A disulfide wet adhesive patch and its preparation and application

By introducing cleavable functional monomers and electrospinning technology into wet adhesive materials, instant adhesion and long-term stability of wet adhesive materials are achieved, solving the problems of slow adhesion formation and weak bonding ability of existing materials. , improves biocompatibility and mechanical properties, and is suitable for a variety of tissue surfaces.

CN118512634BActive Publication Date: 2024-10-29修原(辽宁)生物有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410979287.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-29
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing wet adhesion materials have shortcomings in aspects such as long adhesion formation time, weak binding ability, mismatched mechanical properties, low biocompatibility or inability to be benignly detached, making it difficult to meet clinical needs.

Method used

A composite hydrogel containing cleavable functional monomers is used to achieve instant adhesion and long-term stability through the dual mechanism of physical cross-linking and covalent cross-linking. Nanofiber membranes are prepared using electrospinning technology to optimize the structure of the material. and exist in forms to improve adhesion properties and biocompatibility.

Benefits of technology

It achieves instant adhesion and long-term stability in the short term, can trigger separation on demand, has good biocompatibility and mechanical properties, is suitable for a variety of tissue surfaces, and promotes wound healing and cell growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118512634B_ABST
    Figure CN118512634B_ABST
Patent Text Reader

Abstract

The present invention relates to a bioadhesive hydrogel, specifically a disulfide wet adhesive patch and its preparation and application, wherein the wet adhesive patch forms physical cross-linking and covalent cross-linking bonding forces with the wet biological tissue surface in the form of a hydrogel. The disulfide wet adhesive patch includes a wet adhesive hydrogel or a wet adhesive electrostatic spinning film, a preparation method of a composite hydrogel containing a cleavable functional monomer, and in particular a modification and purification method of the simplified functional monomer. An extracellular matrix-like nanofiber wet adhesive film is prepared using electrostatic spinning technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to bioadhesive hydrogel, in particular to a disulfide wet adhesive patch and its preparation and application. The wet adhesive patch forms physical cross-linking and covalent cross-linking bonding forces with the wet biological tissue surface in the form of hydrogel. Background Art

[0002] Every year, countless patients suffer from minor skin injuries or severe tissue damage. Choosing the right solution and wound treatment can effectively avoid wound infection, reduce fluid loss, and promote the recovery of tissue structure and function at the wound site. In clinical medicine, wound treatment mainly includes reconnecting injured tissues and closing wound edges. In traditional medical practice, sutures or tissue fixation nails are usually used to promote wound closure, so that the tissue structure is closely connected and can withstand a certain mechanical force to prevent wound dehiscence. Although suture treatment greatly reduces the exposure area of ​​the wound and the risk of wound infection, there are some situations where suture is not applicable, such as: organs or soft tissues with complex external and internal fine structures may leak liquid or air; large wounds are difficult to achieve effective closure using sutures, and the suture process often takes a long time, increasing the risk of wound infection and postoperative complications. With the continuous development of modern medical technology and the gradual development of new materials, wet adhesives such as tissue adhesives, hemostats and tissue sealants (usually suitable for wet environments caused by blood and body fluids) have gradually replaced traditional sutures and tissue fixation nails to strongly adhere to tissues to achieve wound closure or sealing.

[0003] Medical wet adhesives that have been clinically approved in the past few decades include bio-based materials, cyanoacrylates, and polymer hydrogels. Among them, hydrogel medical wet adhesives are called bioadhesive hydrogels because of their inherent tissue adhesion. Compared with other wet adhesives, bioadhesive hydrogels have been widely studied because of their biological tissue structure, strong tissue adhesion, easy availability, adjustable mechanical properties, and good biocompatibility. Cited by Taboada GM, Yang KS, Pereira MJN, et al. Overcoming the translational barriers of tissue adhesives Nature Reviews Materials. 5(4), 310-329 (2020). However, most hydrogel medical wet adhesives have inherent limitations, including slow adhesion formation and lack of triggerable benign detachment. For example, Xie et al. first synthesized a hyperbranched polymer named HB-PBAE through the Michael addition reaction between dopamine (DOPA), poly (ethylene glycol) diacrylate (PEGDA 700) and pentaerythritol triacrylate (PETA). Then, HB-PBAE, poly(1-vinylimidazole) (PVI), gelatin and Fe 3+ To prepare DOPA-based adhesive hydrogel, although the adhesive reduces the probability of damage caused by wound replacement, the process of adhesion formation is relatively slow, and the stability and strength of long-term adhesion need to be considered, cited by Xie T, Ding J, Han XX et al., Wound dressing changefacilitated by spraying zinc ions. Mater. Horiz. 7,605-614 (2020).

[0004] First, in the process of realizing the specific functions of wet adhesive materials, the modification process of raw materials is relatively complicated. In addition, in the process of material application, most commercially available wet adhesive materials have inherent defects such as long adhesion formation time, weak tissue bonding ability, mismatched mechanical properties, low biocompatibility or inability to benignly detach.

[0005] In order to overcome the defects of the above-mentioned existing materials, the present invention provides a disulfide wet adhesive patch and its preparation method and application, which realize the simplification of the modification process and purification method of the raw materials, the rapid adhesion to the moist tissue surface or wound to form a tough adhesive film, the wet adhesive that can be separated from the adhered tissue surface or wound without damage as needed, and the further optimization of the existence form of the wet adhesive material, to obtain an extracellular matrix-like nanofiber membrane, and conduct practical application tests. Summary of the invention

[0006] In order to obtain an ideal medical wet adhesive hydrogel, the present invention provides a method for preparing a composite hydrogel containing a cleavable functional monomer, and endows the wet adhesive material with a new structural feature and a unique adhesion mechanism, that is, the composite hydrogel with a semi-interpenetrating network structure removes interfacial water from the wet tissue surface, and in a short time range, the wet adhesive hydrogel produces instant physical crosslinking. In the long term, the cleavable functional monomers in the wet adhesive hydrogel form covalent crosslinks with the surface of biological tissues, further improving the stability and strength of long-term adhesion. Secondly, the wet adhesive hydrogel can meet different trigger separation requirements on different time scales, and can immediately dissociate and replace the wrongly positioned wet adhesive hydrogel after adhesion, or trigger separation in a wide time range in an efficient, biocompatible and non-secondary wound damage manner. Finally, the electrospinning technology is used to give the wet adhesive material a nanofiber structure similar to the extracellular matrix, which is easier for cell growth and tissue repair.

[0007] The preparation method is as follows: using disulfide monomer, 4-dimethylaminopyridine (DMAP), hydroxyethyl methacrylate (HEMA), N-hydroxysuccinimide (NHS) and 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) as raw materials to obtain disulfide functional monomers, and using polyvinyl alcohol 1788 (PVA), photoinitiator, crosslinker and disulfide functional monomers as raw materials to obtain a wet adhesion hydrogel with disulfide functional monomers. Compared with the existing technology, the wet adhesion hydrogel has the ability to trigger separation on different time scales, so that it can dissociate and replace the mispositioned wet adhesion hydrogel immediately after adhesion, or trigger separation in a wide time range (within minutes to hours) in an efficient, biocompatible and secondary wound-free manner.

[0008] A method for preparing a disulfide wet adhesive patch, wherein the disulfide wet adhesive patch comprises a wet adhesive hydrogel or a wet adhesive electrospun film;

[0009] The preparation process of wet adhesion hydrogel is as follows:

[0010] 1) dissolving the first crosslinking agent in water at 25-150°C (preferably 40-100°C, more preferably 60-80°C); adding acrylic acid, a photoinitiator and a second crosslinking agent to the mixed solution, stirring until completely dissolved, to obtain a stock solution;

[0011] The first cross-linking agent may be one or more of polyvinyl alcohol 1788, polyethylene oxide, polyacrylic acid, polyvinyl pyrrolidone, polyethylene imine, polyacrylamide, polyethylene glycol, polyvinyl butyral, cellulose, ethyl cellulose, and zein;

[0012] The second cross-linking agent may be one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, methylenebis(o-chloroaniline), p-quinonedioxime, poly(ethylene glycol) methacrylate, poly(ethylene glycol) dimethacrylate, diisocyanate, bismaleimide and triallyl isocyanate;

[0013] 2) dissolving the NHS ester functionalized monomer having a disulfide bond in acetone, and adding the monomer to the stock solution and stirring to obtain a precursor solution;

[0014] Placing the precursor solution on a flat plate mold or between two transparent molds stacked one above the other at a desired distance from each other, and curing it under ultraviolet light to obtain a wet-adhesive hydrogel having disulfide functional monomers;

[0015] Alternatively, the wet adhesion electrospun film preparation process is as follows:

[0016] 1) dissolving polyvinyl alcohol 1788 (PVA) in water at 25-150°C (preferably 40-100°C, more preferably 60-80°C); adding polyacrylic acid, benzophenone and poly(ethylene glycol) dimethacrylate to the mixed solution and stirring until completely dissolved;

[0017] 2) dissolving the NHS ester functionalized monomer having a disulfide bond in acetone, and adding it to the above stock solution and stirring to obtain a precursor solution; electrospinning the precursor solution to obtain a nanofiber membrane, and then UV curing it to obtain a nanofiber membrane having a disulfide functional monomer.

[0018] Preparation of wet adhesion hydrogels:

[0019] The mass percentage of the first cross-linking agent in the stock solution of step (1) is 2 to 40 wt % (preferably 5 to 20 wt %, more preferably 7 to 14 wt %);

[0020] The mass percentage of the acrylic acid in the stock solution of step (1) is 7 to 60 wt % (preferably 10 to 40 wt %, more preferably 14 to 35 wt %);

[0021] The photoinitiator in the stock solution of step (1) may be one or more of 2-hydroxy-2-methylpropiophenone (1173), dialkoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, α-ketoglutaric acid, benzophenone, 4-methylbenzophenone, and 2,4,6-trimethylbenzophenone;

[0022] The mass percentage of the photoinitiator is 0.01 to 15 wt% (preferably 0.1 to 10 wt%, more preferably 0.1 to 1 wt%);

[0023] The mass percentage of the second cross-linking agent in the stock solution of step (1) is 0.01-1.5 wt % (preferably 0.01-1 wt %, more preferably 0.01-0.1 wt %);

[0024] Or, during the preparation of wet adhesion electrospun films:

[0025] The mass percentage of polyvinyl alcohol 1788 (PVA) in step (1) is 1-50 wt% (preferably 5-30 wt%, more preferably 5-20 wt%);

[0026] The mass percentage of the polyacrylic acid in step (1) is 1 to 50 wt % (preferably 5 to 30 wt %, more preferably 5 to 20 wt %);

[0027] The photoinitiator in step (1) may be one or more of 2-hydroxy-2-methylpropiophenone (1173), dialkoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, α-ketoglutaric acid, benzophenone, 4-methylbenzophenone, and 2,4,6-trimethylbenzophenone;

[0028] The mass percentage of the photoinitiator in step (1) is 0.01-20 wt% (preferably 0.01-5 wt%, more preferably 0.1-2 wt%);

[0029] The cross-linking agent in step (1) may be one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (AD), methylenebis(o-chloroaniline) (MOCA), quinonedioxime (QO), poly(ethylene glycol) methacrylate, poly(ethylene glycol) dimethacrylate, diisocyanate, bismaleimide and triallyl isocyanate;

[0030] The mass percentage of the cross-linking agent in step (1) is 0.01-30 wt % (preferably 0.1-15 wt %, more preferably 1-10 wt %).

[0031] Preparation of wet adhesion hydrogels:

[0032] When the volume of the stock solution in step 1) is 5-30 mL, the mass of the NHS ester functionalized monomer having a disulfide bond in step (2) is 5-1000 mg (preferably 25-500 mg, more preferably 25-300 mg); the volume of acetone in step (2) is 0.1-10 mL (preferably 0.5-5 mL, more preferably 0.5-3 mL);

[0033] The prepared disulfide wet adhesive patch has a thickness of 0.01 to 5 mm (preferably 0.1 to 3 mm, more preferably 0.5 to 2 mm);

[0034] Or, during the preparation of wet adhesion electrospun films:

[0035] When the volume of the stock solution in step 1) is 5-30 mL, the mass of the functional monomer of the disulfide in step (2) is 5-1000 mg (preferably 25-500 mg, more preferably 25-300 mg); the volume of acetone in step (2) is 0.1-10 mL (preferably 0.5-5 mL, more preferably 0.5-3 mL);

[0036] In step (2), the precursor solution is placed in a syringe with a metal needle, the metal needle is connected to the positive electrode, the receiving plate is used as the negative electrode, and then the distance between the two electrodes is fixed, and then high voltage is applied; at the same time, the propeller speed is set to push the syringe, and the nanofiber membrane is obtained by electrospinning.

[0037] The volume of the syringe in step (2) is 1 to 50 mL (preferably 5 to 20 mL, more preferably 5 to 10 mL);

[0038] The inner diameter of the metal needle of the syringe in step (2) is 0.1-5 mm (preferably 0.5-3 mm, more preferably 0.5-1 mm);

[0039] Preferably, the distance between the two poles in step (2) is 5 to 30 cm (preferably 5 to 20 cm, more preferably 8 to 12 cm);

[0040] Preferably, the high voltage in step (2) is 3-50 kV (preferably 5-30 kV, more preferably 5-20 kV);

[0041] Preferably, the propeller speed in step (2) is set to 0.01-5 mL / h (preferably 0.1-3 mL / h, more preferably 0.1-1 mL / h);

[0042] The thickness of the prepared disulfide wet-adhesive nanofiber membrane is 0.01-2 mm (preferably 0.1-1 mm, more preferably 0.1-0.5 mm).

[0043] During the preparation of wet-adhesive hydrogels or wet-adhesive electrospun films;

[0044] The stirring rate in step (1) is 10-5000 rpm, and the time is 1-120 min (preferably 100-2000 rpm, and the time is 5-60 min, more preferably 600-1000 rpm, and the time is 5-30 min);

[0045] The stirring rate in step (2) is 10-5000 rpm, and the time is 1-120 min (preferably 100-2000 rpm, and the time is 5-60 min, more preferably 600-1000 rpm, and the time is 5-30 min);

[0046] In the preparation process of the wet adhesion hydrogel: the instrument used for the UV curing in step (2) is a SCIENTZ03-II UV cross-linking instrument, and the UV cross-linking instrument used in step (2) has a light curing time of 5 to 120 min (preferably 10 to 60 min, more preferably 15 to 30 min);

[0047] Or, in the preparation process of the wet adhesion electrospinning film: the instrument used for the ultraviolet light curing in step (2) is a SCIENTZ03-II type ultraviolet cross-linking instrument; the light curing time of the ultraviolet cross-linking instrument used in step (2) is 15~45 min.

[0048] The method for preparing the NHS ester functionalized monomer having a disulfide bond comprises the following steps:

[0049] 1) Mixing and stirring the disulfide monomer and acetic anhydride until they are completely dissolved, and then concentrating to remove unreacted acetic anhydride;

[0050] 2) 4-Dimethylaminopyridine (DMAP) and hydroxyethyl methacrylate (HEMA) were dissolved in dichloromethane (DCM) and stirred at room temperature to allow DMAP to activate the hydroxyl groups in HEMA;

[0051] 3) Dissolve the product obtained in step (1) in anhydrous DCM and transfer it to the mixed solution of step (2), stirring for 5 to 60 min;

[0052] 4) adding a saturated sodium bicarbonate (NaHCO3) solution to maintain the steady-state structure of the product of step (3), acidifying the mixture with hydrochloric acid (HCl) to a pH of less than or equal to 2.0, and extracting with DCM; drying the organic phase over anhydrous sodium sulfate (Na2SO4), filtering and concentrating it to a thick oil, and then purifying the crude product through a silica gel chromatography column using a mixture of methanol (MeOH) and DCM as an eluent, and finally concentrating it to a thick oil;

[0053] 5) The oily liquid obtained in step (4) was then dissolved in anhydrous DCM and stirred with N-hydroxysuccinimide (NHS) in an ice bath;

[0054] 6) Add 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride (EDC) dissolved in anhydrous DCM dropwise into the above mixture and stir magnetically under nitrogen atmosphere at room temperature for 5-60 min;

[0055] 7) The mixed solution is added dropwise into petroleum ether as a precipitant to obtain white floccules, which are then washed with water, filtered and dried to obtain a powdery disulfide functional monomer.

[0056] The disulfide monomer in step (1) may be one or more of diphenyl disulfide, dimethyl disulfide, 3-carboxypropyl disulfide, dithioglycolic acid and cystine;

[0057] Preferably, the final concentration of the disulfide monomer in step (1) is 1×10 -3 ~5×10 -2 mol / L (preferably 2×10 -3 ~3×10 -2 mol / L, more preferably 5×10 -3 ~2×10 -2 mol / L).

[0058] The volume of acetic anhydride in step (1) is 3 to 50 mL (preferably 5~30 mL, more preferably 5 to 15 mL);

[0059] The stirring rate in step (1) is 10-1000 rpm for 0.5-10 h (preferably 200-600 rpm for 2-6 h, more preferably 400-600 rpm for 3-4 h);

[0060] The mass of 4-dimethylaminopyridine (DMAP) in step (2) is 0.01-3 g (preferably 0.01-1 g, more preferably 0.01-0.03 g);

[0061] The final concentration of hydroxyethyl methacrylate (HEMA) in step (2) is 1×10 -3 ~5×10 -2 mol / L (preferably 2×10 -3 ~3×10 -2 mol / L, more preferably 5×10 -3 ~2×10 -2 mol / L);

[0062] The volume of anhydrous dichloromethane (DCM) in step (2) is 5 to 50 mL (preferably 5~30 mL, preferably 8-20 mL);

[0063] The stirring rate in step (2) is 10-1000 rpm, and the time is 0.5-10 h (preferably 200-600 rpm, and the time is 2-6 h, more preferably 300-600 rpm, and the time is 0.5-2 h);

[0064] The volume of anhydrous DCM in step (3) is 5 to 50 mL (preferably 5~30 mL, preferably 8-20 mL);

[0065] The stirring rate in step (3) is 10-1000 rpm for 6-48 h (preferably 200-600 rpm for 10-24 h, more preferably 300-600 rpm for 12-18 h);

[0066] The volume of saturated sodium bicarbonate (NaHCO3) in step (4) is 5-100 mL (preferably 10~60 mL, preferably 20-30 mL);

[0067] The concentration of hydrochloric acid (HCl) in step (4) is 0.01~10 mol / L (preferably 0.1~5 mol / L, more preferably 1~3 mol / L);

[0068] The volume of methanol (MeOH) and DCM as eluent in step (4) is 1:1-500 (preferably 1:1-300, more preferably 1:1-20)

[0069] The volume of anhydrous DCM in step (5) is 5 to 100 mL (preferably 10~60 mL, preferably 20-30 mL);

[0070] The final concentration of N-hydroxysuccinimide (NHS) in step (5) is 1×10 -3 ~5×10 -2 mol / L (preferably 2×10 -3 ~3×10-2 mol / L, more preferably 5×10 -3 ~2×10 -2 mol / L);

[0071] The stirring rate in step (5) is 10-1000 rpm, and the time is 0.5-10 h (preferably 200-600 rpm, and the time is 2-6 h, more preferably 300-600 rpm, and the time is 0.5-2 h);

[0072] The volume of anhydrous DCM in step (6) is 5 to 100 mL (preferably 10~60 mL, preferably 20-30 mL);

[0073] The final concentration of 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride (EDC) in step (6) is 1×10 -3 ~5×10 -2 mol / L (preferably 2×10 -3 ~3×10 -2 mol / L, more preferably 5×10 -3 ~2×10 -2 mol / L);

[0074] The stirring rate in step (6) is 10-1000 rpm for 6-48 h (preferably 200-600 rpm for 10-24 h, more preferably 300-600 rpm for 12-18 h);

[0075] The volume of petroleum ether in step (7) is 100-2000 mL (preferably 200-1000 mL, more preferably 300-500 mL);

[0076] The volume of water in step (7) is 100-2000 mL (preferably 200-1000 mL, more preferably 300-500 mL);

[0077] The conditions for water washing in step (7) are ultrasonic treatment for 5 min to 10 h (preferably 15 min to 5 h, more preferably 30 min to 2 h).

[0078] A disulfide wet adhesive patch prepared by the preparation method.

[0079] The wet adhesive patch is adhered to the surface of a wet biological tissue or organ (preferably an isolated tissue or organ).

[0080] The triggered separation process of the wet adhesive patch adhered to the wet tissue and organ surface from the biological tissue surface is as follows: wet-apply or apply the triggering solution to the wet adhesive hydrogel adhered to the biological tissue surface (preferably an isolated tissue and organ), and after standing for 5 to 45 minutes, the triggered wet adhesive hydrogel can be peeled off;

[0081] The trigger solution contained sodium bicarbonate (SBC) and glutathione (reduced form) (GSH) dissolved in phosphate buffered saline (PBS); the concentration of the sodium bicarbonate (SBC) was 5×10 -3 ~50 mol / L (preferably 5×10 -2 ~30 mol / L, more preferably 5×10 -1 ~10 mol / L); the concentration of glutathione (reduced form) is 5×10 -3 ~10 mol / L (preferably 5×10 -2 ~5mol / L, more preferably 5×10 -2 ~1 mol / L); the phosphate buffer (PBS concentration is 1×10 -2 ~10 mol / L (preferably 1×10 -2 ~1 mol / L, more preferably 1×10 -1 ~1 mol / L), PH=4.0~12.0 (preferably 5.0~10.0, more preferably 6.0~8.0).

[0082] The purpose of the present invention can be achieved by the following preferred technical solutions:

[0083] The first object of the present invention is to provide a method for preparing a disulfide functional monomer, comprising the following steps:

[0084] (1) The disulfide monomer and acetic anhydride were added to a round-bottom flask equipped with a magnetic stirring bar and magnetically stirred at room temperature until they were completely dissolved. Then, the unreacted acetic anhydride was removed by vacuum.

[0085] (2) 4-Dimethylaminopyridine (DMAP) and hydroxyethyl methacrylate (HEMA) were dissolved in anhydrous dichloromethane (DCM) and magnetically stirred at room temperature to allow DMAP to activate the hydroxyl groups in HEMA.

[0086] (3) Dissolve the product obtained in step (1) in anhydrous DCM and slowly transfer it to the mixed solution of step (2), and stir magnetically overnight.

[0087] (4) Saturated sodium bicarbonate (NaHCO3) solution was added to complete the reaction of step (3), and the mixture was acidified to pH = 2.0 with hydrochloric acid (HCl), and extracted with DCM. The organic phase was dried over anhydrous sodium sulfate (Na2SO4), filtered and concentrated in vacuo, and the crude product was eluted with a mixture of methanol (MeOH) and DCM through a silica gel chromatography column ( Figure 1 ) and finally concentrated in vacuo.

[0088] (5) The oily liquid obtained in step (4) was then dissolved in anhydrous DCM and stirred with N-hydroxysuccinimide (NHS) in an ice bath.

[0089] (6) 1-Ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) dissolved in anhydrous DCM was added dropwise to the above mixture and stirred magnetically under nitrogen atmosphere at room temperature overnight.

[0090] (7) The mixed solution is added dropwise into petroleum ether as a precipitant to obtain a white flocculent, which is then washed with ultrapure water, filtered and dried to obtain a powdery disulfide functional monomer.

[0091] Preferably, the disulfide monomer in step (1) can be diphenyl disulfide, dimethyl disulfide, 3-carboxypropyl disulfide, dithioglycolic acid and cystine;

[0092] Further preferably, the concentration of the disulfide monomer in step (1) is 5×10 -3 ~2×10 -2 mol / L;

[0093] Preferably, the volume of acetic anhydride in step (1) is 5 to 30 mL;

[0094] Further preferably, the stirring rate in step (1) is 200-600 rpm and the time is 2-6 h.

[0095] Preferably, the apparatus used for vacuum removal of the solvent in step (1) is a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump;

[0096] More preferably, the cooling temperature of the rotary evaporation is -20°C, the water bath heating temperature is 30-60°C, and the rotation speed is 30-120 r / min.

[0097] Preferably, the mass of 4-dimethylaminopyridine (DMAP) in step (2) is 0.01-0.03 g;

[0098] Preferably, the concentration of hydroxyethyl methacrylate (HEMA) in step (2) is 5×10 -3 ~2×10 -2 mol / L;

[0099] Preferably, the volume of anhydrous dichloromethane (DCM) in step (2) is 8 to 20 mL;

[0100] Further preferably, the stirring rate in step (2) is 300-600 rpm and the time is 0.5-2 h.

[0101] Preferably, the volume of anhydrous DCM in step (3) is 8 to 20 mL;

[0102] Further preferably, the stirring rate in step (3) is 300-600 rpm and the time is 12-18 h.

[0103] Preferably, the volume of saturated sodium bicarbonate (NaHCO3) in step (4) is 20-60 mL;

[0104] Preferably, the concentration of hydrochloric acid (HCl) in step (4) is 1 to 10 mol / L;

[0105] Preferably, the apparatus used for vacuum concentration in step (4) is a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump;

[0106] More preferably, the cooling temperature of the rotary evaporation is -20°C, the water bath heating temperature is 30-60°C, and the rotation speed is 30-120 r / min.

[0107] Preferably, the volume ratio of methanol (MeOH) and DCM used as eluents in step (4) is 1:500 to 1:20.

[0108] Preferably, the volume of anhydrous DCM in step (5) is 10 to 40 mL;

[0109] Preferably, the concentration of N-hydroxysuccinimide (NHS) in step (5) is 5×10 -3 ~2×10 -2 mol / L;

[0110] Further preferably, the stirring rate in step (5) is 300-600 rpm and the time is 0.5-2 h.

[0111] Preferably, the volume of anhydrous DCM in step (6) is 5 to 20 mL;

[0112] Preferably, the concentration of 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride (EDC) in step (6) is 5×10 -3 ~2×10 -2 mol / L;

[0113] Further preferably, the stirring rate in step (6) is 300-600 rpm and the time is 12-18 h.

[0114] Preferably, the volume of petroleum ether in step (7) is 300-500 mL;

[0115] Preferably, the ultrapure water in step (7) is derived from a ULUP-IV-20TE ultrapure water machine;

[0116] Further preferably, the volume of the ultrapure water in step (7) is 300-500 mL;

[0117] Further preferably, the ultrapure water washing in step (7) is carried out under ultrasonic treatment for 30 min to 2 h.

[0118] The second object of the present invention is to provide a method for gelling the disulfide functional monomer prepared by the above preparation method, comprising the following steps:

[0119] Under heating conditions, the first crosslinking agent is dissolved in deionized water. Acrylic acid, photoinitiator and second crosslinking agent are added to the mixed solution in sequence, and stirred magnetically until completely dissolved.

[0120] Then, the functional monomer with disulfide is dissolved in acetone and added to the above stock solution and stirred magnetically to obtain a precursor solution. The precursor solution is injected into a glass mold with a certain spacing ( Figure 2 ) and cured under UV light to obtain a wet-adhesive hydrogel with disulfide functional monomers.

[0121] Preferably, the heating temperature in step (1) is 60-80°C;

[0122] Preferably, in step (1), the first cross-linking agent may be polyvinyl alcohol 1788 (PVA), polyethylene oxide, polyacrylic acid, polyvinyl pyrrolidone, polyethylene imine, polyacrylamide, polyethylene glycol, polyvinyl butyral, cellulose, ethyl cellulose, or zein.

[0123] Further preferably, in step (1), the mass percentage of the first cross-linking agent is 7-14 wt %;

[0124] Preferably, the mass percentage of acrylic acid in step (1) is 14-35 wt %;

[0125] Preferably, the photoinitiator in step (1) can be 2-hydroxy-2-methylpropiophenone (1173), dialkoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, α-ketoglutaric acid, benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone;

[0126] Further preferably, the mass percentage of the photoinitiator in step (1) is 0.1-1 wt %;

[0127] Preferably, in step (1), the second cross-linking agent may be 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (AD), methylenebis(o-chloroaniline) (MOCA), quinonedioxime (QO), poly(ethylene glycol) methacrylate, poly(ethylene glycol) dimethacrylate, diisocyanate, bismaleimide and triallyl isocyanate;

[0128] Further preferably, the mass percentage of the cross-linking agent in step (1) is 0.01-0.1wt%;

[0129] Further preferably, the stirring rate in step (1) is 600-1000 rpm and the time is 5-30 min.

[0130] Preferably, the mass of the NHS ester functionalized monomer having a disulfide bond in step (2) is 25-300 mg;

[0131] Preferably, the volume of acetone in step (2) is 0.5-3 mL;

[0132] Preferably, the instrument used for UV curing in step (2) is a SCIENTZ03-II UV cross-linking instrument;

[0133] Further preferably, the UV cross-linking device used in step (2) is used for photocuring for 15 to 30 minutes.

[0134] Further preferably, the stirring rate in step (1) is 600-1000 rpm and the time is 5-30 min.

[0135] The third object of the present invention is to provide an application of the wet adhesive hydrogel, wherein the dry wet adhesive patch is used for rapid hemostasis and repair of moist tissue and organ surfaces, and the components of the hydrogel in the adhesive layer of the wet adhesive patch (after contacting water) will form covalent bonds and hydrogen bonds at the junction when encountering the moist tissue surface, so as to achieve the purpose of tight adhesion and firm bonding.

[0136] A fourth object of the present invention is to provide a biocompatible triggered separation of the wet adhesion hydrogel ( Figure 3 ), since the adhesion mechanism of wet adhesion hydrogel relies on first removing the interfacial water on the wet biological tissue surface and then physically and covalently cross-linking with the tissue surface, triggerable separation requires the use of a trigger solution to cut off the cross-linking force between the wet adhesion hydrogel and the biological tissue surface. The configuration method of the trigger solution is as follows:

[0137] A certain amount of sodium bicarbonate (SBC) and glutathione (reduced form) (GSH) were dissolved in phosphate buffered saline (PBS), respectively.

[0138] Use a rubber-tipped dropper to take part of the trigger solution and apply it to the wet-adhesive hydrogel that has adhered to the surface of the biological tissue. After standing, use tweezers to peel off the triggered wet-adhesive hydrogel.

[0139] Preferably, the concentration of sodium bicarbonate (SBC) in step (1) is 5×10 -1 ~10 mol / L;

[0140] Preferably, the concentration of glutathione (reduced form) in step (1) is 5×10 -2 ~1 mol / L;

[0141] Preferably, the concentration of the phosphate buffer (PBS) in step (1) is 1×10 -2 ~1 mol / L, PH=6.0~8.0.

[0142] Preferably, the standing time in step (2) is 5 to 45 min.

[0143] The wet adhesive patch exists in various forms. That is to say, the process of forming a hydrogel by UV curing in the second invention purpose in the technical solution can be improved to transform the original hydrogel form into an electrospinning film, but the formula of the precursor solution needs to be fine-tuned. The specific formula is as follows:

[0144] Under heating conditions, polyvinyl alcohol 1788 (PVA) was dissolved in deionized water. Polyacrylic acid, benzophenone and poly (ethylene glycol) dimethacrylate were added to the mixed solution in sequence and stirred magnetically until completely dissolved.

[0145] The disulfide functional monomer is then dissolved in acetone and added to the above stock solution for magnetic stirring to obtain a precursor solution. The precursor solution is placed in a syringe with a metal needle, the metal needle is connected to the positive electrode, the receiving plate is used as the negative electrode, and then the distance between the two electrodes is fixed, and then high voltage is applied. At the same time, the propeller speed is set to push the syringe, and a nanofiber membrane is obtained by electrospinning, and then after UV curing, a nanofiber membrane with a disulfide functional monomer is obtained.

[0146] Preferably, the heating temperature in step (1) is 60-80°C;

[0147] Preferably, the mass percentage of polyvinyl alcohol 1788 (PVA) in step (1) is 5-20 wt %;

[0148] Preferably, the mass percentage of the polyacrylic acid in step (1) is 5-20 wt %;

[0149] Preferably, the photoinitiator in step (1) can be 2-hydroxy-2-methylpropiophenone (1173), dialkoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, α-ketoglutaric acid, benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone;

[0150] Further preferably, the mass percentage of the photoinitiator in step (1) is 0.1-2 wt %;

[0151] Preferably, the cross-linking agent in step (1) may be 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (AD), methylenebis(o-chloroaniline) (MOCA), quinonedioxime (QO), poly(ethylene glycol) methacrylate, poly(ethylene glycol) dimethacrylate, diisocyanate, bismaleimide and triallyl isocyanate;

[0152] Further preferably, the mass percentage of the cross-linking agent in step (1) is 1-10wt%;

[0153] Further preferably, the stirring rate in step (1) is 600-1000 rpm and the time is 5-30 min.

[0154] Preferably, the mass of the functional monomer of the disulfide in step (2) is 25-300 mg;

[0155] Preferably, the volume of acetone in step (2) is 0.5-3 mL.

[0156] Preferably, the volume of the syringe in step (2) is 5 to 20 mL;

[0157] Further preferably, the inner diameter of the metal needle of the syringe in step (2) is 0.5-1 mm.

[0158] Preferably, the distance between the two poles in step (2) is 5 to 30 cm;

[0159] Preferably, the high voltage in step (2) is 5-20 kV;

[0160] Preferably, the propeller speed in step (2) is set to 0.1-2 mL / h.

[0161] Preferably, the instrument used for UV curing in step (2) is a SCIENTZ03-II UV cross-linking instrument;

[0162] Further preferably, the photocuring time of the UV cross-linking device used in step (2) is 15 to 45 minutes.

[0163] The present invention forms adhesion force by means of physical crosslinking and covalent crosslinking between the wet adhesion hydrogel and the wet biological tissue surface. The contribution of these two bonding modes to the adhesion force at different time scales is quite different. Specifically, in the time range of 30 s to 10 min (short term), the semi-interpenetrating network structure composed of cleavable disulfide functional monomers and polyvinyl alcohol 1788 (PVA) and polyacrylic acid (PAA) will first remove interfacial water from the wet tissue surface, so that the wet adhesion hydrogel has the ability of immediate physical crosslinking (such as hydrogen bonding and van der Waals force) and plays a leading role in the adhesion between the wet adhesion hydrogel and the wet biological tissue surface. However, as time goes by, due to the equilibrium state generated by the gradual neutralization of the carboxylic acid groups in the wet adhesion hydrogel, the contribution of physical crosslinking to adhesion gradually decreases, weakening the physical crosslinking force formed between the wet adhesion hydrogel and the wet biological tissue surface. Therefore, over a long period of time, the cleavable disulfide functional monomers in the wet adhesion hydrogel will form covalent cross-linking (such as amide bonds) forces with the primary amine groups on the surface of biological tissues, and gradually deepen the degree of adhesion contribution to the surface of biological tissues, further improving the stability and strength of long-term adhesion. In addition, the wet adhesion hydrogel can meet different triggering separation requirements on different time scales, enabling it to re-dissociate and replace the wrongly positioned wet adhesion hydrogel immediately after adhesion or trigger separation in an efficient, biocompatible and non-secondary wound-injury manner over a wide time range (minutes to hours).

[0164] Compared with the prior art, the technical problems to be solved by the present invention are mainly to simplify the modification and purification methods of functional monomers, accelerate the adhesion formation speed of wet adhesive patches, enhance the flexibility and mechanical properties of wet adhesive patches, separate from the adhered tissue surface or wound on demand without secondary damage, and optimize the structural morphology and existence form of wet adhesive materials to obtain extracellular matrix-like nanofiber membranes. The beneficial effects obtained by the present invention are as follows:

[0165] The present invention simplifies the modification and purification process of the cleavable functional monomer, saves the process cost of the pilot scale-up and other conversion processes, and is easier to successfully convert in the actual application process.

[0166] The wet adhesion hydrogel of the present invention can achieve instant (5 s to 30 s) super-strong adhesion on a variety of wet dynamic tissue surfaces, and can achieve beneficial on-demand separation by using a biocompatible trigger solution.

[0167] The adhesion mechanism of the wet adhesion hydrogel of the present invention relies on removing the interfacial water on the wet biological tissue surface and then physically and covalently cross-linking with the tissue surface, further improving the stability and strength of long-term adhesion.

[0168] The wet adhesive hydrogel of the present invention can be transformed into a tough hydrogel having mechanical compliance and stretchability comparable to that of soft tissue after contacting with a wet biological tissue surface.

[0169] The present invention adopts electrostatic spinning technology to optimize the structure of the wet adhesive patch so that it has a nanofiber structure similar to the extracellular matrix, which is beneficial to cell growth and tissue repair.

[0170] The present invention uses an isolated chicken heart to verify the wet adhesion hydrogel and the triggering solution, proving that the hydrogel has a triggerable benign detachment ability.

[0171] The present invention simplifies a modification and purification method of a cleavable disulfide functional monomer, and provides a preparation method of a wet adhesive patch containing the functional monomer, which gives it a unique adhesion mechanism, that is, by means of physical crosslinking and covalent crosslinking between the wet adhesive water patch and the wet biological tissue, in a short time range (30 s~10 min), the semi-interpenetrating network structure composed of the cleavable disulfide functional monomer and polyvinyl alcohol 1788 (PVA) and polyacrylic acid (PAA) produces instant physical crosslinking. In the long term, the cleavable disulfide functional monomer in the wet adhesive patch will form covalent crosslinks with the surface of the biological tissue, further accelerating the adhesion formation speed of the wet adhesive patch and improving its toughness and mechanical properties. In addition, the wet adhesive patch can meet different trigger separation requirements on demand at different time scales, so as to adjust the adhesion position in real time, or meet the trigger separation requirements of high efficiency, biocompatibility and no secondary damage in a wider time range. Finally, electrospinning technology was used to further optimize the structural characteristics of the wet adhesion material to make it more beneficial to cell growth and tissue repair, and corresponding practical application tests were carried out. BRIEF DESCRIPTION OF THE DRAWINGS

[0172] Figure 1 The present invention provides a schematic diagram of the structure of a silica gel chromatography column, which is filled with 200-300 mesh column chromatography silica gel. In the figure, 1 is medical absorbent cotton, 2 is quartz sand (SiO2, 40-80 mesh), 3 is a DCM+MeOH mixed solution containing column chromatography silica gel (200-300 mesh), and 4 is 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid to be purified.

[0173] Figure 2 A schematic diagram of a light-cured glass mold for a wet-adhesive hydrogel containing a disulfide functional monomer provided by the present invention.

[0174] Figure 3 Schematic diagram of wet adhesion and triggered separation of the disulfide wet adhesion patch provided by the present invention.

[0175] Figure 4 This is a nuclear magnetic resonance test image of the disulfide functional monomer provided by the present invention, and illustration i is a white powdery disulfide functional monomer. DETAILED DESCRIPTION

[0176] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0177] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed as common technical features disclosed in the prior art.

[0178] In the present invention, the main functional component of the wet adhesive patch having disulfide functional monomers is [-C 14 H 18 O8NS2-] n .

[0179] In the present invention, the raw materials used in the preparation are: dithioglycolic acid (C4H6O4S2, 96%), hydroxyethyl methacrylate (HEMA, C6H 10 O3, 96%), benzophenone (C 13 H 10 O, AR), 2-hydroxy-2-methylpropiophenone (1173, C 10 H 12 O2, 97%) and 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride (EDC, C8H 18 ClN3, 98%) was purchased from Shanghai Roen Chemical Technology Co., Ltd.; acetic anhydride ((CH3CO)2O, 98.5%) was purchased from Tianjin Jindong Tianzheng Fine Chemical Reagent Factory; anhydrous dichloromethane (DCM, CH2Cl2, 99.9%, water <30 ppm) was purchased from Adamas Reagent Co., Ltd.; petroleum ether (30 ℃~60 ℃), acetone (CH3COCH3, 99.5%), sodium bicarbonate (SBC, NaHCO3, 99.5%), quartz sand (SiO2, 40-80 mesh, 99%), anhydrous sodium sulfate (Na2SO4, 99%), hydrochloric acid (HCl, 36%-38%), disodium hydrogen phosphate (Na2HPO4, 99.5%) and sodium dihydrogen phosphate (NaH2PO4, 99.5%) were purchased from Tianjin Komiou Chemical Reagent Co., Ltd.; methanol (MeOH, CH3OH, 99.5%), acrylic acid (C3H4O2, 99%), column chromatography silica gel (200-300 mesh 54-75 μm), 4-dimethylaminopyridine (DMAP, C7H 10 N2, 99%), poly(ethylene glycol) methacrylate (H2C=C(CH3)CO(OCH2CH2) n OH, average molecular weight ~500), N-hydroxysuccinimide (NHS, C4H5NO3, 98%), polyacrylic acid ((C3H4O2) n , average molecular weight ~450000), polyvinyl alcohol 1788 type (PVA, [-CH2CHOH-] n , alcoholysis degree: 87~89%) and glutathione (reduced form) (GSH, C 10 H 17N3O6S, 98%) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; poly(ethylene glycol) dimethacrylate (average molecular weight ~500, 99.9%) was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.; deionized water and ultrapure water were both from ULUP-IV-20TE ultrapure water machine (Sichuan Youpu Ultrapure Technology Co., Ltd.).

[0180] Example 1

[0181] This embodiment provides a method for preparing a disulfide functional monomer, comprising the following steps:

[0182] (1) The final concentration is 1×10 -2 mol / L dithioglycolic acid and 16 mL of acetic anhydride were added to a round-bottom flask equipped with a magnetic stirring bar, and magnetically stirred at 350 rpm for 3 h at room temperature to completely dissolve the mixed solution. Then, the remaining acetic anhydride was removed by vacuum using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump, wherein the cooling temperature of the rotary evaporation was -20 °C, the water bath heating temperature was 40 °C, and the rotation speed was 100 r / min. Finally, a colorless oily 1,4,5-oxadithiophene-2,7-dione was obtained.

[0183] (2) Add 0.015 g of 4-dimethylaminopyridine (DMAP) and a final concentration of 1×10 -2 mol / L hydroxyethyl methacrylate (HEMA) was dissolved in 7 mL of anhydrous dichloromethane (DCM) and magnetically stirred at 400 rpm for 0.5 h at room temperature to ensure that 4-dimethylaminopyridine (DMAP) could completely activate the hydroxyl groups in hydroxyethyl methacrylate (HEMA). Then 8 mL of anhydrous DCM was used to dissolve the colorless oil obtained in step (1) and slowly transferred to the mixed solution in step (2), maintaining a magnetic stirring time of 400 rpm for 12 h.

[0184] (3) Add 30 mL of saturated sodium bicarbonate (NaHCO3) solution was added to the mixed solution of step (2) until no bubbles were generated during stirring, so that the final product of (2) was more stable under cationic conditions. The mixture was then acidified to pH = 2.0 with 1 mol / L hydrochloric acid (HCl), and extracted with 45 mL DCM. The organic phase was then dried over anhydrous sodium sulfate (Na2SO4) to remove excess water, filtered through a sand core funnel to separate the solid and liquid, and the liquid was concentrated into a thick oily substance using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump. The cooling temperature of the rotary evaporation was -20 °C, the water bath heating temperature was 40 °C, and the rotation speed was 100 r / min. Finally, the crude product was precipitated with methanol (MeOH) and DCM ( Dichloromethane ) was used as an eluent to purify the mixture through a silica gel chromatography column, and the separation state of the product and impurities was confirmed by thin layer chromatography silica gel plate spot plate, and then a pink oily 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid was obtained after vacuum concentration, wherein the volume ratio of methanol (MeOH) to DCM was 1:20, and the instrument used for vacuum concentration was a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump. The cooling temperature of the rotary evaporation was -20 °C, the water bath heating temperature was 40 °C, and the rotation speed was 100 r / min. In addition, 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid was analyzed by 1H NMR nuclear magnetic resonance and Fourier transform infrared spectroscopy (FTIR), respectively verifying that it has the corresponding carboxylic acid structure. Figure 1 This is a schematic diagram of the structure of the silica gel chromatography column provided by the present invention, and is filled with 200-300 mesh column chromatography silica gel.

[0185] (4) Then the 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid obtained above was dissolved in 15 mL of anhydrous DCM and mixed with a final concentration of 1×10 -2 mol / L N-hydroxysuccinimide (NHS) was stirred in an ice bath at a rate of 470 rpm for 0.5 h. Then, a final concentration of 1×10 -2 1-Ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) was added dropwise to the mixture, and the mixture was stirred magnetically overnight at room temperature under a nitrogen atmosphere at a rate of 470 rpm for 12 h to obtain an orange-red mixed solution.

[0186] (5) The mixed solution was added dropwise to petroleum ether as a precipitant to obtain a white flocculent, which was then filtered and ultrasonically washed with ultrapure water for 30 min, and then filtered to remove the waste liquid and dried at room temperature to obtain a white powdery disulfide functional monomer with a yield of 83%. The volume of petroleum ether was 500 mL, and the volume of ultrapure water was 500 mL.

[0187] This embodiment provides a method for gelling a disulfide functional monomer, comprising the following steps:

[0188] (1) Polyvinyl alcohol 1788 (PVA) with a final concentration of 7 wt %, acrylic acid (35 wt %), 0.2 wt % 2-hydroxy-2-methylpropiophenone (1173), and 0.1 wt % poly(ethylene glycol) methacrylate were dissolved in deionized water under heating at 80 °C and stirred magnetically at 1000 rpm for 5 min at room temperature to obtain 5 mL of a stock solution.

[0189] (2) Dissolve 50 mg of disulfide functional monomer in 500 μL acetone and add it to the above stock solution and stir it magnetically until it is completely dissolved. The stirring rate is 100 rpm and the time is 30 min to obtain a precursor solution. Inject 200 μL of the precursor solution into a mold with a spacing of 0.34 mm between two glass slides (the thickness of the wet-adhesive hydrogel) ( Figure 2 ) and cured in a SCIENTZ03-II UV cross-linker with a wavelength of 365 nm for 30 min, and the water content was controlled to be 1-20 μL by gravimetric analysis. Finally, a wet adhesion hydrogel with disulfide functional monomers was obtained.

[0190] Figure 2 Schematic diagram of a light-cured glass mold for wet-adhesive hydrogel with disulfide functional monomers provided by the present invention. The upper and lower layers of the mold are both glass sheets with a size of (width × length) 25 × 75 mm, and the middle interlayer is a double-sided adhesive tape (dark green elongated strip) with a size of (length × width × height) 20 × 1 × 0.34 mm. The two glass sheets are staggered and overlapped with a distance of 2 mm from each other in both the length direction and the width direction, and the overlapped area is 21 × 67 mm 2 , which facilitates the subsequent separation of the mold and removal of the wet-adhered hydrogel.

[0191] The dry wet adhesive hydrogel was placed on the surface of a wet chicken heart and pressed for 5 s. The adhesive layer of the wet adhesive hydrogel quickly formed hydrogen bonds and covalent crosslinks at the junction after contacting water. The interfacial toughness between the wet adhesive hydrogel and the chicken heart was measured according to the standard test method for tissue adhesives (180° peel test, ASTM F2256-05 (2015)). When the contact and mild pressure (1 kPa) were applied for less than 5 s, the wet adhesive hydrogel could form an interfacial toughness of more than 352 J m on the chicken heart surface. −2 The strong adhesion of the wet-adhesive hydrogel was 350 J m −2 , the degree of numerical change is negligible, indicating that the wet adhesion hydrogel after adhesion behavior has long-term adhesion stability and high adhesion strength.

[0192] Figure 3 The present invention is a schematic diagram of the adhesion and separation structure between the disulfide wet adhesion patch and the wet biological tissue wetted with water, which specifically shows that the water on the surface of the biological tissue will spontaneously penetrate into the network of the hydrogel, so that the cross-linking force of hydrogen bonds and amide bonds formed at the junction of the two can quickly close the wound and the tissue to achieve the purpose of rapid hemostasis. In addition, the disulfide wet adhesion patch can prevent wound infection in time, and maintain flexibility while bearing mechanical forces, providing lasting support for wound healing, and effectively promoting the self-repair of tissues. Finally, the cross-linking force is cut off by phosphate buffer (PBS) containing sodium bicarbonate (SBC) and glutathione (reduced form) (GSH), so that the disulfide wet adhesion hydrogel can be efficiently peeled off.

[0193] This example provides a biocompatible triggered separation of the wet-adhesive hydrogel, and the configuration method of the trigger solution is as follows:

[0194] (1) Dissolve sodium bicarbonate (SBC) and glutathione (reduced form, GSH) at a final concentration of 0.5 mol / L in 0.01 M phosphate buffered saline (PBS) at pH 6.8.

[0195] (2) Use a rubber-tipped dropper to take 2 mL of the above trigger solution and drop it on a (width × length × thickness) 1 × 2 × 0.34 mm cm 2After standing for 10 min, sodium bicarbonate (SBC) will gradually destroy the hydrogen bonds between the wet adhesive hydrogels, and glutathione (reduced form, GSH) will also break the disulfide bonds. Finally, the triggered wet adhesive hydrogel can be gently peeled off with tweezers (at this time, the adhesion force is close to 0 J m −2 ).

[0196] The disulfide functional monomer in this embodiment was analyzed by 1H NMR nuclear magnetic resonance and Fourier transform infrared spectroscopy (FTIR), respectively verifying that the disulfide functional monomer has the corresponding structure of carboxylic acid and NHS ester. The 1H NMR nuclear magnetic resonance test results are as follows: Figure 4 As shown, the peak position and coverage area of ​​each absorption peak can correspond to the type of hydrogen group and the number of hydrogen nuclei that cause the absorption (see the lowercase English annotations in the spectrum for details), indicating that the functional properties of disulfide have been successfully prepared. Illustration i is a white powdery disulfide functional monomer.

[0197] A simple adhesion and triggered separation experiment was conducted on the wet adhesive patch with disulfide functional monomers in this embodiment. The obtained wet adhesive patch with disulfide functional monomers was macroscopically shown as a transparent elastomer with a certain thickness. The dried wet adhesive patch with disulfide functional monomers was cut into appropriate sizes and placed on the wet surface of the chicken heart wound. The patch can be tightly combined with the wound surface and can give the chicken heart the ability to relax and contract. A phosphate buffered saline (PBS) containing sodium bicarbonate (SBC) and glutathione (reduced form) (GSH) was wet applied to the patch adhered to the chicken heart wound surface to cut off the cross-linking force at the junction, so that the wet adhesive patch with disulfide functional monomers can be detached as a whole.

[0198] Example 2

[0199] The process and conditions are the same as in Example 1, except that:

[0200] This embodiment provides a wet adhesive patch without adding disulfide functional monomers. In contrast to the above-mentioned embodiment 1, in this embodiment, a disulfide functional monomer gelation method is fine-tuned, that is, only a stock solution is used as a precursor solution, which is injected into a glass mold with a certain spacing distance ( Figure 2 ), the specific experimental contents are as follows:

[0201] (1) Polyvinyl alcohol 1788 (PVA) with a final concentration of 7 wt %, acrylic acid (35 wt %), 0.2 wt % 2-hydroxy-2-methylpropiophenone (1173), and 0.1 wt % poly(ethylene glycol) methacrylate were dissolved in deionized water under heating at 80 °C and stirred magnetically at 1000 rpm for 5 min at room temperature to obtain 5 mL of a stock solution.

[0202] (2) Then inject 200 μL of the precursor solution into the mold with a thickness of 0.34 mm between two glass sheets ( Figure 2 ) and cured in a SCIENTZ03-II UV cross-linker with a wavelength of 365 nm for 30 min, and the water content was controlled to be 1-20 μL by gravimetric analysis. Finally, a wet adhesion hydrogel without disulfide functional monomers was obtained.

[0203] The remaining steps and conditions are the same as in Example 1.

[0204] The wet adhesive patch without disulfide functional monomer prepared by the above preparation method is still a transparent elastomer with a certain thickness. However, after being cut into appropriate sizes and placed on the wet chicken heart wound surface, the bonding force between the patch and the wound surface is about 130 J m −2 The same method was used to drop 2 mL of phosphate buffered saline (PBS) containing sodium bicarbonate (SBC) and glutathione (reduced form) (GSH) onto a 1×2 cm2 spherical surface of the chicken heart wound. 2 After standing for 10 min, the wet adhesive patch did not fall off, and its adhesion force was about 128 J m −2 .

[0205] Example 3

[0206] The process and conditions are the same as in Example 1, except that:

[0207] This embodiment provides a method for gelling a disulfide functional monomer, which includes the following steps:

[0208] (1) Polyvinyl alcohol 1788 (PVA), 7 wt% polyacrylic acid (PAA), 0.2 wt% benzophenone, and 10 wt% poly(ethylene glycol) dimethacrylate) were dissolved in deionized water at a final concentration of 7 wt% under heating at 80 °C and stirred magnetically at 1000 rpm for 5 min at room temperature to obtain 5 mL of a stock solution.

[0209] (2) Dissolve 50 mg of disulfide functional monomer in 500 μL of acetone, add it to the above stock solution and stir it magnetically until it is completely dissolved. The stirring rate is 1000 rpm and the time is 5 min to obtain a precursor solution.

[0210] (3) The precursor solution obtained in step (2) was placed in a 10 mL syringe with a metal needle with an inner diameter of 1 mm. The metal needle was connected to the positive electrode and the receiving plate was used as the negative electrode. The distance between the two electrodes was fixed at 12 cm, and a high voltage of 16 kV was applied. At the same time, the propeller speed was set to 0.2 mL / h and the spinning time was set to 6 h. The composite film containing nanofiber filaments and small droplets was observed by electron microscopy. Then, the composite film was cured for 30 min using a SCIENTZ03-II UV crosslinker with a wavelength of 365 nm to obtain a nanofiber membrane with a disulfide functional monomer having a thickness of 0.17 mm.

[0211] The dry nanofiber membrane was placed on the surface of a wet chicken heart and pressed for 5 s. The adhesion layer of the nanofiber membrane quickly formed hydrogen bonds and amide bonds at the junction after contacting water. The interfacial toughness between the wet adhesion hydrogel and the chicken heart was measured according to the standard test method for tissue adhesives (180° peel test, ASTM F2256-05 (2015)). When the contact and mild pressure (1 kPa) were applied for less than 5 s, the wet adhesion hydrogel could form an interfacial toughness of about 482 J m −2 The adhesion of the adhesive proves its ability to adhere instantly and tenaciously.

[0212] The remaining steps are the same as in Example 1.

[0213] The nanofiber membrane with disulfide functional monomers obtained by the above preparation method still exhibits strong wet adhesion ability, and the extracellular matrix-like structure of the nanofiber membrane can temporarily replicate the functions of the dermis and epidermis during wound healing and promote the complete recovery of the two tissue layers to avoid wound contraction and scar formation. In addition, compared with the hydrogel morphology, the three-dimensional network structure of the nanofiber membrane can be superimposed to form a tissue engineering scaffold, with a fiber diameter of approximately 340~1200 nm, a fiber pore size of 90~130 μm, and a highly porous matrix with a porosity of 60~90%, which is sufficient to allow and promote cell migration and proliferation. Therefore, the structure can allow cells to enter the defect space / wound bed and form soft tissue.

[0214] Example 4

[0215] This embodiment provides a method for preparing a disulfide functional monomer, comprising the following steps:

[0216] (1) The final concentration is 1×10 -3 mol / L dithioglycolic acid and 3mL of acetic anhydride were added to a round-bottom flask equipped with a magnetic stirring bar, and magnetically stirred at 10rpm for 0.5h at room temperature to completely dissolve the mixed solution. Then, the remaining acetic anhydride was removed by vacuum using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump, wherein the cooling temperature of the rotary evaporation was -20°C, the water bath heating temperature was 40°C, and the rotation speed was 100 r / min. Finally, a colorless oily 1,4,5-oxadithiophene-2,7-dione was obtained.

[0217] (2) Add 0.01 g of 4-dimethylaminopyridine (DMAP) and a final concentration of 1 × 10 -3 mol / L hydroxyethyl methacrylate (HEMA) was dissolved in 5 mL of anhydrous dichloromethane (DCM) and stirred magnetically at 10 rpm for 1 h at room temperature to ensure that 4-dimethylaminopyridine (DMAP) could completely activate the hydroxyl groups in hydroxyethyl methacrylate (HEMA). 5 mL of anhydrous DCM was then used to dissolve the colorless oil obtained in step (1) and slowly transferred to the mixed solution in step (2), and stirred magnetically at 10 rpm for 6 h.

[0218] (3) Add 5 mL of saturated sodium bicarbonate (NaHCO3) solution to the mixed solution of step (2) until no bubbles are generated during stirring, so that the final product of (2) is more stable under cationic conditions. Then, the mixture is acidified to pH = 2.0 with 0.01 mol / L hydrochloric acid (HCl), and extracted with 45 mL of DCM. The organic phase is then dried over anhydrous sodium sulfate (Na2SO4) to remove excess water, filtered through a sand core funnel to separate the solid and liquid, and the liquid is concentrated into a thick oily substance using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump. The cooling temperature of the rotary evaporator is -20 °C, the water bath heating temperature is 40 °C, and the rotation speed is 100 r / min. Finally, the crude product is precipitated with methanol (MeOH) and DCM ( Dichloromethane) as the eluent and purified by silica gel chromatography column, and the separation state of the product and impurities was confirmed by thin layer chromatography silica gel plate spot plate, and then vacuum concentrated to obtain pink oily 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid, wherein the volume ratio of methanol (MeOH) and DCM was 1:1, and the instrument used for vacuum concentration was RE-52AA rotary evaporator equipped with 2XZ-4 rotary vane vacuum pump and DLSB-5L / 20 low temperature coolant circulation pump, the cooling temperature of rotary evaporation was -20 ℃, the water bath heating temperature was 40 ℃, and the rotation speed was 100 r / min. In addition, 1H NMR nuclear magnetic resonance and Fourier transform infrared spectroscopy (FTIR) were performed on 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid, respectively verifying that it has the corresponding carboxylic acid structure.

[0219] (4) Then the 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid obtained above was dissolved in 5 mL of anhydrous DCM and mixed with a final concentration of 1×10 -3 mol / L N-hydroxysuccinimide (NHS) was stirred in an ice bath at a rate of 10 rpm for 1 h. Then, a final concentration of 1×10 -3 1-Ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) was added dropwise to the mixture, and the mixture was stirred under a nitrogen atmosphere at room temperature overnight at a rate of 10 rpm for 6 h to obtain an orange-red mixed solution.

[0220] (5) The mixed solution was added dropwise to petroleum ether as a precipitant to obtain a white flocculent, which was filtered and ultrasonically washed with ultrapure water for 5 minutes, then filtered to remove the waste liquid and dried at room temperature to obtain a white powdery disulfide functional monomer with a yield of 83%. The volume of petroleum ether was 100 mL and the volume of ultrapure water was 100 mL.

[0221] This embodiment provides a method for gelling a disulfide functional monomer, comprising the following steps:

[0222] (1) Polyvinyl alcohol 1788 (PVA) type 2, acrylic acid 7, 0.01 wt% 2-hydroxy-2-methylpropiophenone (1173), and poly(ethylene glycol) methacrylate (PEG) were dissolved in deionized water at a final concentration of 2 wt% under heating at 25 °C and stirred magnetically at 10 rpm for 1 min at room temperature to obtain 5 mL of a stock solution.

[0223] (2) Dissolve 5 mg of disulfide functional monomer in 100 μL acetone and add it to the above stock solution and stir it magnetically until it is completely dissolved. The stirring rate is 10 rpm and the time is 1 min to obtain a precursor solution. Inject 200 μL of the precursor solution into a mold with a spacing of 0.01 mm between two glass slides (the thickness of the wet-adhesive hydrogel) and cure it in a SCIENTZ03-II UV crosslinker with a wavelength of 365 nm for 5 min. The water content is controlled to be 1-20 μL by gravimetric analysis. Finally, a wet-adhesive hydrogel with disulfide functional monomer is obtained.

[0224] This example provides a biocompatible triggered separation of the wet-adhesive hydrogel, and the configuration method of the trigger solution is as follows:

[0225] (1) The final concentration was 5×10 -3 mol / L sodium bicarbonate (SBC) and 5×10 -3 mol / L glutathione (reduced form, GSH) was dissolved in 0.01 M phosphate buffered saline (PBS) at pH = 4.0.

[0226] (2) Use a rubber-tipped dropper to take 2 mL of the above trigger solution and drop it on a (width × length × thickness) 1 × 2 × 0.34 mm cm 2 After standing for 5 min, sodium bicarbonate (SBC) will gradually destroy the hydrogen bonds between the wet adhesive hydrogels, and glutathione (reduced form, GSH) will also break the disulfide bonds. Finally, the triggered wet adhesive hydrogel can be gently peeled off with tweezers (at this time, the adhesion force is close to 0 J m −2 ).

[0227] Example 5

[0228] This embodiment provides a method for preparing a disulfide functional monomer, comprising the following steps:

[0229] (1) The final concentration is 1×10 -2 mol / L dithioglycolic acid and 50mL of acetic anhydride were added to a round-bottom flask equipped with a magnetic stirring bar, and magnetically stirred at 1000rpm for 10h at room temperature to completely dissolve the mixed solution. Then, the remaining acetic anhydride was removed by vacuum using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump, wherein the cooling temperature of the rotary evaporation was -20°C, the water bath heating temperature was 40°C, and the rotation speed was 100 r / min. Finally, a colorless oily 1,4,5-oxadithiophene-2,7-dione was obtained.

[0230] (2) 3 g of 4-dimethylaminopyridine (DMAP) and a final concentration of 5 × 10 -2 mol / L hydroxyethyl methacrylate (HEMA) was dissolved in 50 mL of anhydrous dichloromethane (DCM) and magnetically stirred at 1000 rpm for 10 h at room temperature to ensure that 4-dimethylaminopyridine (DMAP) could completely activate the hydroxyl groups in hydroxyethyl methacrylate (HEMA). Then 50 mL of anhydrous DCM was used to dissolve the colorless oil obtained in step (1) and slowly transferred to the mixed solution in step (2), and magnetically stirred at 1000 rpm for 48 h.

[0231] (3) Add 100 mL of saturated sodium bicarbonate (NaHCO3) solution to the mixed solution of step (2) until no bubbles are generated during stirring, so that the final product of (2) is more stable under cationic conditions. Then, the mixture is acidified to pH = 2.0 with 10 mol / L hydrochloric acid (HCl), and extracted with 45 mL of DCM. The organic phase is then dried over anhydrous sodium sulfate (Na2SO4) to remove excess water, filtered through a sand core funnel to separate the solid and liquid, and the liquid is concentrated into a thick oily substance using a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump. The cooling temperature of the rotary evaporator is -20 °C, the water bath heating temperature is 40 °C, and the rotation speed is 100 r / min. Finally, the crude product is precipitated with methanol (MeOH) and DCM ( Dichloromethane ) was used as an eluent to purify the mixture through a silica gel chromatography column, and the separation state of the product and impurities was confirmed by thin layer chromatography silica gel plate spot plate, and then a pink oily 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid was obtained after vacuum concentration, wherein the volume ratio of methanol (MeOH) to DCM was 1:500, and the instrument used for vacuum concentration was a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump. The cooling temperature of the rotary evaporation was -20 °C, the water bath heating temperature was 40 °C, and the rotation speed was 100 r / min. In addition, 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid was analyzed by 1H NMR nuclear magnetic resonance and Fourier transform infrared spectroscopy (FTIR), respectively verifying that it has the corresponding carboxylic acid structure.

[0232] (4) Then the 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid obtained above was dissolved in 100 mL of anhydrous DCM and mixed with a final concentration of 5×10 -2mol / L N-hydroxysuccinimide (NHS) was stirred in an ice bath at a rate of 1000 rpm for 10 h. Then, a final concentration of 5×10 -2 1-Ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) was added dropwise to the mixture, and the mixture was stirred magnetically for 48 h at a rate of 1000 rpm in a nitrogen atmosphere at room temperature to obtain an orange-red mixed solution.

[0233] (5) The mixed solution was added dropwise to petroleum ether as a precipitant to obtain a white flocculent, which was then filtered and ultrasonically washed with ultrapure water for 10 h, and then filtered to remove the waste liquid and dried at room temperature to obtain a white powdery disulfide functional monomer with a yield of 83%. The volume of petroleum ether was 2000 mL, and the volume of ultrapure water was 2000 mL.

[0234] This embodiment provides a method for gelling a disulfide functional monomer, comprising the following steps:

[0235] (1) Polyvinyl alcohol 1788 (PVA) with a final concentration of 40 wt %, 60 wt % acrylic acid, 15 wt % 2-hydroxy-2-methylpropiophenone (1173), and 30 wt % poly(ethylene glycol) methacrylate were dissolved in deionized water under heating at 150 °C and magnetically stirred at 5000 rpm for 120 min at room temperature to obtain 30 mL of a stock solution.

[0236] (2) Dissolve 1000 mg of disulfide functional monomer in 10 mL of acetone and add it to the above stock solution and stir it magnetically until it is completely dissolved. The stirring rate is 5000 rpm for 120 min to obtain a precursor solution. Inject 200 μL of the precursor solution into a mold with a 5 mm interval between two glass slides (the thickness of the wet-adhesive hydrogel) and cure it in a SCIENTZ03-II UV crosslinker with a wavelength of 365 nm for 120 min. The water content is controlled to be 1-20 μL by gravimetric analysis. Finally, a wet-adhesive hydrogel with disulfide functional monomer is obtained.

[0237] This example provides a biocompatible triggered separation of the wet-adhesive hydrogel, and the configuration method of the trigger solution is as follows:

[0238] (1) Dissolve sodium bicarbonate (SBC) and glutathione (reduced form, GSH) at a final concentration of 50 mol / L in 10 M phosphate buffered saline (PBS) at pH = 12.0.

[0239] (2) Use a rubber-tipped dropper to take 2 mL of the above trigger solution and drop it on a (width × length × thickness) 1 × 2 × 0.34 mm cm 2 After standing for 10 min, sodium bicarbonate (SBC) will gradually destroy the hydrogen bonds between the wet adhesive hydrogels, and glutathione (reduced form, GSH) will also break the disulfide bonds. Finally, the triggered wet adhesive hydrogel can be gently peeled off with tweezers (at this time, the adhesion force is close to 0 J m −2 ).

[0240] Example 6

[0241] The process and conditions are the same as in Example 1, except that:

[0242] This embodiment provides a method for gelling a disulfide functional monomer, which includes the following steps:

[0243] (1) Dissolve polyvinyl alcohol 1788 (PVA), 1 wt % polyacrylic acid (PAA), 0.01 wt % benzophenone, and 0.01 wt % poly(ethylene glycol) dimethacrylate) in deionized water at 25 °C and stir magnetically at 10 rpm for 1 min at room temperature to obtain 5 mL of a stock solution.

[0244] (2) Dissolve 5 mg of disulfide functional monomer in 0.1 mL of acetone, add the mixture to the above stock solution and stir magnetically until the mixture is completely dissolved. The stirring speed is 10 rpm and the time is 1 min to obtain a precursor solution.

[0245] (3) The precursor solution obtained in step (2) is placed in a 1mL syringe with a metal needle with an inner diameter of 0.1 mm. The metal needle is connected to the positive electrode and the receiving plate is used as the negative electrode. Then the distance between the two electrodes is fixed to 5 cm, and a high voltage of 3kV is applied. At the same time, the propeller speed is set to 0.01mL / h and the spinning time is 6 h. The composite film containing nanofiber filaments and small droplets can be observed by electron microscopy. Then, the composite film is cured for 15 minutes using a SCIENTZ03-II type UV crosslinker with a wavelength of 365 nm, and a nanofiber membrane with a disulfide functional monomer having a thickness of 0.01 mm is obtained.

[0246] The dry nanofiber membrane was placed on the surface of a wet chicken heart and pressed for 5 s. The adhesion layer of the nanofiber membrane quickly formed hydrogen bonds and amide bonds at the junction after contacting water. The interfacial toughness between the wet adhesion hydrogel and the chicken heart was measured according to the standard test method for tissue adhesives (180° peel test, ASTM F2256-05 (2015)). When the contact and mild pressure (1 kPa) were applied for less than 5 s, the wet adhesion hydrogel could form an interfacial toughness of about 493 J m −2 The adhesion of the adhesive proves its ability to adhere instantly and tenaciously.

[0247] The remaining steps are the same as in Example 1.

[0248] The nanofiber membrane with disulfide functional monomers obtained by the above preparation method still exhibits strong wet adhesion ability, and the extracellular matrix-like structure of the nanofiber membrane can temporarily replicate the functions of the dermis and epidermis during wound healing and promote the complete recovery of the two tissue layers to avoid wound contraction and scar formation. In addition, compared with the hydrogel morphology, the three-dimensional network structure of the nanofiber membrane can be superimposed to form a tissue engineering scaffold, with a fiber diameter of approximately 340~1200 nm, a fiber pore size of 90~130 μm, and a highly porous matrix with a porosity of 60~90%, which is sufficient to allow and promote cell migration and proliferation. Therefore, the structure can allow cells to enter the defect space / wound bed and form soft tissue.

[0249] Example 7

[0250] The process and conditions are the same as in Example 1, except that:

[0251] This embodiment provides a method for gelling a disulfide functional monomer, which includes the following steps:

[0252] (1) Polyvinyl alcohol 1788 (PVA), 50 wt % polyacrylic acid (PAA), 20 wt % benzophenone, and 30 wt % poly(ethylene glycol) dimethacrylate were dissolved in deionized water at a final concentration of 50 wt % under heating at 150 °C and magnetically stirred at 5000 rpm for 120 min at room temperature to obtain 30 mL of a stock solution.

[0253] (2) Dissolve 1000 mg of disulfide functional monomer in 10 mL of acetone and add it to the above stock solution and stir it magnetically until it is completely dissolved at a rate of 5000 rpm for 120 min to obtain a precursor solution.

[0254] (3) The precursor solution obtained in step (2) is placed in a 50mL syringe with a metal needle, and the metal needle is connected to the positive electrode. The inner diameter of the metal needle of the syringe is 5mm, and the receiving plate is used as the negative electrode. Then the distance between the two electrodes is fixed to 30cm, and a high voltage of 50kV is applied. At the same time, the propeller speed is set to 5mL / h, and the spinning time is 6 hours. The composite film containing nanofiber filaments and small droplets can be observed by electron microscopy. Then, the SCIENTZ03-II type ultraviolet crosslinker is used for ultraviolet curing for 45 minutes with a wavelength of 365nm to obtain a nanofiber membrane with a disulfide functional monomer with a thickness of 2mm.

[0255] The dry nanofiber membrane was placed on the surface of a wet chicken heart and pressed for 5 s. The adhesion layer of the nanofiber membrane quickly formed hydrogen bonds and amide bonds at the junction after contacting water. The interfacial toughness between the wet adhesion hydrogel and the chicken heart was measured according to the standard test method for tissue adhesives (180° peel test, ASTM F2256-05 (2015)). When the contact and mild pressure (1 kPa) were applied for less than 5 s, the wet adhesion hydrogel could form an interfacial toughness of about 465 J m −2 The adhesion of the adhesive proves its ability to adhere instantly and tenaciously.

[0256] The remaining steps are the same as in Example 1.

[0257] The nanofiber membrane with disulfide functional monomers obtained by the above preparation method still exhibits strong wet adhesion ability, and the extracellular matrix-like structure of the nanofiber membrane can temporarily replicate the functions of the dermis and epidermis during wound healing and promote the complete recovery of the two tissue layers to avoid wound contraction and scar formation. In addition, compared with the hydrogel morphology, the three-dimensional network structure of the nanofiber membrane can be superimposed to form a tissue engineering scaffold, with a fiber diameter of approximately 340~1200 nm, a fiber pore size of 90~130 μm, and a highly porous matrix with a porosity of 60~90%, which is sufficient to allow and promote cell migration and proliferation. Therefore, the structure can allow cells to enter the defect space / wound bed and form soft tissue.

[0258] Comparative Example 1

[0259] The process and conditions are the same as those in Example 1, except that: the modification preparation method of the disulfide functional monomer is different from that in Example 1, specifically, an equimolar amount of the disulfide monomer (dithioglycolic acid) is replaced one by one with an equimolar amount of diphenyl disulfide, dimethyl disulfide, 3-carboxypropyl disulfide and cystine, and the structural formula of the obtained disulfide functional monomer and the performance parameters of gelation and triggered separation are shown in the following table:

[0260] Table 1 Structural formula of disulfide functional monomers and performance parameters after gelation

[0261]

[0262] The remaining steps and conditions are the same as in Example 1.

[0263] It is shown that the wet adhesive patch of disulfide functional monomer obtained by the above preparation method has universal applicability in triggering separation at different time scales, and can dissociate and replace the mispositioned wet adhesive hydrogel in an efficient, biocompatible and non-secondary wound-injury manner. In addition, the wet adhesive patch can achieve instant super-strong adhesion on the wet dynamic tissue surface and achieve the purpose of on-demand separation by using a biocompatible trigger solution.

[0264] Comparative Example 2

[0265] The process and conditions are the same as those in Example 1, except that the purification method of the final product disulfide functional monomer is different, specifically as follows:

[0266] (1) The final concentration is 1×10 -2 mol / L 6-(2-(methacryloyloxy)ethoxy)hept-6-enoic acid was dissolved in 15 mL of anhydrous DCM and mixed with a final concentration of 1×10 -2 mol / L N-hydroxysuccinimide (NHS) was stirred in an ice bath at a rate of 470 rpm for 0.5 h. Then, a final concentration of 1×10 -2 1-Ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) was added dropwise to the mixture, and the mixture was stirred magnetically overnight under nitrogen atmosphere at room temperature to obtain an orange-red mixed solution.

[0267] (2) The instrument used was a RE-52AA rotary evaporator equipped with a 2XZ-4 rotary vane vacuum pump and a DLSB-5L / 20 low-temperature coolant circulation pump to concentrate the liquid into a thick orange-red oil. The cooling temperature of the rotary evaporator was -20°C, the water bath heating temperature was 40°C, and the rotation speed was 100 r / min.

[0268] (3) Then, a mixture of ethyl acetate and petroleum ether is selected as an eluent to purify the thick orange-red oil through a silica gel chromatography column, and the separation state of the product and impurities is confirmed by thin layer chromatography silica gel plate spot plate, and then after vacuum concentration, a yellow oily disulfide functional monomer is obtained, wherein the volume of ethyl acetate and petroleum ether is 1:1.

[0269] The remaining steps and conditions are the same as in Example 1.

[0270] Although the structure of the yellow oily disulfide functional monomer is roughly the same as that of the white powdery disulfide functional monomer in Example 1 after 1H NMR nuclear magnetic resonance and Fourier transform infrared spectroscopy (FTIR) testing, there are a few impurity peaks in both the 1H NMR nuclear magnetic resonance spectrum and the Fourier transform infrared spectroscopy (FTIR) spectrum, proving that pure disulfide functional monomers are not obtained, and the yield of the yellow oily disulfide functional monomer is as low as about 14%. In addition, it is not only time-consuming (more than 8 h), but also has high technical requirements for operators. Therefore, the modification and purification method of the disulfide functional monomer in Example 1 not only has a pure product without impurities, saves time and cost, but also greatly improves the yield (about 83%), which is an efficient and convenient purification method.

Claims

1. A method for preparing a disulfide wet adhesive patch, characterized in that: The disulfide wet-adhesive patch includes a wet-adhesive hydrogel or a wet-adhesive electrospun film; The preparation process of wet adhesion hydrogel is as follows: 1) Dissolve the first crosslinking agent in water at 25-150°C; add acrylic acid, photoinitiator and second crosslinking agent to the first crosslinking agent aqueous solution and stir until completely dissolved to obtain a stock solution; The first cross-linking agent may be one or more of polyvinyl alcohol 1788, polyethylene oxide, polyacrylic acid, polyvinyl pyrrolidone, polyethylene imine, polyacrylamide, polyethylene glycol, polyvinyl butyral, cellulose, ethyl cellulose, and zein; The second crosslinking agent is one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, methylenebis(o-chloroaniline), p-quinonedioxime, poly(ethylene glycol) methacrylate, poly(ethylene glycol) dimethacrylate, diisocyanate, bismaleimide and triallyl isocyanate; 2) dissolving the NHS ester functionalized monomer having a disulfide bond in acetone, and adding the monomer to the stock solution and stirring to obtain a precursor solution; Placing the precursor solution on a flat plate mold or between two transparent molds stacked one above the other at a desired distance from each other, and curing it under ultraviolet light to obtain a wet-adhesive hydrogel having disulfide functional monomers; Alternatively, the wet adhesion electrospun film preparation process is as follows: 1) Dissolve polyvinyl alcohol 1788 in water at 25-150°C; add polyacrylic acid, benzophenone and poly(ethylene glycol) dimethacrylate to the polyvinyl alcohol 1788 aqueous solution and stir until completely dissolved to obtain a stock solution; 2) dissolving the NHS ester functionalized monomer having a disulfide bond in acetone, and adding the monomer to the stock solution and stirring to obtain a precursor solution; The precursor solution is electrospun to obtain a nanofiber membrane, and then ultraviolet light is cured to obtain a nanofiber membrane with disulfide functional monomers; Preparation of wet adhesion hydrogels: The mass percentage of the first cross-linking agent in the stock solution of step (1) is 2-40 wt %; The mass percentage of acrylic acid in the stock solution of step (1) is 7-60 wt %; The photoinitiator in the stock solution of step (1) may be one or more of 2-hydroxy-2-methylpropiophenone, dialkoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, α-ketoglutaric acid, benzophenone, 4-methylbenzophenone, and 2,4,6-trimethylbenzophenone; The mass percentage of the photoinitiator is 0.01-15 wt %; The mass percentage of the second cross-linking agent in the stock solution of step (1) is 0.01-1.5 wt %; Or, during the preparation of wet adhesion electrospun films: The mass percentage of polyvinyl alcohol 1788 in step (1) is 1-50 wt%; The mass percentage of the polyacrylic acid in step (1) is 1-50 wt %; The mass percentage of benzophenone in step (1) is 0.01-20 wt %; The mass percentage of the poly(ethylene glycol) dimethacrylate in step (1) is 0.01-30 wt %; Preparation of wet adhesion hydrogels: When the volume of the stock solution in step 1) is 5-30 mL, the mass of the NHS ester functionalized monomer having a disulfide bond in step (2) is 5-1000 mg; the volume of acetone in step (2) is 0.1-10 mL; The thickness of the prepared disulfide wet-adhesive patch ranged from 0.01 to 5 mm; Or, during the preparation of wet adhesion electrospun films: When the volume of the stock solution in step 1) is 5-30 mL, the mass of the functional monomer of the disulfide in step (2) is 5-1000 mg; the volume of acetone in step (2) is 0.1-10 mL; In step (2), the precursor solution is placed in a syringe with a metal needle, the metal needle is connected to the positive electrode, the receiving plate is used as the negative electrode, and then the distance between the two electrodes is fixed, and then high voltage is applied; at the same time, the propeller speed is set to push the syringe, and the nanofiber membrane is obtained by electrospinning. The volume of the syringe in step (2) is 1 to 50 mL; The inner diameter of the metal needle of the syringe in step (2) is 0.1-5 mm; The distance between the two poles in step (2) is 5 to 30 cm; The high voltage in step (2) is 3-50 kV; The propeller speed in step (2) is set to 0.01-5 mL / h; The thickness of the prepared disulfide wet-adhesive nanofiber membranes was 0.01-2 mm; The method for preparing the NHS ester functionalized monomer having a disulfide bond comprises the following steps: 1) Mixing and stirring the disulfide monomer and acetic anhydride until they are completely dissolved, and then concentrating to remove unreacted acetic anhydride; 2) 4-Dimethylaminopyridine (DMAP) and hydroxyethyl methacrylate (HEMA) were dissolved in dichloromethane (DCM) and stirred at room temperature to allow DMAP to activate the hydroxyl groups in HEMA; 3) Dissolve the product obtained in step (1) in anhydrous DCM and transfer it to the mixed solution of step (2), stirring for 5 to 60 minutes; 4) adding a saturated sodium bicarbonate (NaHCO3) solution to maintain the steady-state structure of the product of step (3), acidifying the mixture with hydrochloric acid (HCl) to a pH of less than or equal to 2.0, and extracting with DCM; drying the organic phase over anhydrous sodium sulfate (Na2SO4), filtering and concentrating it to a thick oil, and then purifying the crude product through a silica gel chromatography column using a mixture of methanol (MeOH) and DCM as an eluent, and finally concentrating it to a thick oil; 5) The oily liquid obtained in step (4) was then dissolved in anhydrous DCM and stirred with N-hydroxysuccinimide (NHS) in an ice bath; 6) Add 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride (EDC) dissolved in anhydrous DCM dropwise into the above mixture and stir magnetically under nitrogen atmosphere at room temperature for 5-60 min; 7) The solution obtained in step (6) is added dropwise to petroleum ether as a precipitant to obtain white floccules, which are then washed with water, filtered and dried to obtain a powdery disulfide functional monomer.

2. The preparation method according to claim 1, characterized in that: During the preparation of wet-adhesive hydrogels or wet-adhesive electrospun films; The stirring rate in step (1) is 10-5000 rpm and the time is 1-120 min; The stirring rate in step (2) is 10-5000 rpm and the time is 1-120 min; In the preparation process of the wet adhesion hydrogel: the instrument used for the UV curing in step (2) is a SCIENTZ03-II UV cross-linking instrument, and the UV cross-linking instrument used in step (2) has a light curing time of 5 to 120 min; Or, in the preparation process of the wet adhesion electrospinning film: the instrument used for the ultraviolet light curing in step (2) is a SCIENTZ03-II type ultraviolet cross-linking instrument; the light curing time of the ultraviolet cross-linking instrument used in step (2) is 15~45 min.

3. The preparation method according to claim 1, characterized in that: The disulfide monomer in step (1) is one or more of diphenyl disulfide, dimethyl disulfide, 3-carboxypropyl disulfide, dithioglycolic acid and cystine; The final concentration of the disulfide monomer in step (1) is 1×10 -3 ~5×10 -2 mol / L.

4. The preparation method according to claim 1, characterized in that: The volume of acetic anhydride in step (1) is 3-50 mL; The stirring rate in step (1) is 10-1000 rpm and the time is 0.5-10 h; The mass of 4-dimethylaminopyridine (DMAP) in step (2) is 0.01-3 g; The final concentration of hydroxyethyl methacrylate (HEMA) in step (2) is 1×10 -3 ~5×10 -2 mol / L; The volume of anhydrous dichloromethane (DCM) in step (2) is 5-50 mL; The stirring rate in step (2) is 10-1000 rpm and the time is 0.5-10 h; The volume of anhydrous DCM in step (3) is 5-50 mL; The stirring rate in step (3) is 10-1000 rpm and the time is 6-48 h; The volume of saturated sodium bicarbonate (NaHCO3) in step (4) is 5-100 mL; The concentration of hydrochloric acid (HCl) in step (4) is 0.01-10 mol / L; The volume of methanol (MeOH) and DCM used as eluent in step (4) is 1:1-500; The volume of anhydrous DCM in step (5) is 5-100 mL; The final concentration of N-hydroxysuccinimide (NHS) in step (5) is 1×10 -3 ~5×10 -2 mol / L; The stirring rate in step (5) is 10-1000 rpm and the time is 0.5-10 h; The volume of anhydrous DCM in step (6) is 5-100 mL; The final concentration of 1-ethyl-(3-(dimethylaminopropyl)carbodiimide hydrochloride) (EDC) in step (6) is 1×10 -3 ~5×10 -2 mol / L; The stirring rate in step (6) is 10-1000 rpm and the time is 6-48 h; The volume of petroleum ether in step (7) is 100-2000 mL; The volume of water in step (7) is 100-2000 mL; The conditions used for water washing in step (7) are ultrasonic treatment for 5 min to 10 h.

5. A disulfide wet adhesive patch prepared by the method for preparing a disulfide wet adhesive patch according to any one of claims 1 to 4.

6. Use of the disulfide wet adhesive patch according to claim 5 in a product for treating tissue surface repair.

7. The use according to claim 6, characterized in that: The triggered separation process of the wet adhesive patch adhered to the wet tissue and organ surface and the biological tissue surface is as follows: the trigger solution is wet applied or applied to the wet adhesive hydrogel adhered to the biological tissue surface, and after standing for 5 to 45 minutes, the triggered wet adhesive hydrogel can be peeled off; The trigger solution contains sodium bicarbonate and glutathione dissolved in phosphate buffer; the concentration of sodium bicarbonate is 5×10 -3 ~50mol / L; the concentration of glutathione is 5×10 -3 ~10 mol / L; the concentration of the phosphate buffer is 1×10 -2 ~10mol / L, PH=4.0~12.0.

Citation Information

Patent Citations

  • Adhesive material with triggered on-demand detachment

    CN115697426A

  • Shape memory adhesive material for diabetic wound healing

    CN117202942A