A method for preparing durable flame retardant coated polyester fabric

By coating the ammonium polyphosphate flame retardant with cyclodextrin and scraping it in the polyurethane emulsion, the problems of poor compatibility and insufficient stability of the flame retardant polyurethane coating are solved, and efficient flame retardant and water-resistant properties are achieved. Improves the durability of the coating.

CN118516866BActive Publication Date: 2024-11-19JIANGSU HENGLI CHEM FIBER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410985975.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-19
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing flame retardant polyurethane coatings have problems such as poor compatibility, poor stability, poor adhesion performance and insufficient washing resistance during use, especially the poor compatibility between ammonium polyphosphate as an inorganic substance and polymer. , resulting in unsatisfactory flame retardant performance.

Method used

Cyclodextrin coated ammonium polyphosphate flame retardant is used to carry out esterification reactions at a specific temperature by dicyandiamide and sodium hypophosphite catalysts to form a cyclodextrin coated ammonium polyphosphate flame retardant, and mix it into polyurethane. The emulsion is scraped and pre-baked and baked to produce a durable flame-retardant coated polyester fabric.

Benefits of technology

The compatibility and stability of ammonium polyphosphate and polyurethane are improved, the adhesion and washing resistance of the flame retardant coating are enhanced, and the flame retardant efficiency and the durability of the coating are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of flame retardant coating materials, and relates to a method for preparing a durable flame retardant coating polyester fabric, wherein the preparation method is as follows: first, cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite are added to a mixed solution of N,N-dimethylformamide and water, and reacted at 70-80°C to obtain a cyclodextrin-coated ammonium polyphosphate flame retardant, and then the cyclodextrin-coated ammonium polyphosphate flame retardant is mixed into a polyurethane emulsion to obtain a scraping liquid, and then the scraping liquid is used to scrape the polyester fabric, and then the durable flame retardant coating polyester fabric is obtained after pre-baking and baking. The cyclodextrin-coated ammonium polyphosphate flame retardant of the invention has good compatibility between cyclodextrin and ammonium polyphosphate, has high stability, and is not easy to precipitate, and the flame retardant coating polyester fabric prepared by the cyclodextrin-coated ammonium polyphosphate flame retardant has good water washing resistance and flame retardant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant coating materials and relates to a method for preparing a durable flame retardant coated polyester fabric. Background Art

[0002] At present, the flame retardant performance of polyester fabrics is usually improved by flame retardant polyurethane coating. This method is favored because of its easy operation, good durability and wide application prospects. The combination of flame retardants and polyurethane is usually carried out by adding blending and copolymerization. (i) Addition blending, that is, directly adding flame retardants to polyurethane to form flame retardant polyurethane, has become the current research focus due to its simple operation and cost-effectiveness; (ii) Copolymerization, although the flame retardant can be chemically reacted with the polyurethane macromolecular chain segment, the preparation process is cumbersome and costly, so it is rarely used in industrial applications.

[0003] Ammonium polyphosphate, a phosphorus-nitrogen composite material, has become the best halogen-free flame retardant for flame retardant modification of polyurethane and its coated textiles due to its low cost, low toxicity and excellent flame retardant effect. However, as an inorganic substance, ammonium polyphosphate has problems such as poor compatibility with polymers, easy migration and exudation, and reduced mechanical properties of the polymer matrix. Therefore, ammonium polyphosphate is usually modified by coupling agent treatment or microencapsulation.

[0004] For example, in the literature (Research on the flame retardant properties of microencapsulated ammonium polyphosphate polyurethane rigid foam [J]. Plastic Industry, 2017, 45(8): 105-108.), ammonium polyphosphate (APP) is coated with melamine resin and aluminum hydroxide as coating materials to obtain melamine formaldehyde resin microencapsulated APP (MF-APP) and aluminum hydroxide microencapsulated APP (ATH-APP), and then MF-APP, ATH-APP and uncoated APP are used as white materials, and polyisocyanate is used as black material to prepare full water foamed flame retardant polyurethane rigid foam (RPUF) by a one-step method. The prepared melamine formaldehyde resin has high viscosity, but it will release formaldehyde during use, which is harmful to the human body.

[0005] In addition, conventional coating materials cannot form covalent bonds with ammonium polyphosphate, and their compatibility with ammonium polyphosphate is also poor, with defects such as low coating efficiency and instability. When the flame-retardant polyurethane prepared by them is used as a coating finishing agent for textiles, it cannot meet the requirements of high adhesion, water washability and compatibility between flame-retardant polyurethane and textiles. In addition, with the continuous improvement of environmental awareness, the use of natural polymer materials to prepare coated ammonium polyphosphate flame retardants has become a current research hotspot. Cyclodextrin is a natural cyclic oligosaccharide compound whose molecules are cone-shaped, so it has a cavity structure and has good compatibility with polyurethane, providing a new direction for the modification of flame retardants.

[0006] For example, patent application CN105176061A discloses a method for preparing a flame-retardant polyurethane resin, wherein the preparation method is to coat resorcinol bis(diphenyl) phosphate RDP with cyclodextrin to obtain a cyclodextrin / RDP inclusion compound, and a flame-retardant polyurethane resin is developed using the cyclodextrin / RDP inclusion compound. However, the flame retardant resorcinol bis(diphenyl) phosphate mainly enters the cavity of cyclodextrin, so that the cyclodextrin / RDP inclusion compound has good compatibility with polyurethane, but the cavity of cyclodextrin is large and has always been in an open state, and the flame retardant resorcinol bis(diphenyl) phosphate can easily migrate out of the cyclodextrin cavity, contact with the polyurethane material and further migrate, resulting in poor stability of the flame-retardant polyurethane resin.

[0007] Therefore, it is of great significance to study a method for preparing a durable flame retardant coated polyester fabric to solve the above problems. Summary of the invention

[0008] The purpose of the invention is to solve the problems existing in the prior art and provide a method for preparing a durable flame retardant coated polyester fabric.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a durable flame-retardant coated polyester fabric comprises mixing a cyclodextrin-coated ammonium polyphosphate flame retardant into a polyurethane emulsion to obtain a coating liquid, then coating the polyester fabric with the coating liquid, and then pre-baking and baking to obtain the durable flame-retardant coated polyester fabric.

[0011] The cyclodextrin-coated ammonium polyphosphate flame retardant is obtained by adding cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and reacting at 70-80°C. In this process, dicyandiamide and sodium hypophosphite are catalysts. Both dicyandiamide and sodium hypophosphite can catalyze the esterification reaction between the alcohol hydroxyl groups in the cyclodextrin molecules and the ammonium phosphate groups of ammonium polyphosphate. The combination of the two can play a more efficient role. The role of N,N-dimethylformamide is to promote the swelling of ammonium polyphosphate and the dissolution of cyclodextrin. In addition, the reaction temperature of 70-80°C can also help to increase the movement of ammonium polyphosphate molecules and enter the cyclodextrin cavity, but too high a temperature will result in waste.

[0012] As the preferred technical solution:

[0013] In the method for preparing a durable flame-retardant coated polyester fabric as described above, the content of cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 10-15wt%. Although a high amount of cyclodextrin-coated ammonium polyphosphate flame retardant will have a good flame retardant effect, a too high amount will be wasteful.

[0014] As described above, in the method for preparing a durable flame-retardant coated polyester fabric, the pre-baking temperature is 70~80°C, and the pre-baking time is 2~4 minutes; the baking temperature is 150~170°C, and the baking time is 3~5 minutes. The purpose of setting the baking temperature and time in this way is to ensure that the polyurethane can form a good film on the surface of the polyester fabric.

[0015] The method for preparing a durable flame retardant coated polyester fabric as described above, wherein the coating amount of the durable flame retardant coated polyester fabric is 30-50 g / m 2 .

[0016] The method for preparing a durable flame-retardant coated polyester fabric as described above, the specific preparation process of the cyclodextrin-coated ammonium polyphosphate flame retardant is as follows: first, cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite are added to a mixture of N,N-dimethylformamide and water, and the mixture is stirred and reacted at 70-80°C for 2-3 hours. After the reaction, the mixture of N,N-dimethylformamide and water is distilled under reduced pressure until 1 / 4-1 / 3 of the mixture remains, which helps to create a humid environment and promote the reaction between ammonium polyphosphate and cyclodextrin during high-temperature drying. The product is then dried, washed and dried in sequence to obtain the cyclodextrin-coated ammonium polyphosphate flame retardant.

[0017] In the preparation method of a durable flame-retardant coated polyester fabric as described above, the molar ratio of cyclodextrin to ammonium polyphosphate is 1:1~3. Theoretically, each cyclodextrin can coat multiple ammonium polyphosphates. Although a slight excess of cyclodextrin helps to coat the ammonium polyphosphate, too much cyclodextrin is wasteful, resulting in low coating efficiency; the molar ratio of dicyandiamide to ammonium polyphosphate is 0.5~0.7:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.3~0.5:1, the dosage ratio of ammonium polyphosphate to N,N-dimethylformamide is 1g:2~3mL, and the volume ratio of N,N-dimethylformamide to water is 1:1~1.2.

[0018] In the method for preparing a durable flame retardant coated polyester fabric as described above, the pressure of the vacuum distillation is 35-45 kPa and the temperature is 40-50° C.;

[0019] The drying temperature is 145~155℃ and the time is 1~2h. This drying temperature is more conducive to promoting the esterification reaction between ammonium polyphosphate and cyclodextrin.

[0020] Washing means washing with ethanol for 3 times, and the ratio of ethanol to product in each washing is 10-15 mL:1 g;

[0021] The drying temperature is 70~90℃ and the time is 30~50min, so that the ethanol can be completely evaporated.

[0022] According to the preparation method of the durable flame retardant coated polyester fabric as described above, the damaged length of the durable flame retardant coated polyester fabric is not higher than 12.0 cm, and the damaged length after 35 times of washing is not higher than 14.0 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 13.9-14.3N (the peeling force between the non-flame retardant polyurethane coating and the polyester fabric is 15.1N, and the peeling force between the unmodified ammonium polyphosphate polyurethane coating and the polyester fabric is 10.2N), indicating that the cyclodextrin-coated ammonium polyphosphate flame retardant has little effect on the adhesion performance of polyurethane, has better compatibility with polyurethane, and the flame retardant coated polyester fabric has good water washing resistance.

[0023] The principle of the present invention is:

[0024] The cyclodextrin molecule contains a cavity inside, and can enclose ammonium polyphosphate to form an inclusion complex through physical coating; in the presence of dicyandiamide and sodium hypophosphite catalysts, the alcohol hydroxyl group in the cyclodextrin molecule undergoes an esterification reaction with the ammonium phosphate group of ammonium polyphosphate, and the ammonium polyphosphate is fixed in the cyclodextrin to obtain a cyclodextrin-coated ammonium polyphosphate flame retardant; the cyclodextrin encapsulates the ammonium polyphosphate in the internal cavity through physical and chemical bonding (specifically covalent bonding), the two have good compatibility and a relatively stable combination, the ammonium polyphosphate particles are not easy to diffuse out of the cyclodextrin, and the coating stability is good.

[0025] The surface of cyclodextrin molecules contains a large number of hydroxyl groups, which have good compatibility with the hydroxyl groups and ester bonds in polyurethane molecules. The ammonium polyphosphate coated with cyclodextrin is organically combined through the high adhesion between the surface cyclodextrin and the polyurethane. After being coated and modified with cyclodextrin, the ammonium polyphosphate does not have direct contact with the polyurethane, can be well dispersed in the polyurethane, and has high stability and is not easy to precipitate. It has little effect on the adhesion performance of the flame-retardant polyurethane coating, and the flame-retardant coated polyester fabric has good water washing resistance.

[0026] In addition, ammonium polyphosphate is an efficient acid source and gas source, and cyclodextrin as a polysaccharide compound is an efficient carbon-forming agent. Ammonium polyphosphate decomposes to produce polyphosphoric acid and ammonia during heating. Polyphosphoric acid can effectively catalyze the decomposition of cyclodextrin into carbon. The flame retardant system improves the flame retardant properties of coated polyester fabrics through the expansion flame retardant mechanism and has high flame retardant efficiency.

[0027] Beneficial effects:

[0028] (1) The cyclodextrin of the present invention encapsulates ammonium polyphosphate in the internal cavity by means of physical and chemical bonding, so that the ammonium polyphosphate does not come into direct contact with the polyurethane and can be well dispersed in the polyurethane. The cyclodextrin and the ammonium polyphosphate have good compatibility, high stability, and are not easy to precipitate. The cyclodextrin has little effect on the adhesion performance of the flame-retardant polyurethane coating, thereby making the flame-retardant coated polyester fabric have good water-washing resistance.

[0029] (2) The ammonium polyphosphate of the present invention decomposes to produce polyphosphoric acid and ammonia during heating. The polyphosphoric acid can effectively catalyze the decomposition of cyclodextrin into carbon. The flame retardant system improves the flame retardant properties of the coated polyester fabric through an expansion flame retardant mechanism and has a high flame retardant efficiency. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0031] The testing methods of the relevant performance indicators in the following embodiments and comparative examples are as follows:

[0032] Damage length: GB / T 5455-2014 “Determination of damage length in vertical direction, smoldering and afterflaming time of textile combustion performance” is used to test the damage length of flame retardant coated polyester fabric.

[0033] Damaged length after 35 washes: In the present invention, the flame retardant coated polyester fabric is washed according to AATCC 61-2013 "Accelerated Test for Color Fastness to Laundering for Household and Commercial Use".

[0034] Peel force: Refer to FZ∕T 01085-2018 "Test method for peel strength of adhesive interlining" to test the peel force of flame retardant coated polyester fabric.

[0035] Example 1

[0036] A method for preparing a durable flame retardant coated polyester fabric, comprising the following steps:

[0037] (1) Preparation of raw materials;

[0038] β-cyclodextrin: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number C804562;

[0039] Ammonium polyphosphate: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., the product number is A875132;

[0040] Dicyandiamide;

[0041] Sodium hypophosphite;

[0042] A mixture of N,N-dimethylformamide and water: the volume ratio of N,N-dimethylformamide to water is 1:1.2;

[0043] Polyurethane emulsion: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number W909580;

[0044] (2) Preparation of β-cyclodextrin-coated ammonium polyphosphate flame retardant;

[0045] (2.1) Add β-cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and stir at 75°C for 2.5 h; wherein the molar ratio of β-cyclodextrin to ammonium polyphosphate is 1:2, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.6:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.4:1, and the amount ratio of ammonium polyphosphate to N,N-dimethylformamide is 1 g:2.5 mL;

[0046] (2.2) After the reaction in step (2.1) is completed, vacuum distillation is performed at 45°C and 40 kPa until 1 / 4 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried at 150°C for 1.5 hours, and then the dried product is washed with ethanol for 3 times, and finally dried at 80°C for 40 minutes to obtain β-cyclodextrin-coated ammonium polyphosphate flame retardant; wherein the ratio of ethanol to product used in each washing is 13 mL:1 g;

[0047] (3) The β-cyclodextrin-coated ammonium polyphosphate flame retardant prepared in step (2) is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, followed by pre-baking at 75°C for 3 minutes, and finally baking at 160°C for 4 minutes to obtain a polyester fabric with a durable flame retardant coating; wherein the content of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 12.5wt%.

[0048] The coating amount of the final durable flame retardant coated polyester fabric is 40g / m 2 The damaged length of the durable flame retardant coated polyester fabric is 10.5 cm, and the damaged length after 35 washes is 13.1 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 14.1N.

[0049] Comparative Example 1

[0050] A method for preparing a flame-retardant coated polyester fabric is basically the same as that in Example 1, except that step (2) is not performed, and the β-cyclodextrin-coated ammonium polyphosphate flame retardant in step (3) is replaced by an ammonium polyphosphate flame retardant of equal mass (manufacturer and product number are the same as those in Example 1).

[0051] The damaged length of the flame-retardant coated polyester fabric finally obtained was 13.5 cm, and the damaged length after 35 times of washing was 30 cm. The peeling force between the coating and the polyester fabric in the durable flame-retardant coated polyester fabric was 11.5N.

[0052] By comparing Comparative Example 1 with Example 1, it can be seen that the flame retardant property of the flame-retardant coated polyester fabric prepared in Comparative Example 1 is reduced, the water washing resistance is reduced, and the peeling force between the coating and the polyester fabric is reduced. This is because the compatibility of ammonium polyphosphate in polyurethane is poor, and the dispersion performance in polyurethane is poor, which makes the polyurethane coating formed on the polyester fabric have poor film-forming properties, thereby causing the coating to easily crack during the washing process; in addition, due to the poor compatibility of ammonium polyphosphate with polyurethane, the ammonium polyphosphate and polyurethane are not firmly combined, so that the ammonium polyphosphate will precipitate between the polyurethane coating and the fabric, affecting the adhesion performance of the flame-retardant polyurethane coating to the polyester fabric. During the washing process, the ammonium polyphosphate will be slowly washed away, and ultimately the flame retardant property of the flame-retardant coated polyester fabric is reduced.

[0053] Comparative Example 2

[0054] A method for preparing a flame-retardant coated polyester fabric is basically the same as that of Example 1, except that: in step (2.1), β-cyclodextrin and ammonium polyphosphate are added to a mixture of N,N-dimethylformamide and water, and dicyandiamide and sodium hypophosphite are not added.

[0055] The damaged length of the flame-retardant coated polyester fabric finally obtained was 12.8 cm, and the damaged length after 35 times of washing was 30 cm. The peeling force between the coating and the polyester fabric in the durable flame-retardant coated polyester fabric was 12.3N.

[0056] By comparing Comparative Example 2 with Example 1, it can be seen that the flame retardant properties of the flame-retardant coated polyester fabric prepared in Comparative Example 2 are reduced, and the water washing resistance is reduced. This is because dicyandiamide and sodium hypophosphite, as catalysts, can catalyze the esterification reaction between the alcohol hydroxyl groups in the cyclodextrin molecules and the ammonium phosphate groups of ammonium polyphosphate, and the combination of the two can also play a more efficient role. The lack of the catalytic effect of the two in Comparative Example 2 will lead to insufficient coating of ammonium polyphosphate by cyclodextrin, and ammonium polyphosphate can easily diffuse out from the cyclodextrin cavity, thereby reducing the dispersibility of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in polyurethane, and affecting the adhesion of the flame retardant coating to the polyester fabric, so that the water washing resistance of the flame retardant coated polyester fabric is reduced; in addition, due to the poor dispersibility of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in polyurethane, it will eventually lead to a reduction in the flame retardant properties of the flame retardant coated polyester fabric.

[0057] Example 2

[0058] A method for preparing a durable flame retardant coated polyester fabric, comprising the following steps:

[0059] (1) Preparation of raw materials;

[0060] β-cyclodextrin: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number C804562;

[0061] Ammonium polyphosphate: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., the product number is A875132;

[0062] Dicyandiamide;

[0063] Sodium hypophosphite;

[0064] A mixture of N,N-dimethylformamide and water: the volume ratio of N,N-dimethylformamide to water is 1:1.1;

[0065] Polyurethane emulsion: water-based polyurethane, manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number W909580;

[0066] (2) Preparation of β-cyclodextrin-coated ammonium polyphosphate flame retardant;

[0067] (2.1) Add β-cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and stir at 73°C for 2.8 h; wherein the molar ratio of β-cyclodextrin to ammonium polyphosphate is 1:1.5, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.55:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.35:1, and the amount ratio of ammonium polyphosphate to N,N-dimethylformamide is 1 g:2.3 mL;

[0068] (2.2) After the reaction in step (2.1) is completed, vacuum distillation is performed at 42°C and 38 kPa until 1 / 3 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried at 148°C for 1.8 hours, and then the dried product is washed with ethanol for 3 times, and finally dried at 75°C for 45 minutes to obtain β-cyclodextrin-coated ammonium polyphosphate flame retardant; wherein the ratio of ethanol to product used in each washing is 12 mL: 1 g;

[0069] (3) The β-cyclodextrin-coated ammonium polyphosphate flame retardant prepared in step (2) is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, followed by pre-baking at 73° C. for 3.5 min, and finally baking at 155° C. for 4.5 min to obtain a polyester fabric with a durable flame retardant coating; wherein the content of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 11 wt %.

[0070] The coating weight of the final durable flame retardant coated polyester fabric is 35g / m 2 The damaged length of the durable flame retardant coated polyester fabric is 11.2 cm, and the damaged length after 35 washes is 13.5 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 14.2N.

[0071] Example 3

[0072] A method for preparing a durable flame retardant coated polyester fabric, comprising the following steps:

[0073] (1) Preparation of raw materials;

[0074] β-cyclodextrin: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number C804562;

[0075] Ammonium polyphosphate: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., the product number is A875132;

[0076] Dicyandiamide;

[0077] Sodium hypophosphite;

[0078] A mixture of N,N-dimethylformamide and water: the volume ratio of N,N-dimethylformamide to water is 1:1;

[0079] Polyurethane emulsion: water-based polyurethane, manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number W909580;

[0080] (2) Preparation of β-cyclodextrin-coated ammonium polyphosphate flame retardant;

[0081] (2.1) Add β-cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and stir at 70°C for 3 h; wherein the molar ratio of β-cyclodextrin to ammonium polyphosphate is 1:1, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.5:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.3:1, and the amount ratio of ammonium polyphosphate to N,N-dimethylformamide is 1 g:2 mL;

[0082] (2.2) After the reaction in step (2.1) is completed, vacuum distillation is performed at 40°C and 35 kPa until 1 / 4 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried at 145°C for 2 hours, and then the dried product is washed with ethanol for 3 times, and finally dried at 70°C for 50 minutes to obtain β-cyclodextrin-coated ammonium polyphosphate flame retardant; wherein the ratio of ethanol to product used in each washing is 10 mL: 1 g;

[0083] (3) The β-cyclodextrin-coated ammonium polyphosphate flame retardant prepared in step (2) is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, followed by pre-baking at 70° C. for 4 min, and finally baking at 150° C. for 5 min, to obtain a polyester fabric with a durable flame retardant coating; wherein the content of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 10 wt %.

[0084] The coating amount of the final durable flame retardant coated polyester fabric is 30g / m 2The damaged length of the durable flame retardant coated polyester fabric is 12 cm, and the damaged length after 35 washes is 14 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 14.3N.

[0085] Example 4

[0086] A method for preparing a durable flame retardant coated polyester fabric, comprising the following steps:

[0087] (1) Preparation of raw materials;

[0088] β-cyclodextrin: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number C804562;

[0089] Ammonium polyphosphate: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., the product number is A875132;

[0090] Dicyandiamide;

[0091] Sodium hypophosphite;

[0092] A mixture of N,N-dimethylformamide and water: the volume ratio of N,N-dimethylformamide to water is 1:1.1;

[0093] Polyurethane emulsion: water-based polyurethane, manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number W909580;

[0094] (2) Preparation of β-cyclodextrin-coated ammonium polyphosphate flame retardant;

[0095] (2.1) Add β-cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and stir at 78°C for 2.3 h; wherein the molar ratio of β-cyclodextrin to ammonium polyphosphate is 1:2.5, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.65:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.45:1, and the amount ratio of ammonium polyphosphate to N,N-dimethylformamide is 1 g:2.8 mL;

[0096] (2.2) After the reaction in step (2.1) is completed, vacuum distillation is performed at 47°C and 43 kPa until 1 / 3 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried at 153°C for 1.3 h, and then the dried product is washed with ethanol for 3 times, and finally dried at 85°C for 35 min to obtain β-cyclodextrin-coated ammonium polyphosphate flame retardant; wherein the ratio of ethanol to product used in each washing is 15 mL:1 g;

[0097] (3) The β-cyclodextrin-coated ammonium polyphosphate flame retardant prepared in step (2) is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, followed by pre-baking at 78° C. for 2.5 min, and finally baking at 165° C. for 3.5 min to obtain a polyester fabric with a durable flame retardant coating; wherein the content of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 14 wt %.

[0098] The coating weight of the final durable flame retardant coated polyester fabric is 45g / m 2 The damaged length of the durable flame retardant coated polyester fabric is 9.9 cm, and the damaged length after 35 washes is 12.8 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 14.0N.

[0099] Example 5

[0100] A method for preparing a durable flame retardant coated polyester fabric, comprising the following steps:

[0101] (1) Preparation of raw materials;

[0102] β-cyclodextrin: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number C804562;

[0103] Ammonium polyphosphate: The manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd., the product number is A875132;

[0104] Dicyandiamide;

[0105] Sodium hypophosphite;

[0106] A mixture of N,N-dimethylformamide and water: the volume ratio of N,N-dimethylformamide to water is 1:1.2;

[0107] Polyurethane emulsion: manufacturer Shanghai MacLean Biochemical Technology Co., Ltd., product number W909580;

[0108] (2) Preparation of β-cyclodextrin-coated ammonium polyphosphate flame retardant;

[0109] (2.1) Add β-cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and stir at 80°C for 2 h; wherein the molar ratio of β-cyclodextrin to ammonium polyphosphate is 1:3, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.7:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.5:1, and the amount ratio of ammonium polyphosphate to N,N-dimethylformamide is 1 g:3 mL;

[0110] (2.2) After the reaction in step (2.1) is completed, vacuum distillation is performed at 50°C and 45 kPa until 1 / 4 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried at 155°C for 1 hour, and then the dried product is washed with ethanol for 3 times, and finally dried at 90°C for 30 minutes to obtain β-cyclodextrin-coated ammonium polyphosphate flame retardant; wherein the ratio of ethanol to product used in each washing is 14 mL:1 g;

[0111] (3) The β-cyclodextrin-coated ammonium polyphosphate flame retardant prepared in step (2) is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, followed by pre-baking at 80° C. for 2 min, and finally baking at 170° C. for 3 min, to obtain a polyester fabric with a durable flame retardant coating; wherein the content of the β-cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 15 wt %.

[0112] The coating amount of the final durable flame retardant coated polyester fabric is 50g / m 2 The damaged length of the durable flame retardant coated polyester fabric is 9.5 cm, and the damaged length after 35 washes is 12.4 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 13.9N.

Claims

1. A method for preparing a durable flame retardant coated polyester fabric, characterized in that: The cyclodextrin-coated ammonium polyphosphate flame retardant is mixed into a polyurethane emulsion to obtain a coating liquid, and then the coating liquid is used to coat a polyester fabric, and then the polyester fabric with a durable flame retardant coating is obtained after pre-baking and baking; The cyclodextrin-coated ammonium polyphosphate flame retardant is obtained by adding cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite to a mixture of N,N-dimethylformamide and water, and reacting at 70-80°C. The cyclodextrin coats the ammonium polyphosphate in the internal cavity by physical and chemical bonding. The content of cyclodextrin-coated ammonium polyphosphate flame retardant in the coating liquid is 10-15wt%; The damaged length of the durable flame retardant coated polyester fabric is no more than 12.0 cm, and the damaged length after 35 times of washing is no more than 14.0 cm. The peeling force between the coating and the polyester fabric in the durable flame retardant coated polyester fabric is 13.9~14.3N.

2. The method for preparing a durable flame retardant coated polyester fabric according to claim 1, characterized in that: The pre-baking temperature is 70~80℃, and the pre-baking time is 2~4min; the baking temperature is 150~170℃, and the baking time is 3~5min.

3. The method for preparing a durable flame retardant coated polyester fabric according to claim 1, characterized in that: Durable flame retardant coated polyester fabric coating weight is 30~50g / m 2 .

4. The method for preparing a durable flame retardant coated polyester fabric according to claim 1, characterized in that: The specific preparation process of cyclodextrin coated ammonium polyphosphate flame retardant is as follows: first, cyclodextrin, ammonium polyphosphate, dicyandiamide and sodium hypophosphite are added to a mixture of N,N-dimethylformamide and water, and stirred for reaction at 70-80°C for 2-3 hours. After the reaction, reduced pressure distillation is performed until 1 / 4-1 / 3 of the mixture of N,N-dimethylformamide and water remains, and then the product is dried, washed and dried in sequence to obtain cyclodextrin coated ammonium polyphosphate flame retardant.

5. The method for preparing a durable flame retardant coated polyester fabric according to claim 4, characterized in that: The molar ratio of cyclodextrin to ammonium polyphosphate is 1:1-3, the molar ratio of dicyandiamide to ammonium polyphosphate is 0.5-0.7:1, the molar ratio of sodium hypophosphite to ammonium polyphosphate is 0.3-0.5:1, the dosage ratio of ammonium polyphosphate to N,N-dimethylformamide is 1g:2-3mL, and the volume ratio of N,N-dimethylformamide to water is 1:1-1.

2.

6. The method for preparing a durable flame retardant coated polyester fabric according to claim 4, characterized in that: The pressure of vacuum distillation is 35~45kPa and the temperature is 40~50℃; The drying temperature is 145~155℃ and the time is 1~2h; Washing means washing with ethanol for 3 times, and the ratio of ethanol to product in each washing is 10-15 mL:1 g; The drying temperature is 70~90℃ and the time is 30~50min.

Citation Information

Patent Citations

  • Preparation method of flame-retardant polyurethane resin

    CN105176061A

  • Watersoluble coating glue containing multiple coating modified poly-ammonium phosphate and uses on textile finishing

    CN101492881A

  • Flame-retardant coating adhesive for textile, finishing method of flame-retardant fabric with flame-retardant coating adhesive and flame-retardant fabric with flame-retardant coating adhesive

    CN104862971A