 4-8 parts of plasticizer, 5-8 parts of maleic anhydride grafted EPDM rubber, 3-6 parts of stearic acid, 2-5 parts of antioxidant, 1-2 parts of polymethylvinylsiloxane; The carbon fiber reinforced modified porous titanium dioxide material is prepared by the following method: 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 6-10 hours to obtain a precursor solution; 2) Add 10g polyvinyl pyrrolidone, 10g ethylenediamine, and 20-30g carbon fiber to 100ml precursor solution, stir evenly, and dry to obtain a gel; 3) Soaking the gel in ethanol for 30-60 hours, drying, calcining at 500-600° C. in air for 6-8 hours, crushing and grinding; 4) Add 50g of the product of step 3, 5g of hexadecyltrimethylammonium bromide, 20-25g of 1-butyl-3-methylimidazole chloride, 2-4g of chitosan, and 1-2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a carbon fiber reinforced modified porous titanium dioxide material.
2. A bend-insensitive butterfly cable as claimed in claim 1, characterized in that: The plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.
3. A bend-insensitive butterfly cable as claimed in claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant 1010, antioxidant 1790, antioxidant 245, antioxidant 168, antioxidant CA, antioxidant 264, and antioxidant 1076.
4. A method for preparing a bend-insensitive butterfly cable as described in any one of claims 1 to 3, comprising adding polyethylene, EPDM rubber, polyamide, ethylene-vinyl acetate copolymer, plasticizer, maleic anhydride grafted EPDM rubber, and polymethylvinylsiloxane into a mixer according to a predetermined mass ratio and mixing them evenly, then adding carbon fiber reinforced modified porous titanium dioxide material, stearic acid, and an antioxidant into the mixer, mixing evenly, thermally dissolving, and granulating to obtain a sheath raw material, and then adding the sheath raw material into a screw extruder, extruding and coating it on the surface of the optical fiber and the reinforcement to obtain the butterfly cable.