A metal ceramic tool and a method for preparing the same
By reducing the particle size of the hard phase raw materials and using TiAlN coating and hot isostatic pressing, the problems of tissue uniformity and insufficient interface bonding during the sintering process of cermet tools are solved, and their mechanical properties and comprehensive properties are significantly improved, making it suitable for CNC tools.
Patent Information
- Application Number
- CN202410986640.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The insufficient degree of tissue homogenization and interface wettability of cermet tools during the sintering process results in low transverse fracture strength and toughness, which limits their application.
By reducing the particle size of hard phase raw materials, plating TiAlN coating and performing hot isostatic pressing treatment, the comprehensive performance of cermet materials can be improved. Specific steps include ball milling, molding, vacuum sintering, TiAlN coating using multi-arc ion plating technology, and hot isostatic pressing.
It improves the mechanical properties and interface bonding strength of cermet materials, enhances the density and comprehensive performance of the material, and makes it more suitable for CNC cutting tools.
Smart Images

Figure CN118513556B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of numerical control tools, in particular to a metal ceramic tool and a preparation method thereof. Background Art
[0002] With the development of high-speed precision cutting and numerical control technology, the requirements for tool cutting performance are also increasing. Ti(C,N)-based cermet is a composite material with refractory intermetallic compounds TiC and TiN as hard phases, metal Ni or Ni and Co as bonding phases, and carbide materials as reinforcing phases. It is widely used in tool materials because of its advantages such as high hardness, excellent wear resistance, low friction coefficient and good thermal stability. However, compared with cemented carbide, cermet has more components, and the degree of organizational homogenization and interface wettability are insufficient during the sintering process, resulting in relatively low transverse fracture strength and toughness, which also limits its application. Based on this, a cermet tool and its preparation method are proposed. Summary of the invention
[0003] In order to address the deficiencies of the prior art, the present invention provides a metal ceramic tool and a preparation method thereof, which improves the comprehensive performance of the metal ceramic material by reducing the particle size of the hard phase raw material, coating the TiAlN coating and performing hot isostatic pressing.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for preparing a metal ceramic tool, comprising the following steps:
[0005] (1) Micron-sized Ni (nickel) powder, Co (cobalt) powder, WC (tungsten carbide) powder, MO2C (molybdenum carbide) powder, Cr3C2 (chromium carbide) powder, submicron-sized TiC (titanium carbide) powder and nano-sized TiN (titanium nitride) powder are sequentially poured into a ball mill for ball milling. After the ball milling is completed, the slurry is separated and spray-dried to obtain a premix;
[0006] (2) pouring the premix into a mold for compression molding, vacuum degreasing the obtained tool blank, and then vacuum sintering the obtained tool blank to obtain a tool blank;
[0007] (3) Using TiAl alloy target as target material, Ar (argon) and N2 (nitrogen) as auxiliary gases (the purity of Ar and N2 is greater than 99.999%), a TiAlN (titanium aluminum nitride) coating is plated on the surface of the tool blank by multi-arc ion plating technology to obtain a tool blank;
[0008] (4) Using N2 as the pressure medium, the tool blank is subjected to hot isostatic pressing treatment. After cooling, a metal ceramic tool is obtained.
[0009] Preferably, in step (1), the ball milling treatment is specifically as follows: after adding each powder (including micron-sized Ni powder, Co powder, WC powder, MO2C powder, Cr3C2 powder, submicron-sized TiC powder and nano-sized TiN powder) into a ball mill, anhydrous ethanol, 10wt% polyvinyl alcohol solution and Tween-80 are added, and the ball milling is performed at a speed of 100-150rpm for 25-30h; wherein the amount of anhydrous ethanol added is 35% of the total mass of each powder, the amount of polyvinyl alcohol solution added is 4.5% of the total mass of each powder, and the amount of Tween-80 added is 0.6% of the total mass of each powder.
[0010] Preferably, in step (1), the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53 μm, 1.26 μm, 3.27 μm, 3.35 μm and 3.63 μm respectively; the average particle size of TiC powder is 0.55 μm; and the average particle size of TiN powder is 100 nm.
[0011] Preferably, in step (2), the compression molding is specifically performed by controlling the pressure to 250-300 MPa and maintaining the pressure for 15-20 seconds.
[0012] Preferably, in step (2), vacuum degreasing is specifically performed by degreasing at 250-350° C. for 3-5 hours under a vacuum degree of 5-8 Pa.
[0013] Preferably, in step (2), the vacuum sintering process is specifically as follows: controlling the vacuum degree to be 1×10 -1 Pa, keep warm at 1420-1430℃ for 40-60min.
[0014] Preferably, in step (3), the multi-arc ion plating technology is specifically as follows: controlling the target current to 65A, the bias voltage to -300V, the N2 partial pressure to 0.35Pa, the deposition temperature to 450°C, and the deposition time to 100min.
[0015] Preferably, in step (3), the TiAl alloy target is composed of 60% Ti and 40% Al in terms of mass percentage.
[0016] Preferably, in step (4), the hot isostatic pressing treatment is specifically: keeping the temperature at 900-1000° C. for 2.5-3.5 h at a pressure of 90-100 MPa.
[0017] The present invention also provides a metal ceramic tool prepared by the above preparation method, which comprises the following raw materials, by mass percentage: TiC powder 40-45%, TiN powder 10-20%, Ni powder 5-10%, Co powder 5-10%, WC powder 10-12%, MO2C powder 5-8%, and Cr3C2 powder 5-10%.
[0018] The present invention provides a metal ceramic tool and a preparation method thereof, which have the following beneficial effects compared with the prior art:
[0019] The present invention uses submicron TiC powder and nanometer TiN powder together, so that the particle size of the hard phase is reduced, which is conducive to a more uniform structure of the metal ceramic material, better formation of the annular phase, and a relatively small grain size, thereby improving the density and ultimately improving the mechanical properties of the metal ceramic material, so that it can be better applied to CNC tools.
[0020] The present invention adopts a TiAl alloy target, and plates a TiAlN coating on the surface of the sintered metal ceramic through a multi-arc ion plating technology, and undergoes a hot isostatic pressing treatment. The high temperature and high pressure not only improve the density of the material and eliminate the pores between the TiAlN coating and the metal ceramic substrate, but also make the elements between the coating and the substrate diffuse and migrate with each other, have good interface bonding strength, and improve the bonding force of the coating on the substrate, thereby ultimately improving the comprehensive performance of the metal ceramic material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The description of the exemplary embodiments of the present application is used to explain the present application and does not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 This is a metallographic diagram of the tool blank after vacuum sintering in Comparative Example 1 of the present invention;
[0023] Figure 2 This is a metallographic diagram of the tool blank after hot isostatic pressing in Comparative Example 2 of the present invention;
[0024] Figure 3 This is a metallographic diagram of the metal ceramic tool in Example 4 of the present invention. DETAILED DESCRIPTION
[0025] The following examples are used to explain the implementation methods of the present application in detail, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.
[0026] Example 1
[0027] A method for preparing a metal ceramic tool comprises the following steps:
[0028] (1) In terms of mass percentage, 10% of micron-sized Ni powder, 5% of Co powder, 10% of WC powder, 8% of MO2C powder, 10% of Cr3C2 powder, 45% of submicron-sized TiC powder and 12% of nano-sized TiN powder were poured into a ball mill in sequence, and then anhydrous ethanol accounting for 35% of the total mass of each powder, 10wt% polyvinyl alcohol (PVOH-10) solution accounting for 4.5% of the total mass of each powder and Tween-80 accounting for 0.6% of the total mass of each powder were added, and the mixture was ball-milled at a speed of 150 rpm for 25 h. After the ball milling was completed, the slurry was separated and spray-dried to obtain a premix;
[0029] Among them, the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53μm, 1.26μm, 3.27μm, 3.35μm and 3.63μm respectively; the average particle size of TiC powder is 0.55μm; and the average particle size of TiN powder is 100nm.
[0030] (2) The premix was poured into a mold, and compression molded at a pressure of 300 MPa and maintained at this pressure for 15 seconds. The obtained tool blank was subjected to vacuum degreasing treatment, that is, degreasing at 350°C for 3 hours under a vacuum degree of 5 Pa. The obtained tool blank was then subjected to vacuum sintering treatment, that is, the vacuum degree was controlled to be 1×10 -1 Pa, and kept warm at 1420℃ for 60min to obtain the tool blank.
[0031] (3) Using a TiAl alloy target (the TiAl alloy target is composed of 60% Ti and 40% Al in mass percentage) as the target material and Ar and N2 as the auxiliary gases, a TiAlN coating is plated on the surface of the tool blank by multi-arc ion plating technology. During the process, the target current is controlled to 65A, the bias voltage is -300V, the N2 partial pressure is 0.35Pa, the deposition temperature is 450℃, and the deposition time is 100min to obtain a fine tool blank.
[0032] (4) Using N2 as the pressure medium, the tool blank was subjected to hot isostatic pressing treatment, that is, at a pressure of 100 MPa, kept at 900°C for 2.5 h, and after cooling, a metal ceramic tool was obtained.
[0033] Example 2
[0034] A method for preparing a metal ceramic tool comprises the following steps:
[0035] (1) Based on the mass percentage, 5% of the micron-level Ni powder, 10% of Co powder, 12% of WC powder, 8% of MO2C powder, 5% of Cr3C2 powder, 40% of the sub-micron-level TiC powder and 20% of the nano-level TiN powder are poured into the ball mill in sequence, and then anhydrous ethanol accounting for 35% of the total mass of each powder, 10wt% of the polyvinyl alcohol (PVOH-10) solution accounting for 4.5% of the total mass of each powder, and Tween-80 accounting for 0.6% of the total mass of each powder, and ball milling at a speed of 100rpm for 25 hours. After the ball mill is finished, the slurry is separated and spray dried to obtain a premix;
[0036] Among them, the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53μm, 1.26μm, 3.27μm, 3.35μm and 3.63μm respectively; the average particle size of TiC powder is 0.55μm; and the average particle size of TiN powder is 100nm.
[0037] (2) The premix is poured into a mold, and the mold is pressed at a pressure of 250 MPa and maintained at the pressure for 20 seconds. The obtained tool blank is subjected to vacuum degreasing treatment, that is, degreasing at 250 °C for 5 hours under a vacuum degree of 8 Pa, and then the obtained tool blank is subjected to vacuum sintering treatment, that is, the vacuum degree is controlled to be 1×10 -2 Pa, and kept warm at 1430℃ for 40min to obtain the tool blank.
[0038] (3) Using a TiAl alloy target (the TiAl alloy target is composed of 60% Ti and 40% Al in mass percentage) as the target material and Ar and N2 as the auxiliary gases, a TiAlN coating is plated on the surface of the tool blank by multi-arc ion plating technology. During the process, the target current is controlled to 65A, the bias voltage is -300V, the N2 partial pressure is 0.35Pa, the deposition temperature is 450℃, and the deposition time is 100min to obtain a fine tool blank.
[0039] (4) Using N2 as the pressure medium, the tool blank was subjected to hot isostatic pressing treatment, that is, at a pressure of 90 MPa and kept at 1000°C for 3.5 hours. After cooling, a metal ceramic tool was obtained.
[0040] Example 3
[0041] A method for preparing a metal ceramic tool comprises the following steps:
[0042] (1) Based on the mass percentage, 5% of micron-level Ni powder, 10% of Co powder, 12% of WC powder, 8% of MO2C powder, 5% of Cr3C2 powder, 40% of sub-micron-level TiC powder and 20% of nano-level TiN powder are poured into the ball mill in sequence, and then anhydrous ethanol accounting for 35% of the total mass of each powder, 10 wt% polyvinyl alcohol (PVOH-10) solution accounting for 4.5% of the total mass of each powder, and Tween-80 accounting for 0.6% of the total mass of each powder, and ball milling at a speed of 120 rpm for 28 hours. After the ball mill is finished, the slurry is separated and spray dried to obtain a premix;
[0043] Among them, the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53μm, 1.26μm, 3.27μm, 3.35μm and 3.63μm respectively; the average particle size of TiC powder is 0.55μm; and the average particle size of TiN powder is 100nm.
[0044] (2) The premix was poured into a mold, and compression molded at a pressure of 280 MPa and maintained at this pressure for 17 seconds. The obtained tool blank was subjected to vacuum degreasing treatment, that is, degreasing at 300 °C for 4 hours under a vacuum degree of 6 Pa, and then the obtained tool blank was subjected to vacuum sintering treatment, that is, the vacuum degree was controlled to be 1×10 -2 Pa, and kept warm at 1425℃ for 50min to obtain the tool blank.
[0045] (3) Using a TiAl alloy target (the TiAl alloy target is composed of 60% Ti and 40% Al in mass percentage) as the target material and Ar and N2 as the auxiliary gases, a TiAlN coating is plated on the surface of the tool blank by multi-arc ion plating technology. During the process, the target current is controlled to 65A, the bias voltage is -300V, the N2 partial pressure is 0.35Pa, the deposition temperature is 450℃, and the deposition time is 100min to obtain a fine tool blank.
[0046] (4) Using N2 as the pressure medium, the tool blank was subjected to hot isostatic pressing treatment, that is, at a pressure of 100 MPa, kept at 1000°C for 2.5 hours, and after cooling, a metal ceramic tool was obtained.
[0047] Example 4
[0048] A method for preparing a metal ceramic tool comprises the following steps:
[0049] (1) Based on the mass percentage, 10% of the micron-scale Ni powder, 8% of Co powder, 12% of WC powder, 8% of MO2C powder, 7% of Cr3C2 powder, 42% of the sub-micron-scale TiC powder and 13% of the nano-scale TiN powder are poured into the ball mill in sequence, and then anhydrous ethanol accounting for 35% of the total mass of each powder, 10wt% polyvinyl alcohol (PVOH-10) solution accounting for 4.5% of the total mass of each powder, and Tween-80 accounting for 0.6% of the total mass of each powder, and ball milling at a speed of 100 rpm for 25 hours. After the ball mill is finished, the slurry is separated and spray dried to obtain a premix;
[0050] Among them, the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53μm, 1.26μm, 3.27μm, 3.35μm and 3.63μm respectively; the average particle size of TiC powder is 0.55μm; and the average particle size of TiN powder is 100nm.
[0051] (2) The premix is poured into a mold, and compression molded at a pressure of 250 MPa and maintained at this pressure for 15 seconds. The obtained tool blank is subjected to vacuum degreasing treatment, that is, degreasing at 250 °C for 5 hours under a vacuum degree of 8 Pa, and then the obtained tool blank is subjected to vacuum sintering treatment, that is, the vacuum degree is controlled to be 1×10 -2 Pa, and kept warm at 1420℃ for 60min to obtain the tool blank.
[0052] (3) Using a TiAl alloy target (the TiAl alloy target is composed of 60% Ti and 40% Al in mass percentage) as the target material and Ar and N2 as the auxiliary gases, a TiAlN coating is plated on the surface of the tool blank by multi-arc ion plating technology. During the process, the target current is controlled to 65A, the bias voltage is -300V, the N2 partial pressure is 0.35Pa, the deposition temperature is 450℃, and the deposition time is 100min to obtain a fine tool blank.
[0053] (4) Using N2 as the pressure medium, the tool blank was subjected to hot isostatic pressing treatment, that is, at a pressure of 90 MPa and kept at 900°C for 3.5 hours. After cooling, a metal ceramic tool was obtained.
[0054] Comparative Example 1
[0055] A method for preparing a metal ceramic tool comprises the following steps:
[0056] (1) In terms of mass percentage, 5% Ni powder, 10% Co powder, 12% WC powder, 8% MO2C powder, 5% Cr3C2 powder, 40% TiC powder and 20% TiN powder of micron size are poured into a ball mill in sequence, and then anhydrous ethanol accounting for 35% of the total mass of each powder, 10wt% polyvinyl alcohol (PVOH-10) solution accounting for 4.5% of the total mass of each powder and Tween-80 accounting for 0.6% of the total mass of each powder are added, and the mixture is ball milled at a speed of 120 rpm for 28 h. After the ball milling is completed, the slurry is separated and spray dried to obtain a premix;
[0057] Among them, the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53μm, 1.26μm, 3.27μm, 3.35μm and 3.63μm respectively; the average particle size of TiC powder is 2.55μm; and the average particle size of TiN powder is 2.76μm.
[0058] (2), (3), and (4) remain the same as the corresponding steps in Example 4.
[0059] Comparative Example 2
[0060] A method for preparing a metal ceramic tool is basically the same as that of Example 4, except that the obtained tool blank is not plated with a TiAlN coating, but is directly subjected to hot isostatic pressing treatment, and after cooling, a metal ceramic tool is obtained.
[0061] Comparative Example 3
[0062] A method for preparing a metal ceramic tool is basically the same as that of Example 4, except that the obtained tool blank is not subjected to hot isostatic pressing and is directly used as a metal ceramic tool.
[0063] Comparative Example 4
[0064] A method for preparing a metal ceramic tool is basically the same as that of Example 4, except that the obtained tool blank is not subjected to subsequent TiAlN coating and hot isostatic pressing treatment, and the tool blank is directly used as a metal ceramic tool.
[0065] Quality Inspection
[0066] Samples meeting the testing standards were prepared using the preparation methods in Examples 1-4 and Comparative Examples 1-4, and the quality of each sample was tested using the sample as a test object.
[0067] 1. Hardness test: The test instrument is HV-120 Vickers hardness tester, and the test conditions are 10kg load and 15s holding time. After unloading the load, use the optical microscope attached to the hardness tester to accurately measure the lengths L1 and L2 of the two diagonals of the square pyramid indentation, and take the average value of the diagonal length L = (L1 + L2) / 2 and substitute it into the following formula to calculate the hardness.
[0068] In the formula, is the applied load, N; is the average diagonal length of the indentation, mm.
[0069] 2. Bending strength test: The test instrument is QJ211S universal mechanical testing machine, using three-point bending method, the test span is 16mm, and the pressing speed is 0.1mm / min. The formula for calculating the bending strength is as follows:
[0070]
[0071] In the formula, is the flexural strength, MPa; is the maximum load value, KN; is the span, mm; b is the width, mm; h is the thickness, mm.
[0072] 3. Fracture toughness Test: The test instrument is a QJ211S universal mechanical testing machine. A notch with a depth of about 1 mm is machined in the middle of the sample using a wire cutting device. The test span is 16 mm and the pressing speed is 0.1 mm / min. The formula for calculating fracture toughness is as follows:
[0073]
[0074] Where a is the crack length, mm; P is the maximum load value, N; L is the span, mm; b is the width, mm; h is the thickness, mm.
[0075] The specific results are shown in the following table.
[0076] Table 1 Performance test
[0077] category Hardness (HRA) Flexural strength (MPa) <![CDATA[Fracture toughness (MPa·m 1 / 2 ).]]> Example 1 91.4 2418 16.3 Example 2 91.8 2454 16.7 Example 3 93.1 2350 14.8 Example 4 92.5 2492 15.4 Comparative Example 1 90.2 2286 13.9 Comparative Example 2 90.4 2191 14.1 Comparative Example 3 90.7 2198 14.3 Comparative Example 4 90.0 2012 12.6
[0078] From the above table we can know:
[0079] (1) The hardness of the samples in Examples 1-4 was maintained above 91.4 HRA, the flexural strength was maintained above 2350 MPa, and the fracture toughness was maintained at 14.8 MPa·m 1 / 2 Above all, the overall quality performance is excellent.
[0080] (2) Comparison of the data of Example 3 with those of Comparative Example 1 shows that the combined use of submicron TiC powder and nano-TiN powder can significantly improve the hardness and flexural strength of the sample by refining the grains and making the structure uniform, but has little effect on the fracture toughness.
[0081] (3) Comparison of the data of Example 3 with those of Comparative Examples 2-4 shows that coating TiAlN and hot isostatic pressing can indeed improve the comprehensive properties of the metal ceramic sample.
[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the equivalents of the appended claims.
Claims
1. A method for preparing a metal ceramic tool, characterized in that: The following steps are involved: (1) Micron-sized Ni powder, Co powder, WC powder, MO2C powder, Cr3C2 powder, submicron-sized TiC powder and nano-sized TiN powder are sequentially poured into a ball mill for ball milling. After the ball milling is completed, the slurry is separated and spray-dried to obtain a premix; (2) pouring the premix into a mold for compression molding, vacuum degreasing the obtained tool blank, and then vacuum sintering the obtained tool blank to obtain a tool blank; (3) Using TiAl alloy target as target material and Ar and N2 as auxiliary gases, a TiAlN coating is plated on the surface of the tool blank by multi-arc ion plating technology to obtain a tool blank; (4) Using N2 as the pressure medium, hot isostatic pressing is performed on the tool blank, and after cooling, a metal ceramic tool is obtained; In step (1), the average particle sizes of Ni powder, Co powder, WC powder, MO2C powder and Cr3C2 powder are 1.53 μm, 1.26 μm, 3.27 μm, 3.35 μm and 3.63 μm respectively; the average particle size of TiC powder is 0.55 μm; and the average particle size of TiN powder is 100 nm.
2. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (1), the ball milling treatment is specifically as follows: after adding each powder into the ball mill, anhydrous ethanol, 10wt% polyvinyl alcohol solution and Tween-80 are added, and the ball milling is carried out at a speed of 100-150rpm for 25-30h; wherein the amount of anhydrous ethanol added is 35% of the total mass of each powder, the amount of polyvinyl alcohol solution added is 4.5% of the total mass of each powder, and the amount of Tween-80 added is 0.6% of the total mass of each powder.
3. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (2), the compression molding is specifically as follows: controlling the pressure to 250-300 MPa and maintaining the pressure for 15-20 seconds.
4. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (2), vacuum degreasing is specifically performed by degreasing at 250-350°C for 3-5 hours under a vacuum degree of 5-8 Pa.
5. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (2), the vacuum sintering process is specifically as follows: the vacuum degree is controlled at 1×10 -1 Pa, keep warm at 1420-1430℃ for 40-60min.
6. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (3), the multi-arc ion plating technology is specifically as follows: controlling the target current to 65A, the bias voltage to -300V, the N2 partial pressure to 0.35Pa, the deposition temperature to 450°C, and the deposition time to 100min.
7. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (3), the TiAl alloy target is composed of 60% Ti and 40% Al in terms of mass percentage.
8. The method for preparing a metal ceramic tool according to claim 1, characterized in that: In step (4), the hot isostatic pressing treatment is specifically: keeping the temperature at 900-1000° C. for 2.5-3.5 hours at a pressure of 90-100 MPa.
9. A metal ceramic tool prepared according to any one of claims 1 to 8, characterized in that: Calculated by mass percentage, the following raw materials are included: TiC powder 40-45%, TiN powder 10-20%, Ni powder 5-10%, Co powder 5-10%, WC powder 10-12%, MO2C powder 5-8%, and Cr3C2 powder 5-10%.