A sintered Re-Fe-B permanent magnet and its preparation method and application
By forming Re-Fe-Ti-B rods that are only distributed at grain boundaries in NdFeB magnets, combined with grain boundary widening treatment and pulse aging heat treatment, the problem of insufficient coercive force of rare earth magnets is solved and the magnetic properties are improved. It can prevent the formation of boron-rich phase.
Patent Information
- Application Number
- CN202410954632.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-17
AI Technical Summary
It is difficult to effectively improve the coercivity of rare earth magnets in conventional production processes with existing technology. In particular, the presence of boron-rich phases in neodymium-iron-boron magnets is harmful to magnetic properties, and the method of controlling the cooling rate is difficult to implement, and the precipitated phase Ti-B The stick size is on the small side.
By forming the Ti-based precipitated phase Re-Fe-Ti-B rods in the NdFeB permanent magnet, they are only distributed in the grain boundary phase, and are formed into large sizes through the grain boundary widening treatment and pulse aging heat treatment in the preparation method. Re-Fe-Ti-B rods prevent the formation of boron-rich phases and inhibit grain growth, weakening the magnetic coupling effect.
It improves the magnetic properties of sintered Re-Fe-B permanent magnets, prevents the formation of boron-rich phases, increases the size of Re-Fe-Ti-B rods, weakens the magnetic coupling effect between main phase grains, and improves The coercivity and performance of the magnet.
Smart Images

Figure CN118507190B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth permanent magnet material preparation, and in particular relates to a sintered Re-Fe-B permanent magnet and a preparation method and application thereof. Background Art
[0002] Rare earth magnets, especially neodymium iron boron (NdFeB) magnets, are widely used in various equipment and devices due to their excellent magnetic properties, such as motors, generators, computer hard disk drives, etc. At present, the market for high-performance NdFeB applications is gradually expanding. In order to improve the coercive force of the magnet, heavy rare earth elements such as dysprosium (Dy) and terbium (Tb) are usually added, but the scarcity and high cost of these elements limit their widespread application.
[0003] In the structure of NdFeB, the boron-rich phase is a non-ferromagnetic phase, which is harmful and useless for magnetic properties. In current manufacturing technology, adding some metal elements, such as Ti and Zr, will generate additional precipitation phases with B elements due to their very low solubility in the grain boundary phase, reduce the ratio of the B-rich phase in the non-magnetic phase, and improve the coercive force. Patent document CN116978653A attempts to control the morphology and distribution of the metal precipitation phase by changing the cooling rate, thereby improving the coercive force of the magnet, but the method of controlling the cooling rate has high requirements on equipment, is difficult to implement, and the size of the precipitated phase Ti-B rod is small. Therefore, how to effectively improve the coercive force of rare earth magnets under conventional production processes is still a problem to be solved. Summary of the invention
[0004] In order to solve the above deficiencies of the prior art, the present invention provides the following technical solutions:
[0005] A sintered Re-Fe-B permanent magnet, the sintered Re-Fe-B permanent magnet has a Ti-based precipitation phase, the Ti-based precipitation phase is a Re-Fe-Ti-B rod-shaped object; the length of the Re-Fe-Ti-B rod-shaped object is 100-300nm; in the Ti-based precipitation phase, the atomic percentage content of Re is 1-20at%, the atomic percentage content of Fe is 1-30at%, the atomic percentage content of Ti is 40-90at%, and the atomic percentage content of B is 10-20at%; the atomic percentage content ratio of Ti to B is 4:1-9:1. In the present invention, the Ti-based precipitation phase can also be represented by a Re-Fe-Ti-B phase.
[0006] According to an embodiment of the present invention, the grain boundary phase refers to the grain boundary between any two grains and / or the grain boundary between any three or more grains. In the present invention, the grain boundary between any two grains is recorded as an intergranular grain boundary; the grain boundary between any three or more grains is recorded as a triangular grain boundary, such as Figure 5 shown.
[0007] According to an embodiment of the present invention, the Ti-based precipitated phase is distributed only in the grain boundary phase.
[0008] According to an embodiment of the present invention, the length of the Re-Fe-Ti-B rods is, for example, 150 nm, 200 nm, or 250 nm.
[0009] According to an embodiment of the present invention, the atomic percentage ratio of Ti and B in the Ti-based precipitated phase is 4:1 to 9:1, for example, 5:1, 6:1, 7:1, or 8:1.
[0010] According to an embodiment of the present invention, the composition of the Re-Fe-B permanent magnet is Re a Fe 1-a-b-c-d M1 b Ti c B d ,in:
[0011] Re is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb, 28wt%≤a≤35wt%;
[0012] M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, and Zr, 0.5wt%≤b≤5wt%;
[0013] The content of Ti is 0.05wt%<c≤0.5wt%; preferably, the content of Ti is 0.1wt%<c<0.2wt%;
[0014] The content of B is 0.8 wt%≤d≤1.2 wt%; preferably, the content of B is 0.92 wt%<c<1.05 wt%;
[0015] The rest is Fe and inevitable impurity elements.
[0016] According to an embodiment of the present invention, in the composition of the Re-Fe-B permanent magnet, a, b, c, and d correspond to mass percentages.
[0017] According to an embodiment of the present invention, in the composition of the Re-Fe-B permanent magnet, the atomic contents of Re, Ti and B are [Re], [Ti], [B], respectively, and have the following relationship: [Re]-2[B]+4[Ti]≥1.91at%, preferably 2at%, 2.5at%, 3at%, 3.5at%, 4at%, 5at%, 6at%, 7at%, 8at%, 9at%, 10at%.
[0018] The present invention also provides a method for preparing the sintered Re-Fe-B permanent magnet, the method comprising the following steps:
[0019] (1) Preparing NdFeB quick-solidification thin sheets and performing grain boundary widening treatment on the NdFeB quick-solidification thin sheets;
[0020] (2) crushing the NdFeB quick-solidified flakes to obtain magnetic powder, the average particle size of the magnetic powder is 2 to 5 μm, and then pressing the magnetic powder into a compact;
[0021] (3) Sintering the compact obtained in step (2) in a vacuum environment to obtain the sintered Re-Fe-B permanent magnet.
[0022] According to an embodiment of the present invention, in step (1), the raw materials for preparing the NdFeB quick-setting sheet include:
[0023] Re, the mass content of Re is 28-35wt%; Re is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb;
[0024] M1, the mass content of M1 is 0.5wt%≤M≤5wt%; M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, and Zr;
[0025] Ti, the mass content of Ti is 0.1 wt%<Ti≤0.5wt%;
[0026] B, the mass content of B is 0.8 wt%≤B≤1.2 wt%;
[0027] The rest is Fe and inevitable impurity elements.
[0028] The inventors found that when Re is higher than 35wt%, the excessive Re content will significantly reduce the magnetic energy product of the magnet and cause a significant increase in cost; when Re is lower than 28wt%, there is not enough Re to form Re2Fe 14 B main phase grains, resulting in a significant decline in performance. In M1, the role of Co is to benefit the Curie temperature of the magnet and improve the temperature coefficient of magnetic properties; the role of Ga / Cu / Al is to improve the coercivity of the magnet, and the role of Nb / Zr is to replace part of the iron, which can effectively improve the coercivity and squareness of the magnet; when M is less than 0.5 wt%, the coercivity and temperature stability of the magnet will be significantly reduced; when M is greater than 5wt%, the magnetic energy product of the magnet will be greatly reduced.
[0029] According to an embodiment of the present invention, in order to generate Re-Fe-Ti-B in the grain boundary phase Mutually , it is necessary to further control the atomic contents of Re, Ti, and B, and their corresponding atomic contents have the meanings as described above, such as [Re]-2[B]+4[Ti]≥1.91% (at%).
[0030] If there is too much B in the magnet, a non-magnetic B-rich phase will be formed, causing a significant decrease in the performance of the magnet. At the same time, both Re and Ti consume B, from Re2Fe 14 In terms of B, 2%Re requires 1%B to form the necessary Re2Fe 14 B main phase grains (at%), in addition, Ti also consumes part of B. In order to ensure that the Re-Fe-Ti-B phase can be formed without forming an additional B-rich phase, the atomic contents of Re, Ti, and B need to satisfy the above relationship.
[0031] Illustratively, Nd: 29.5wt%, Ga: 0.2wt%, Al: 0.2wt%, Cu: 0.15wt%, Co: 1.0wt%, Ti: 0.25wt%, B: 1.0wt%, and the rest are Fe and impurity elements.
[0032] According to an embodiment of the present invention, in step (1), the NdFeB quick-setting sheet is prepared by a method known in the art, such as a quick-setting belt spinning technique. Exemplarily, the method for preparing the NdFeB quick-setting sheet is as follows: the raw material is heated to 1300-1600°C by electromagnetic induction to melt, and then the alloy melt is poured on a quenching roller (preferably a polished quenching roller), and after cooling, alloy flakes are obtained, namely, NdFeB quick-setting sheets.
[0033] According to an embodiment of the present invention, the step of the grain boundary widening treatment is as follows: the NdFeB quick-setting thin sheet cooled to 20-80°C is heated to 700-1000°C under vacuum conditions for 1-3 hours, and then cooled to room temperature. Preferably, during the grain boundary widening treatment, the NdFeB quick-setting thin sheet needs to be placed in a high-temperature resistant metal material container to ensure that the NdFeB quick-setting thin sheet is not contaminated.
[0034] The inventors also found that during the grain boundary widening treatment, when the heating temperature is lower than 700°C, the rare earth-rich phase in the grain boundary phase cannot be completely melted, resulting in uneven distribution of the rare earth-rich phase; when the heating temperature is higher than 1000°C, the edges of the main phase grains will melt and the columnar crystals will grow abnormally. When the treatment time is less than 1 hour, it cannot provide heat for uniform distribution of the rare earth-rich phase; when the treatment temperature is higher than 3 hours, it will cause increased costs and waste of energy.
[0035] The inventors found that during the cooling process of the alloy melt, the Re-Fe-Ti-B phase is precipitated first due to the higher melting point of the Re-Fe-Ti-B precipitate, but it is easy to be randomly distributed in the alloy quick-solidified thin sheet. After the alloy quick-solidified thin sheet is subjected to grain boundary widening treatment, the rare earth-rich phase in the grain boundary phase can be melted and flowed, so that the rare earth-rich phase wrapped outside the main phase grains (preferably columnar crystals) can be more evenly distributed, which is conducive to more evenly wrapping the main phase grains during the crushing process. Therefore, during the sintering process, the Re-Fe-Ti-B phase is distributed along the molten rare earth-rich phase to the grain boundary phase, especially gathered at the intergranular grain boundaries and triangular grain boundaries, providing the necessary conditions for the further growth of the Re-Fe-Ti-B phase in the subsequent sintering process.
[0036] According to an embodiment of the present invention, in step (2), the crushing step specifically includes: subjecting the NdFeB quick-solidified thin slices to hydrogen explosion to obtain a coarse crushed powder, and then subjecting the NdFeB quick-solidified thin slices to high-energy ball milling or air flow milling to obtain magnetic powder. Preferably, a lubricant can also be added during crushing, and the lubricant can be a lubricant known in the art, which is not specifically limited in the present invention. Furthermore, the amount of the lubricant added is 0.1~1wt% of the magnetic powder, for example, 0.1~0.5wt%.
[0037] Exemplarily, in step (2), the pulverizing step is as follows: the NdFeB quick-setting flakes are first subjected to hydrogen explosion to obtain a coarse pulverized powder, which is then ground and pulverized by a jet mill to obtain magnetic powder of a target particle size; optionally, after obtaining the magnetic powder of the target particle size, 0.1 to 0.5 wt % of a lubricant can be added to the mixture, for example, the mixture is mixed for 0.1 to 5 hours to uniformly mix the magnetic powder.
[0038] In the present invention, the hydrogen explosion, high-energy ball milling process and air flow milling process can be carried out using process conditions known in the art, as long as the magnetic powder can be obtained.
[0039] According to an embodiment of the present invention, in step (2), the preparation of the green compact includes: orienting and pressing the magnetic powder in a magnetic field to obtain a green compact. Preferably, the magnetic field can be a magnetic field known in the art, for example, the magnetic field strength is 2 T. Preferably, after the orienting and pressing, cold isostatic pressing can be optionally performed; preferably, the cold isostatic pressing can be performed using cold isostatic pressing conditions known in the art, which are not specifically limited in the present invention.
[0040] According to an embodiment of the present invention, in step (3), the sintering treatment comprises: heating the compact in a vacuum environment in stages to a sintering temperature of 1000-1100° C. for 0.5-4 hours, and performing a pulse aging heat treatment after cooling.
[0041] Preferably, the staged heating specifically includes: heating from room temperature to a first insulation temperature (such as 220-260°C, such as 240°C) for 10-60 minutes; then heating to a second insulation temperature (such as 380-420°C, such as 400°C) for 10-60 minutes (such as 30 minutes); then heating to a third insulation temperature (such as 700-750°C, such as 750°C) for 30-120 minutes (such as 90 minutes); further heating to a sintering temperature of 1000~1100°C for 0.5~4 hours (such as 3.5 hours). Furthermore, when heating in stages, the heating rate is 1-10°C / min, such as 5°C / min, 6°C / min, 8°C / min.
[0042] Preferably, the pulse aging heat treatment specifically includes: (a) heating to 700-900°C at a heating rate of 5-15°C / min, keeping the temperature for 2-6 hours, and cooling to room temperature; (b) repeating the operation of step (a) 1-5 times (for example, 2 times, 3 times, 4 times); (c) aging at 450-650°C for 2-6 hours.
[0043] The inventors found that 1) during the pulse aging heat treatment, the temperature of the aging heating process is controlled at 700-900°C in order to melt the rare earth-rich phase; when the aging heating times are too few, sufficient energy cannot be provided for the uniform distribution and crystallization of the Re-Fe-Ti-B rods, so the aging heating process is performed at least twice; 2) when the pulse aging heat treatment is used, the Re-Fe-Ti-B rods are distributed along the molten grain boundaries to the grain boundary phases (such as intergranular grain boundaries and triangular grain boundaries) and aggregate, and the Ti element and the B element crystallize at the Re-Fe-Ti-B rods, so that the size of the Re-Fe-Ti-B rods becomes larger, thereby hindering the growth of the grain size, weakening the magnetic coupling effect between the main phase grains, and improving the performance of the sintered Re-Fe-B permanent magnet.
[0044] The present invention also provides a sintered Re-Fe-B permanent magnet prepared by the above preparation method, and the sintered Re-Fe-B permanent magnet has the meaning as described above.
[0045] The present invention also provides the use of the sintered Re-Fe-B permanent magnet, preferably used in a motor.
[0046] Beneficial effects of the present invention:
[0047] The sintered NdFeB permanent magnet of the present invention forms large-sized Re-Fe-Ti-B rods through formula design combined with process optimization, prevents the formation of a boron-rich phase, and the Re-Fe-Ti-B rods are aggregated in the grain boundary phase, which can hinder the growth of grain size, inhibit the growth of main phase grains, weaken the magnetic coupling effect between main phase grains, and improve the performance of the sintered Re-Fe-B permanent magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 TEM image of Example 1.
[0049] Figure 2 TEM image of Comparative Example 1.
[0050] Figure 3 TEM image of Comparative Example 3-3.
[0051] Figure 4 Schematic diagram of sample column processing.
[0052] Figure 5 It is a schematic diagram of the sintered Re-Fe-B permanent magnet of the present invention. DETAILED DESCRIPTION
[0053] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0054] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0055] Examples 1-5
[0056] A method for preparing a sintered Re-Fe-B permanent magnet, comprising the following steps:
[0057] (1) The raw materials are prepared according to the proportions in Table 1, the prepared materials are vacuum melted at 1420°C for 15 minutes, and then poured onto the surface of the quenching roller, and then dropped into a water cooling barrel for cooling to obtain the desired flakes;
[0058] (2) Take the scales of step (1), perform grain boundary widening treatment, place them in a high-temperature resistant metal container and place them in a vacuum sintering furnace, heat them from room temperature to 900°C, keep them at 900°C for 300 minutes, and cool them to room temperature.
[0059] (3) The scales obtained in step (2) are coarsely crushed by hydrogen explosion and then ground by jet mill to obtain magnetic powder, the target particle size of which is VMD = 3.1 μm.
[0060] (4) filling the magnetic powder of step (3) into a vacuum press mold, pressing and molding the magnetic powder under a magnetic field strength of 2T, and obtaining a green compact after cold isostatic pressing;
[0061] (5) The pressed green sheet of step (4) is placed in a vacuum sintering furnace, and the temperature is increased from room temperature to 240°C at a rate of 6°C / min, and kept at 240°C for 60 min; then the temperature is increased to 400°C at a rate of 4°C / min, and kept at 400°C for 30 min; then the temperature is increased to 750°C at a rate of 5°C / min, and kept at 750°C for 90 min, and then the temperature is increased to 1040°C at a rate of 8°C / min and sintered for 3.5 h; then pulse aging heat treatment is performed: (a) after the first stage aging treatment at 800°C for 4 h, it is cooled to room temperature; (b) the first stage aging treatment of step (a) is repeated three times; (c) the second stage aging treatment is performed at 480°C for 4 h, and the Nd-Fe-B green sheet is obtained, which is the sintered Re-Fe-B permanent magnet.
[0062] Comparative Example 1
[0063] The method for preparing sintered Re-Fe-B permanent magnets in this comparative example is basically the same as that in Example 1, except that the scales in step (1) are not subjected to the grain boundary widening treatment in step (2), but are directly subjected to the treatment in steps (3) to (5).
[0064] Comparative Example 2
[0065] The method for preparing sintered Re-Fe-B permanent magnets in this comparative example is basically the same as that in Example 1, except that: in step (5), pulse aging heat treatment is not performed after sintering is completed;
[0066] The other steps are the same as in Example 1.
[0067] Comparative Examples 3-1, 3-2 and 3-3
[0068] The methods for preparing sintered Re-Fe-B permanent magnets in Comparative Examples 3-1, 3-2 and 3-3 are basically the same as those in Example 1, except that: in step (1), the corresponding raw material formulas in Table 1 are used for mixing and proportioning;
[0069] The other steps are the same as in Example 1.
[0070] Table 1 Raw material ratios of the examples and comparative examples
[0071]
[0072] Test Case
[0073] (1) Magnetic properties test:
[0074] After the Nd-Fe-B blanks prepared in the above examples and comparative examples were uniformly skinned, φ10*10 sample columns were processed along the central symmetric axis of the blanks for magnetic property testing. The sample column processing schematic diagram is shown in FIG. Figure 4 shown.
[0075] (2) Tissue characterization:
[0076] The Nd-Fe-B blanks prepared in the above-mentioned embodiments and comparative examples were sampled at the corners and the center area of each piece to make TEM test samples with a diameter of 3 mm and a thickness of 150 nm, and observed by TEM equipment respectively. After magnification, there is at least one complete main phase grain or grain boundary phase (including rare earth-rich phase) in the observation field, and the element distribution points containing the Ti element in the observation field are analyzed for composition.
[0077] The test results are shown in Table 2.
[0078] Table 2 Test results of examples and comparative examples
[0079]
[0080] Test results:
[0081] Figure 1 TEM image of the sample of Example 1. In the sample of Example 1, Re-Fe-Ti-B phase (which is Re-Fe-Ti-B rod-shaped) is observed. This phase is only distributed at the grain boundary. The composition of this phase is (PrNd) 1.9 Fe 4.1 Ti 81.4 B 12.6 ; and this phase is rod-shaped with a length of about 255nm.
[0082] Figure 2 TEM image of the sample of Comparative Example 1. In the sample of Comparative Example 1, a Re-Fe-Ti-B phase was observed, and the phase was distributed in the main phase grains.
[0083] Comparative Example 3-3
[0084] Figure 3 This is a TEM image of the sample of Comparative Example 3-3. In the sample of Comparative Example 3-3, no Re-Fe-Ti-B phase was observed.
[0085] From Table 1 and Table 2, we can see that:
[0086] Re-Fe-Ti-B phase can be observed in the grain boundary phase of Examples 1, 2, 3, and 4, and Re-Fe-Ti-B rods are distributed along the molten grain boundaries and aggregated at the grain boundary phases (such as intergranular grain boundaries and triangular grain boundaries). Ti and B elements crystallize at the Re-Fe-Ti-B rods, while there is no crystallization of Re-Fe-Ti-B rods in the main phase grains. At the same time, the sizes of the Re-Fe-Ti-B rods were observed to be 255nm, 193nm, 234nm, and 198nm, respectively. Since the large-sized Re-Fe-Ti-B phase is enriched at the grain boundary, it can better hinder the growth of grain size, weaken the magnetic coupling effect between the main phase grains, and improve the performance of the sintered Re-Fe-B permanent magnet.
[0087] Comparison between Example 1 and Comparative Examples 3-1, 3-2 and 3-3 shows that the Re-Fe-Ti-B rods can only be formed in the grain boundary phase of the permanent magnet when the B and Ti contents and ratios are within the present invention.
[0088] From the comparison between Example 1 and Comparative Example 1, it can be seen that if only pulse aging treatment is performed without grain boundary widening treatment, although there is a Re-Fe-Ti-B phase in the grain boundary phase of the permanent magnet, some Re-Fe-Ti-B rods will also enter the main phase grains, thereby destroying the structure of the main phase grains and causing the Br value of the permanent magnet to drop significantly.
[0089] From the comparison between Example 1 and Comparative Example 2, it can be seen that when the composition of the Nd-Fe-B blank is the same, if only the grain boundary widening treatment is performed, although Re-Fe-Ti-B rods can also be generated in the grain boundary phase of the permanent magnet, the size of the Re-Fe-Ti-B rods is significantly reduced due to the lack of pulse aging treatment. Therefore, the magnetic properties of Comparative Example 2 are worse than those of Example 1.
[0090] In summary, the inventors believe that the grain boundary widening treatment and pulse aging treatment can make the Re-Fe-Ti-B phase crystallize and aggregate and grow at the intergranular grain boundaries and triangular grain boundaries to obtain Re-Fe-Ti-B rods, thereby effectively inhibiting the growth of the main phase grains and reducing the proportion of the boron-rich phase inside the permanent magnet, which is ultimately beneficial to improving the magnetic properties of the permanent magnet.
[0091] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sintered Re-Fe-B permanent magnet, characterized in that: The sintered Re-Fe-B permanent magnet has a Ti-based precipitation phase, which is a Re-Fe-Ti-B rod-shaped object; the length of the Re-Fe-Ti-B rod-shaped object is 100-300nm; in the Ti-based precipitation phase, the atomic percentage of Re is 1-20at%, the atomic percentage of Fe is 1-30at%, the atomic percentage of Ti is 40-90at%, and the atomic percentage of B is 10-20at%; the atomic percentage ratio of Ti to B is 4:1-9:1; The composition of the Re-Fe-B permanent magnet is Re a Fe 1-a-b-c-d M1 b Ti c B d ,in: Re is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb, 28wt%≤a≤35wt%; M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, and Zr, 0.5wt%≤b≤5wt%; The content of Ti is 0.05wt%<c≤0.5wt%; The content of B is 0.8 wt%≤d≤1.2 wt%; The rest is Fe and unavoidable impurity elements; In the composition of the Re-Fe-B permanent magnet, the atomic contents of Re, Ti and B are [Re], [Ti], [B] respectively, which have the following relationship: [Re]-2[B]+4[Ti]≥1.91at%.
2. The sintered Re-Fe-B permanent magnet according to claim 1, characterized in that: The Ti-based precipitated phase is only distributed in the grain boundary phase.
3. The method for preparing a sintered Re-Fe-B permanent magnet according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) preparing a NdFeB quick-solidification sheet and performing a grain boundary widening treatment on the NdFeB quick-solidification sheet; (2) crushing the NdFeB quick-solidified thin sheets to obtain magnetic powder, wherein the average particle size of the magnetic powder is 2 to 5 μm, and then pressing the magnetic powder into a compact; (3) Sintering the compact obtained in step (2) in a vacuum environment to obtain the sintered Re-Fe-B permanent magnet.
4. The preparation method according to claim 3, characterized in that: In step (1), the raw materials for preparing the NdFeB quick-setting sheet include: Re, the mass content of Re is 28-35wt%; Re is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb; M1, the mass content of M1 is 0.5wt%≤M≤5wt%; M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, and Zr; Ti, the mass content of Ti is 0.1 wt%<Ti≤0.5wt%; B, the mass content of B is 0.8 wt%≤B≤1.2 wt%; The rest is Fe and inevitable impurity elements.
5. The preparation method according to claim 3, characterized in that: In step (1), the steps of the grain boundary widening treatment are as follows: the NdFeB quick-solidification thin sheet cooled to 20-80°C is heated to 700-1000°C under vacuum conditions for high temperature treatment for 1-3 hours, and then cooled to room temperature.
6. The preparation method according to claim 3, characterized in that: In step (2), the pulverizing step specifically includes: subjecting the NdFeB quick-solidified thin slices to hydrogen explosion to obtain coarse pulverized powder, and then subjecting the powder to high-energy ball milling or air flow milling to obtain magnetic powder.
7. The preparation method according to claim 3, characterized in that: In step (2), the preparation of the green compact includes: orienting and pressing the magnetic powder in a magnetic field to obtain a green compact.
8. The preparation method according to claim 3, characterized in that: In step (3), the sintering treatment includes: heating the compact in a vacuum environment in stages to a sintering temperature of 1000-1100° C. for 0.5-4 hours, and performing a pulse aging heat treatment after cooling.
9. The preparation method according to claim 8, characterized in that: The staged heating specifically includes: heating from room temperature to a first insulation temperature and keeping it for 10-60 minutes; then heating to a second insulation temperature and keeping it for 10-60 minutes; then heating to a third insulation temperature and keeping it for 30-120 minutes; and further heating to a sintering temperature of 1000-1100°C and keeping it for 0.5-4 hours.
10. The preparation method according to claim 8, characterized in that: The pulse aging heat treatment specifically includes: (a) heating to 700-900°C at a heating rate of 5-15°C / min, keeping the temperature for 2-6 hours, and cooling to room temperature; (b) repeating the operation of step (a) 1-5 times; (c) aging at 450-650°C for 2-6 hours.
11. Use of the sintered Re-Fe-B permanent magnet according to claim 1 or 2 in a motor.
Citation Information
Patent Citations
Sintered rare earth magnet and method of manufacture
CN116978653A
Preparation process and application of neodymium iron boron rare earth permanent magnet material with high coercive force
CN116190090A
Low-cost high-coercivity lace-rich neodymium-iron-boron permanent magnet, and preparation method therefor and use thereof
WO2022258070A1