A kind of iron phosphide cobalt nickel nanoflower electrocatalytic material and preparation method thereof
By preparing CoNiFeP/NF self-supporting electrode material through hydrothermal method and phosphating reaction on nickel foam, the problems of high catalyst cost and large overpotential in electrolytic water hydrogen production technology are solved, and low-cost and efficient electrocatalytic performance is achieved. .
Patent Information
- Application Number
- CN202410969698.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In the existing electrolysis water hydrogen production technology, the cost of catalyst materials is high and the overpotential is large, which limits its wide application.
Using nickel foam as the matrix, CoNiFeP/NF self-supporting electrode material was prepared through hydrothermal method and phosphating reaction to form a honeycomb three-dimensional structure to improve the catalytic activity and electrocatalytic performance of the hydrogen evolution reaction.
It achieves low-cost and efficient electrocatalytic performance, has excellent electrocatalytic performance and stability, and significantly reduces overpotential and Tafel slope.
Smart Images

Figure CN118516704B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalytic materials, and specifically relates to an iron phosphide cobalt nickel nanoflower electrocatalytic material and a preparation method thereof. Background Art
[0002] At present, hydrogen production by water electrolysis is one of the main methods for obtaining hydrogen energy. In the process of water electrolysis, both hydrogen evolution reaction and oxygen evolution reaction have large overpotentials, so catalytic electrodes are often used to promote hydrogen evolution reaction and oxygen evolution reaction. Pt has good performance in water electrolysis and hydrogen evolution, and also plays an important role in the battery stack. However, since Pt is very expensive, its wide application is limited. Therefore, people are committed to developing a series of non-precious metal electrode materials represented by transition metals such as Co-based, Ni-based and Fe-based, and have achieved good results.
[0003] A Chinese invention patent with application number CN202110765459.0 and titled "Preparation and Application of a Bimetallic Phosphide Grown on Nickel Foam and Derived with a Prussian Blue Analogue as a Template" discloses a method for preparing a bimetallic phosphide grown on nickel foam and derived with a Prussian blue analogue as a template. First, nickel nitrate, urea, ammonium fluoride and nickel foam are hydrothermally reacted to obtain Ni(OH)2 / NF, and then Ni(OH)2 / NF and potassium ferrocyanide are used as raw materials to prepare a Prussian blue analogue NiFe PBA / NF by a simple hydrothermal method. Finally, NiFe PBA / NF is used as a template to obtain a bimetallic phosphide by phosphating. The bimetallic phosphide is used as an electrocatalyst in the oxygen evolution reaction of water electrolysis. Due to the formation of tetrahedral active sites and active phases, the interlaced structure and the presence of a three-dimensional nickel foam skeleton, it has excellent electrocatalytic performance in the oxygen evolution reaction of water electrolysis, has a small overpotential and a low Tafel slope, and has good stability.
[0004] A Chinese invention patent with application number CN202110228794.7 and titled "A Highly Active Self-Supporting OER Electrocatalyst Material, Preparation Method and Application Thereof" discloses a highly active self-supporting OER electrocatalyst material, preparation method and application thereof. The electrocatalyst material includes a nickel foam substrate and a NiFe2O4 / Ni3S4 / Ni(OH)2 material with a heterogeneous structure grown in situ on the nickel foam substrate. The present invention also provides a method for preparing the above-mentioned electrocatalyst material, comprising the steps of: placing the pretreated nickel foam in an iron source aqueous solution for hydrothermal reaction; after the reaction is completed, washing and drying to obtain a NiFe2O4 / Ni(OH)2 / NF composite material; placing the obtained NiFe2O4 / Ni(OH)2 / NF material in a sulfur source aqueous solution for sulfurization reaction; after the reaction is completed, washing and drying to obtain the obtained material.
[0005] It can be seen that preparing electrocatalytic materials with large specific surface area and dense active catalytic sites based on the three-dimensional skeleton of nickel foam is a way to prepare electrocatalytic materials at a lower cost. Summary of the invention
[0006] The present invention aims to provide a high-performance, self-supporting catalytic material for producing hydrogen through water electrolysis.
[0007] In order to solve the above technical problems, the present invention discloses an iron phosphide cobalt nickel nanoflower electrocatalytic material, wherein the electrocatalytic material is a CoNiFeP / NF self-supporting electrode prepared with nickel foam as a matrix.
[0008] Preferably, the CoNiFeP / NF self-supporting electrode material needs to complete multiple cyclic voltammetry curves to activate and stabilize the catalytic material when testing the hydrogen evolution performance.
[0009] A method for preparing an iron phosphide cobalt nickel nanoflower electrocatalytic material comprises at least the following steps:
[0010] S1. Ultrasonic cleaning of nickel foam was performed with acetone, 0.1 M HCl, ethanol and water respectively, each step was ultrasonically cleaned for 15 min, and the cleaned nickel foam was placed in a vacuum oven at 50-60°C to dry; in Co(NO3)2·6H2O solution, the reaction was carried out at 110-130°C by hydrothermal method for 10-15 hours, and basic cobalt carbonate nanoarrays were grown on the cleaned nickel foam as a precursor, and the mixture was cooled to room temperature. The nickel foam was taken out and washed with water and ethanol for several times, and then placed in a vacuum oven at 50-60°C to dry for 5-10 hours to obtain CoCH / NF nanoarrays;
[0011] S2. Using a mixed solution of Ni(NO3)2·6H2O and Fe(NO3)3·9H2O, the CoCH / NF nanoarray was subjected to a hydrothermal method again, heated to 110-130°C for reaction for 8-10h, and after completion, the nickel foam was taken out and washed several times with water and ethanol, and then dried in a vacuum oven at 50-60°C for 5-10h to obtain a CoCH / NiFe(OH)x / NF precursor;
[0012] S3. Low-temperature phosphating: The CoCH / NiFe(OH)x / NF precursor and sodium hypophosphite powder obtained in S2 are placed in two corundum porcelain boats respectively. The furnace of the tubular furnace is provided with a vacuum or inert gas atmosphere. The furnace is heated to 300°C and kept warm for 3-5 hours. The mixed-phase iron cobalt nickel phosphide / nickel foam electrochemical functional hydrogen evolution material, i.e., the CoNiFeP / NF self-supporting electrode, is obtained through the phosphating reaction.
[0013] Preferably, in S3, the corundum porcelain boat containing sodium hypophosphite powder is placed downstream of the tube furnace, and the corundum porcelain boat containing CoCH / NiFe(OH)x / NF precursor is placed downstream of the tube furnace. The placement distance between the two corundum porcelain boats is not more than 8 cm, and the placement height difference is not more than 2 cm.
[0014] Preferably, in S3, the corundum porcelain boat containing sodium hypophosphite powder and the corundum porcelain boat containing CoCH / NiFe(OH)x / NF precursor are stacked up and down in a cross shape, with the corundum porcelain boat containing sodium hypophosphite powder at the bottom.
[0015] Preferably, in S3, the mass ratio of the CoCH / NiFe(OH)x / NF precursor to the sodium hypophosphite powder is 1:5-1:7.
[0016] Preferably, in S3, the mass ratio of the CoCH / NiFe(OH)x / NF precursor to the sodium hypophosphite powder is 1:6.
[0017] Preferably, in S3, the inert gas is argon.
[0018] The iron phosphide cobalt nickel nanoflower electrocatalytic material and preparation method thereof of the present invention have at least the following advantages:
[0019] (1) The production process is simple and the cost is low: After the precursor is prepared by two hydrothermal reactions, low-temperature phosphating is performed to in situ grow a heterogeneous structure of mixed-phase iron phosphide, cobalt nickel, on the porous skeleton of nickel foam, forming a honeycomb-like three-dimensional structure with a large specific surface area and more exposed active sites. The synergistic effect between the mixed-phase iron phosphide, cobalt nickel, and the catalytic activity of the hydrogen evolution reaction is greatly improved, so that the material of the present invention has self-supporting properties and excellent electrocatalytic performance.
[0020] (2) The CoCH / NiFe(OH)x / NF precursor and sodium hypophosphite powder were placed in two corundum boats. The different placement positions of the two corundum boats caused slight differences in the mixed phase components, which in turn led to changes in the catalytic efficiency of the iron phosphide cobalt nickel nanoflower electrocatalytic material. Through comparison and optimization, the catalytic performance of the material was further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope image of the CoNiFeP / NF material of the present invention;
[0022] Figure 2 3 is a performance comparison diagram of the CoNiFeP / NF-based electrocatalytic material of the present invention in hydrogen evolution, wherein the abscissa is the potential relative to the reversible hydrogen electrode (RHE). DETAILED DESCRIPTION
[0023] The present invention is further described in detail below through examples so that those skilled in the art can implement the invention with reference to the description.
[0024] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0025] Example 1
[0026] A CoNiFeP / NF self-supporting electrode prepared from nickel foam as a matrix. Figure 1 The scanning electron microscope image of the CoNiFeP / NF material shown shows the surface microstructure of the material.
[0027] When testing the hydrogen evolution performance of the CoNiFeP / NF self-supporting electrode material, it is necessary to complete multiple (such as not less than 5) cyclic voltammetry curves to activate and stabilize the catalytic material.
[0028] Example 2
[0029] A method for preparing an iron phosphide cobalt nickel nanoflower electrocatalytic material comprises at least the following steps:
[0030] S1. Ultrasonic cleaning of nickel foam was performed with acetone, 0.1 M HCl, ethanol and water respectively, with each step being ultrasonically cleaned for 15 min, and the cleaned nickel foam was placed in a vacuum oven at 60°C for drying; in Co(NO3)2·6H2O solution, a hydrothermal method was used to react at 120°C for 10 h, and basic cobalt carbonate nanoarrays were grown on the cleaned nickel foam as a precursor, and the mixture was cooled to room temperature. The nickel foam was taken out and cleaned with water and ethanol for several times, and then placed in a vacuum oven at 60°C for drying for 8 h to obtain CoCH / NF nanoarrays;
[0031] S2. Using a mixed solution of Ni(NO3)2·6H2O and Fe(NO3)3·9H2O, the CoCH / NF nanoarray was subjected to a hydrothermal method again, heated to 120°C for 10 hours, and then the nickel foam was taken out and washed several times with water and ethanol, and dried in a vacuum oven at 60°C for 8 hours to obtain the CoCH / NiFe(OH)x / NF precursor;
[0032] S3. Low temperature phosphating: The CoCH / NiFe(OH)x / NF precursor obtained in S2 and sodium hypophosphite powder (CoCH / NiFe(OH)x / NF: NaH2PO2·H2O= 1:6) are placed in two corundum porcelain boats (60*30mm specification), and the furnace of the tube furnace is provided with a vacuum or inert gas atmosphere, and the furnace is heated to 300°C and kept warm for 5 hours; a mixed phase iron cobalt nickel phosphide / nickel foam electrochemical functional hydrogen evolution material, i.e., CoNiFeP / NF self-supporting electrode, is obtained through phosphating reaction. Through electron microscopy observation, the surface nanostructure of the CoCH / NiFe(OH)x / NF precursor prepared by the method of the present invention is relatively smooth and flat. After phosphating, it can be found that the morphology of the surface nanostructure is still maintained and becomes more compact (such as Figure 1 In contrast, the surface nanostructure morphology of the CoCH / NF precursor is destroyed during the phosphating process, and nanoparticles CoP are still attached to its surface, especially on the edge, which is not conducive to the stability of the material's catalytic performance. Relatively speaking, after the surface treatment by this method, the surface nanostructure of the CoCH / NiFe(OH)x / NF precursor can remain relatively stable during the phosphating process. The surface nanostructure of this CoNiFeP / NF material can expose more active sites and promote the release of oxygen / hydrogen bubbles during water decomposition.
[0033] In S3, the corundum boat containing sodium hypophosphite powder is placed upstream of the tube furnace, and the corundum boat containing CoCH / NiFe(OH)x / NF precursor is placed downstream of the tube furnace. The two corundum boats are placed side by side.
[0034] In S3, the inert gas is argon.
[0035] After the CoNiFeP / NF self-supporting electrode material completed 10 cyclic voltammetry curves, the hydrogen evolution performance was tested under alkaline conditions and compared with the hydrogen evolution performance of CoP / NF and NiFeP / NF materials based on nickel foam. The results are as follows Figure 2 As shown (the rightmost curve is the hydrogen evolution performance measurement curve of the CoNiFeP / NF self-supporting electrode material), it can be seen that the CoNiFeP / NF self-supporting electrode material prepared by the method of the present invention has better hydrogen evolution performance.
[0036] Example 3
[0037] Similar to Example 2, the difference is that in S3, the corundum porcelain boat containing sodium hypophosphite powder and the corundum porcelain boat containing CoCH / NiFe(OH)x / NF precursor are stacked up and down in a cross shape, with the corundum porcelain boat containing sodium hypophosphite powder at the bottom. The CoNiFeP / NF self-supporting electrode material obtained after low-temperature phosphating is compared with the CoNiFeP / NF self-supporting electrode material in Example 2. The hydrogen evolution performance is found to be improved by 0.1%-0.3% in the CoNiFeP / NF self-supporting electrode material in this embodiment. We analyzed that the placement of different corundum porcelain boats has a certain influence on the change in the ratio of the mixed components in the formed mixed-phase iron cobalt nickel phosphide / nickel foam, which in turn leads to a slight change in the synergistic effect between the mixed-phase iron cobalt nickel phosphide, thereby leading to a change in the hydrogen evolution performance of the material.
[0038] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.
Claims
1. A method for preparing an iron phosphide cobalt nickel nanoflower electrocatalytic material, characterized in that: The iron phosphide cobalt nickel nanoflower electrocatalytic material is a CoNiFeP / NF self-supporting electrode prepared with nickel foam as the matrix; when testing the hydrogen evolution performance, the CoNiFeP / NF self-supporting electrode material needs to complete multiple cyclic voltammetry curves to activate and stabilize the catalytic material; The method for preparing the iron phosphide cobalt nickel nanoflower electrocatalytic material comprises at least the following steps: S1. Ultrasonic cleaning of nickel foam was performed with acetone, 0.1M HCl, ethanol and water respectively, with each step being ultrasonically cleaned for 15 min, and the cleaned nickel foam was placed in a vacuum oven at 50-60°C to dry; in Co(NO3)2·6H2O solution, a hydrothermal method was used to react at 110-130ºC for 10-15 hours, and basic cobalt carbonate nanoarrays were grown on the cleaned nickel foam as a precursor, and the mixture was cooled to room temperature. The nickel foam was taken out and cleaned with water and ethanol for several times, and then placed in a vacuum oven at 50-60°C to dry for 5-10 hours to obtain CoCH / NF nanoarrays; S2. Using a mixed solution of Ni(NO3)2·6H2O and Fe(NO3)3·9H2O, the CoCH / NF nanoarray was heated to 110-130ºC for 8-10h by hydrothermal method. After completion, the nickel foam was taken out and washed with water and ethanol several times, and then dried in a vacuum oven at 50-60℃ for 5-10h to obtain the CoCH / NiFe(OH)x / NF precursor. S3. Low-temperature phosphating: The CoCH / NiFe(OH)x / NF precursor obtained in S2 and the sodium hypophosphite powder are placed in two corundum porcelain boats respectively, and the furnace of the tube furnace is provided with a vacuum or inert gas atmosphere, and the furnace is heated to 300°C and kept warm for 3-5 hours; a mixed phase iron cobalt nickel phosphide / nickel foam electrochemical functional hydrogen evolution material, i.e., CoNiFeP / NF self-supporting electrode, is obtained through phosphating reaction; In S3, the corundum porcelain boat containing sodium hypophosphite powder is placed upstream of the tube furnace, and the corundum porcelain boat containing CoCH / NiFe(OH)x / NF precursor is placed downstream of the tube furnace, and the two corundum porcelain boats are arranged side by side next to each other; or, in S3, the corundum porcelain boat containing sodium hypophosphite powder and the corundum porcelain boat containing CoCH / NiFe(OH)x / NF precursor are stacked up and down in a cross shape, with the corundum porcelain boat containing sodium hypophosphite powder at the bottom.
2. The method for preparing the iron phosphide cobalt nickel nanoflower electrocatalytic material according to claim 1, characterized in that: In S3, the mass ratio of the CoCH / NiFe(OH)x / NF precursor to the sodium hypophosphite powder is 1:5-1:
7.
3. The method for preparing the iron phosphide cobalt nickel nanoflower electrocatalytic material according to claim 2, characterized in that: In S3, the mass ratio of the CoCH / NiFe(OH)x / NF precursor to the sodium hypophosphite powder is 1:
6.