A low-voltage and low-capacity SCR structure protection device and a manufacturing method thereof

By adopting specific region structure and rapid thermal annealing technology in low-voltage and low-capacitance SCR structure protection devices, a sudden PN junction is formed, which solves the problem of leakage current and capacitance increase, and achieves lower breakdown voltage and higher ESD anti-interference capability, optimizes the device's parameter performance.

CN118522731BActive Publication Date: 2024-11-29JIANGSU JILAI MICROELECTRONICS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410997338.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-29
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

While the existing low-voltage and low-capacitance SCR structure protection devices improve the breakdown voltage and ESD anti-interference ability, they easily lead to an increase in leakage current and an increase in capacitance, and soft breakdown occurs in breakdown characteristics, affecting their application in integrated circuits.

Method used

By forming specific P-region, N+region and P+region structures on the N-single wafer, and using slot design and rapid thermal annealing technology, a sudden PN junction is formed, reducing the overall capacitance and leakage current of the device, while improving breakdown. Voltage to improve ESD anti-interference capability.

Benefits of technology

It realizes that the chip area remains unchanged, and the lower breakdown voltage, lower capacitance and higher ESD anti-interference ability can be obtained. The parameters are optimized to VRWM=2.5V, VBR=3.3~7.0V, IR≤1μA , IPP≥5A, Cj=0.8~1.0pF, VESD≥±20KV.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118522731B_ABST
    Figure CN118522731B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-voltage and low-capacitance SCR structure protection device and a manufacturing method thereof, wherein the device comprises an N-single crystal, a P-region formed on the surface of the N-single crystal, a first N+ region, a second N+ region, a third N+ region, a first P+ region, a second P+ region, a third P+ region, a fourth P+ region, a dielectric layer arranged above the N-single crystal, and a first metal layer and a second metal layer arranged above the dielectric layer, wherein the third N+ region is located below the fourth P+ region, a first groove is formed on one side of the first N+ region, a second groove is formed between the first N+ region and the first P+ region, a third groove is formed between the first P+ region and the fourth P+ region, a fourth groove is formed between the fourth P+ region and the P-region, and a fifth groove is formed on one side of the P-region. The present invention provides a low-voltage and low-capacitance SCR structure protection device, which can obtain lower breakdown voltage, lower capacitance and higher ESD anti-interference capability through reasonable structure and process design under the condition that the chip area remains unchanged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic science and technology, and mainly relates to the field of integrated circuit electrostatic discharge (ESD) protection, and specifically relates to a low-voltage and low-capacitance SCR structure protection device and a manufacturing method thereof. Background Art

[0002] Electrostatic discharge (ESD) is an important cause of damage or even failure of precision integrated circuits. Integrated circuits are susceptible to ESD during production, manufacturing, and operation, causing damage to the product, which in turn weakens product performance and reduces reliability. Therefore, ESD protection devices with excellent performance play a more important role. The design of ESD protection devices needs to consider the following issues: first, strong ESD anti-interference ability; second, the ability to discharge amplified current; and third, low parasitic capacitance.

[0003] Devices commonly used for ESD protection include diodes, BJTs (transistors), SCRs (silicon controlled rectifiers), etc. The BJT structure obtains shallow retrace characteristics due to the introduction of injection modulation effect. The SCR structure achieves deep retrace characteristics through the positive feedback mechanism of PNPN. In terms of residual voltage parameters, the SCR structure is the lowest, followed by the BJT structure, and the diode structure is the highest. Therefore, the SCR structure is also conducive to obtaining a higher discharge current.

[0004] Figure 2 The structure of a conventional low-voltage and low-capacitance SCR protection device is shown. On an N- single crystal 101, the front side is photolithographically processed, and boron is injected and pushed forward to form a P- region 102. The front side is photolithographically processed, and phosphorus is injected and pushed forward to form N+ regions 103a and 103b. The front side is photolithographically processed, and boron is injected and pushed forward to form P+ regions 104a, 104b, and 104c. The front side is photolithographically processed, and phosphorus is injected and pushed forward to form an N+ region 105. The silicon surface dielectric layer 106 plays a role in dielectric isolation. Metal layers 107 and 108 represent the two electrode ports of the ESD protection device, namely the cathode and the anode, respectively. Its equivalent circuit is shown in FIG. Figure 3 As shown, it is equivalent to an SCR structure formed by interconnecting PNP and NPN. The emitter region, base region, and collector region of PNP are respectively composed of P+ region 104a, N- single crystal 101, P- region 102, and P+ region 104c. The emitter region, base region, and collector region of NPN are respectively composed of N+ region 103b, P- region 102, N+ region 103a, and N- single crystal 101. The breakdown voltage of SCR VBR=VBR(Z1) is determined by the breakdown voltage of Z1 diode. Z1 is composed of N+ region 105 and P+ region 104b. The impurity concentration of N+ region 105 and P+ region 104b is generally 2E19~6E19cm -3 、1E19~3E19cm-3 , the breakdown voltage formed by the two is 7~10V. In order to obtain a lower breakdown voltage, it is usually necessary to increase the impurity concentration of the N+ region 105 and the P+ region 104b. However, if the impurity concentration is too high, the leakage current will increase rapidly, and the breakdown characteristics will show soft breakdown. At the same time, due to the ultra-high impurity concentration of the N+ region 105 and the P+ region 104b, the capacitance of the SCR will also increase. In addition, since the breakdown of Z1 determined by the N+ region 105 and the P+ region 104b occurs on the surface of the device, its ESD anti-interference ability is also limited. Figure 2 The parameters of the SCR structure products shown can generally be achieved: VRWM=5V, VBR(IT=1mA)=7~10V, IR(VR=5V)≤1μA, IPP(tp=8 / 20μs)≥5A, Cj(f=1MHz, VR=0V)=1.0~1.2pF, VESD(Contact Mode)≥±15KV. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a low-voltage and low-capacitance SCR structure protection device, which can obtain lower breakdown voltage, lower capacitance and higher ESD anti-interference ability through reasonable structure and process design under the condition of unchanged chip area.

[0006] To achieve the above object, on the one hand, a low-voltage and low-capacitance SCR structure protection device of the present invention has a structure as follows: Figure 1 As shown, it includes an N-single crystal, a P-region formed on the surface of the N-single crystal, a first N+ region, a second N+ region, a third N+ region, a first P+ region, a second P+ region, a third P+ region, a fourth P+ region, a dielectric layer arranged above the N-single crystal, and a first metal layer and a second metal layer arranged above the dielectric layer, the third N+ region is located below the fourth P+ region, a first groove is formed on one side of the first N+ region, a second groove is formed between the first N+ region and the first P+ region, a third groove is formed between the first P+ region and the fourth P+ region, a fourth groove is formed between the fourth P+ region and the P- region, and a fifth groove is formed on one side of the P- region.

[0007] On the other hand, the technical solution adopted by the present invention is: a method for manufacturing a low-voltage and low-capacity SCR structure protection device, comprising the following steps:

[0008] Step 01, preparing an N- single crystal wafer 101, and growing a sacrificial oxide layer;

[0009] Step 02: front-side photolithography, boron implantation, and advancement to form a P-region;

[0010] Step 03: front-side photolithography, phosphorus implantation, and advancement to form an N+ region;

[0011] Step 04: front-side photolithography, boron implantation, and advancement to form a P+ region;

[0012] Step 05: Front photolithography and silicon etching to form a groove. Front photolithography, phosphorus implantation and driving to form an N+ region;

[0013] Step 06: Deposit polysilicon on the front side, perform photolithography on the front side, etch the polysilicon, and only keep the polysilicon for filling the groove. Perform photolithography on the front side, implant boron, and perform rapid thermal annealing to form a P+ region.

[0014] Step 07: Deposit a dielectric layer on the front side to fill the groove and form a silicon surface dielectric layer;

[0015] Step 08: Photolithography on the front side to form a contact hole area;

[0016] Step 09: sputter or evaporate metal on the front side, perform metal photolithography on the front side, and perform metal etching to form a metal area;

[0017] Step 10: Thinning the back side.

[0018] Furthermore, the crystal orientation of the N-single crystal 101 in step 01 is <100> The impurity is phosphorus, and the resistivity is 20-50Ω·cm. The thickness of the sacrificial oxide layer 112 is 500-800Å.

[0019] Furthermore, the boron implantation dose in step 02 is 1E14~5E14cm -2 The energy is 60~100KeV, the temperature condition of boron advancement is 1100~1200℃, and the time is 120~180min to form a P-region.

[0020] Furthermore, the phosphorus implantation dose in step 03 is 3E15~6E15cm -2 The energy is 30~80KeV. The temperature condition of phosphorus driving is 1000~1100℃, the time is 30~90min, and the N+ region is formed.

[0021] Furthermore, the boron implantation dose in step 04 is 2E15~5E15cm -2 , the energy is 40~100KeV, the temperature condition of boron advancement is 950~1050℃, the time is 30~90min, and a P+ region is formed.

[0022] Furthermore, the width of the groove in step 05 is 2-6 μm, and the depth is 0.5-3 μm. The phosphorus implantation dose is 3E15-6E15 cm -2 The energy is 60~120KeV. The temperature condition of phosphorus advancement is 900~1000℃, the time is 30~90min, and the N+ region is formed.

[0023] Furthermore, the polysilicon thickness in step 06 is 0.4-0.8 μm, and the boron implantation dose is 3E15-5E15 cm -2 , energy is 40~80KeV, temperature condition of rapid thermal annealing is 1000~1050℃, time is 10~30s, forming P+ region.

[0024] Furthermore, the silicon surface dielectric layer in step 07 is tetraethoxysilane TEOS, and has a thickness of 15000~20000Å.

[0025] Furthermore, after the contact holes are photoetched in step 08, a layer of TI / TIN is deposited, which can effectively reduce the failure rate of metal overheating while reducing the contact resistance.

[0026] Furthermore, the metal sputtered or evaporated on the front side in step 09 is aluminum, aluminum copper, or aluminum silicon copper, with a thickness of 2-4 μm, an alloy temperature of 360-430° C., and a time of 25-45 min.

[0027] Furthermore, the back surface in step 10 is thinned to a thickness of 150-200 μm.

[0028] The advantages of the present invention are:

[0029] 1. The present invention provides a low-voltage and low-capacitance SCR structure protection device, which can obtain lower breakdown voltage, lower capacitance and higher ESD anti-interference ability through reasonable structure and process design under the condition of unchanged chip area.

[0030] 2. The breakdown voltage VBR=VBR(Z1) of the SCR of the present invention is determined by the breakdown voltage of the Z1 diode. Z1 is composed of an N+ region 105 and a P+ region 110. The P+ region 110 is formed by boron implantation and rapid thermal annealing on the polysilicon above the N+ region 105, and a sudden PN junction formed by the P+ region 110 and the N+ region 105 is established. Rapid thermal annealing can repair the lattice defects caused by boron ion implantation, and obtain a low breakdown voltage of 3.3~7.0V and a lower leakage current. The breakdown point of this sudden PN junction occurs inside the device, and the surface breakdown of the conventional structure is transferred to the body, which can effectively improve the ESD anti-interference ability. The present invention effectively reduces the junction area of ​​the PN junction formed by the P+ region 104a, the P- region 102 and the N- single crystal 101 through grooves 109a, 109b, 109c, 109d, and 109e, thereby reducing the overall capacitance of the device. The parameters of the SCR structure product of the present invention can be achieved through the above structure and process optimization: VRWM=2.5V, VBR(IT=1mA)=3.3~7.0V, IR(VR=2.5V)≤1μA, IPP(tp=8 / 20μs)≥5A, Cj(f=1MHz, VR=0V)=0.8~1.0pF, VESD(Contact Mode)≥±20KV. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly understand the purpose and advantages of the present invention, the following will be described in detail with reference to the accompanying drawings, in which:

[0032] Figure 1 The structure diagram of a low-voltage and low-capacitance SCR structure protection device of the present invention.

[0033] Figure 2 The structural diagram of a low-voltage and low-capacitance SCR structure protection device of conventional structure.

[0034] Figure 3 The invention discloses an equivalent circuit diagram of a low-voltage and low-capacitance SCR structure protection device and a conventional low-voltage and low-capacitance SCR structure protection device.

[0035] Figure 4 The IV characteristic curve diagram of a low-voltage and low-capacitance SCR structure protection device of the present invention.

[0036] Figure 5 The first step of the process of the present invention is to prepare an N-single crystal wafer 101 and grow a sacrificial oxide layer.

[0037] Figure 6 This is the second process of the present invention, namely, front side photolithography, boron implantation, and driving-in to form the P-region 102 .

[0038] Figure 7This is the third process of the present invention, namely, front side photolithography, phosphorus implantation, and drive-in to form N+ regions 103a and 103b.

[0039] Figure 8 This is the fourth process of the present invention, namely, front side photolithography, boron implantation, and driving-in, to form P+ regions 104a, 104b, and 104c.

[0040] Fig. 9 This is the fifth process of the present invention, i.e., front side photolithography and silicon etching, to form grooves 109a, 109b, 109c, 113, 109d, and 109e.

[0041] Fig.10 This is the sixth step of the process of the present invention, namely, depositing polysilicon on the front side, photolithography on the front side, etching the polysilicon, and only retaining the polysilicon filled in the groove 113.

[0042] Fig.11 This is the seventh process step of the present invention, namely, depositing a dielectric layer on the front side to fill the grooves 109a, 109b, 109c, 109d, and 109e and form a silicon surface dielectric layer 106.

[0043] Fig.12 This is the eighth process of the present invention, i.e., forming a contact hole region by front-side photolithography.

[0044] Fig.13 This is the ninth step of the present invention, namely, front-side sputtering or evaporation of metal. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with the accompanying drawings and implementation modes. A detailed description is given by taking a 2.5V voltage level as an example.

[0046] This implementation case uses a 2.5V voltage level for detailed explanation.

[0047] Figures 5 to 13 The present invention provides a process for producing a low-voltage and low-capacity SCR structure protection device.

[0048] First, the crystal orientation of the N-single crystal 101 is <100> , the impurity is phosphorus, and the resistivity is 30~35Ω·cm. A sacrificial oxide layer 112 is grown, and the preferred thickness is 600~680 Å.

[0049] The P-region 102 is patterned by front lithography. The boron implantation dose is 1E14~3E14cm -2 , energy is 60~80KeV, temperature condition of boron advancement is 1150~1180℃, time is 150~180min, and P-region 102 is formed.

[0050] The N+ regions 103a and 103b are patterned by front lithography. The phosphorus implantation dose is 3E15~5E15cm -2 The energy is 30-60 KeV. The temperature condition of phosphorus driving is 1050-1100°C, and the time is 60-90 minutes to form N+ regions 103a and 103b.

[0051] The P+ regions 104a, 104b, and 104c are patterned by front lithography. The boron implantation dose is 2E15~4E15cm -2 The energy is 40~60KeV, the temperature condition of boron advancement is 1000~1050℃, and the time is 30~60min to form P+ regions 104a, 104b, and 104c.

[0052] Through front lithography and silicon etching, grooves 109a, 109b, 109c, 113, 109d, and 109e are formed. The width of grooves 109a, 109b, 109c, 113, 109d, and 109e is 2 to 4 μm, and the depth is 0.5 to 1.5 μm. The phosphorus implantation dose is 3E15 to 5E15 cm -2 The energy is 60-100 KeV. The temperature condition of phosphorus driving is 950-1000° C., and the time is 60-90 min to form the N+ region 105.

[0053] Polysilicon is deposited on the front side, and photolithography is performed on the front side. The polysilicon is etched, and only the polysilicon filled in the groove 113 is retained. The thickness of the polysilicon is 0.4~0.6μm.

[0054] The pattern of the groove 113 is formed by front lithography, and the boron implantation dose is 3E15~5E15cm -2 , energy is 40~60KeV, temperature condition of rapid thermal annealing is 1020~1050℃, time is 20~30s, and P+ region 110 is formed.

[0055] A dielectric layer is deposited on the front side to fill the grooves 109a, 109b, 109c, 109d, and 109e, and to form a silicon surface dielectric layer 106. The isolation dielectric layer is preferably tetraethoxysilane TEOS, with a thickness of 15000-20000Å.

[0056] The contact hole area pattern is formed by photolithography on the front side. After photolithography of the contact hole area, a layer of TI / TIN needs to be deposited. While reducing the contact resistance, it can also effectively reduce the failure rate of metal overheating.

[0057] Sputter or evaporate metal on the front side. Photolithography of metal on the front side to form a metal area. Alloy. The metal sputtered or evaporated on the front side is preferably aluminum silicon copper with a thickness of 2 to 4 μm. The temperature of the alloy is 360 to 400°C and the time is 25 to 45 minutes.

[0058] The back side was thinned to a thickness of 150±10μm.

[0059] The structure of a low-voltage and low-capacity SCR structure protection device of the present invention is as follows Figure 1 As shown, on the N- single crystal 101, the front side is photolithographically processed, boron is implanted and driven, to form the P- region 102, the front side is photolithographically processed, phosphorus is implanted and driven, to form the N+ regions 103a and 103b, the front side is photolithographically processed, boron is implanted and driven, to form the P+ regions 104a, 104b and 104c, the front side is photolithographically processed, silicon is etched, to form the grooves 109a, 109b, 109c and 113 (the description of 113 is shown in FIG. Fig. 9 ), 109d, 109e, front photolithography, phosphorus implantation, driving, forming N+ region 105, front polysilicon deposition, front photolithography, polysilicon etching, forming only in groove 113 (113 description see Fig. 9 ) is filled with polysilicon, the front side is photolithographically processed, boron is implanted, and rapid thermal annealing is performed to form a P+ region 110. A dielectric layer is deposited on the front side to fill the grooves 109a, 109b, 109c, 109d, and 109e, and a silicon surface dielectric layer 106 is formed. The metal layer 107 and the metal layer 108 represent the two electrode ports of the ESD protection device, namely the cathode and the anode, respectively.

[0060] The equivalent circuit of the present invention is as follows Figure 3 As shown, the equivalent structure is an SCR structure formed by interconnecting PNP and NPN. The emitter region, base region, and collector region of PNP are respectively composed of P+ region 104a, N- single crystal 101, P- region 102, and P+ region 104c. The emitter region, base region, and collector region of NPN are respectively composed of N+ region 103b, P- region 102, N+ region 103a, and N- single crystal 101.

[0061] The volt-ampere characteristic curve of the present invention is as follows: Figure 4As shown, when the metal layer 108 is connected to a high potential and the metal layer 107 is connected to a low potential, the current passes through the P+ region 104c, the P- region 102, the N- single crystal 101, and the N+ region 103a in sequence, showing the forward conduction characteristics of the diode. When the metal layer 107 is connected to a high potential and the metal layer 108 is connected to a low potential, the current passes through the P+ region 104a, the N- single crystal 101, the P- region 102, and the N+ region 103b in sequence, showing the deep flyback characteristics of the SCR. The breakdown voltage of the Z1 diode composed of the N+ region 105 and the P+ region 110 is much lower than the breakdown voltage of the NP junction composed of the N- single crystal 101 and the P- region 102, so the Z1 diode starts to break down first, and the current flows from the N+ region 103a, through the N- single crystal 101, the N+ region 105, the P+ region 110, the P+ region 104b, the P- region 102, and finally the P+ region 104c. When the current increases to the PN junction voltage drop between the P- region 102 and the N+ region 103b reaches the PN When the junction turn-on voltage is 0.7V, the NPN composed of the N+ region 103b, P- region 102, N+ region 103a and N- single crystal 101 as the emitter region, base region and collector region respectively, is turned on. When the current increases further, the PNP composed of the P+ region 104a, N- single crystal 101, P- region 102 and P+ region 104c as the emitter region, base region and collector region respectively is also turned on. The NPN and PNP then start the positive feedback mechanism to form the conduction of the SCR structure and obtain a deep retrace characteristic. The breakdown voltage VBR of SCR = VBR (Z1), which is determined by the breakdown voltage of the Z1 diode. Z1 is composed of N+ region 105 and P+ region 110. P+ region 110 is formed by boron implantation and rapid thermal annealing on the polysilicon above N+ region 105, and a sudden PN junction formed by P+ region 110 and N+ region 105 is established. Rapid thermal annealing can repair the lattice defects caused by boron ion implantation, and obtain a low breakdown voltage of 3.3~7.0V and a lower leakage current. The breakdown point of this sudden PN junction occurs inside the device, and the surface breakdown of the conventional structure is transferred to the body, which can effectively improve the ESD anti-interference ability. The present invention effectively reduces the junction area of ​​the PN junction formed by P+ region 104a, P- region 102 and N- single crystal 101 through grooves 109a, 109b, 109c, 109d, and 109e, thereby reducing the overall capacitance of the device. The parameters of the SCR structure product of the present invention can be achieved through the above structure and process optimization: VRWM=2.5V, VBR(IT=1mA)=3.3~7.0V, IR(VR=2.5V)≤1μA, IPP(tp=8 / 20μs)≥5A, Cj(f=1MHz, VR=0V)=0.8~1.0pF, VESD(Contact Mode)≥±20KV.

[0062] Finally, it should be noted that: technicians in this industry should understand that the present invention is not limited to the above-mentioned implementation cases. The above-mentioned embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for manufacturing a low-voltage and low-capacity SCR structure protection device, characterized in that: The following steps are involved: Step 01, preparing an N-single crystal wafer 101, and growing a sacrificial oxide layer; Step 02: front side photolithography, boron implantation and driving-in to form a P-region (102); Step 03: front side photolithography, phosphorus implantation and advancement to form N+ regions (103a) and (103b); Step 04: front side photolithography, boron implantation, and driving-in to form P+ regions (104a), (104b), and (104c); Step 05: front photolithography and silicon etching to form grooves (109a), (109b), (109c), (113), (109d), (109e), front photolithography, phosphorus implantation, and driving to form N+ region (105); Step 06, depositing polysilicon on the front side, photolithography on the front side, etching the polysilicon, leaving only the polysilicon filling the groove (113), photolithography on the front side, boron implantation, rapid thermal annealing, forming a P+ region (110); Step 07: depositing a dielectric layer on the front side to fill the grooves (109a), (109b), (109c), (109d), (109e), and forming a silicon surface dielectric layer (106); Step 08: Photolithography on the front side to form a contact hole area; Step 09: sputter or evaporate metal on the front side, perform metal photolithography on the front side, and perform metal etching to form a metal area; Step 10: thin the back side.

2. The method according to claim 1, characterized in that: The crystal orientation of the N-single crystal (101) in step 01 is <100> , the impurity is phosphorus, the resistivity is 20~50Ω·cm, and the thickness of the sacrificial oxide layer (112) is 500~800Å.

3. The method according to claim 1, characterized in that: The boron implantation dose in step 02 is 1E14~5E14cm -2 , energy is 60~100KeV, temperature condition of boron advancement is 1100~1200℃, time is 120~180min, forming P-region (102).

4. The method according to claim 1, characterized in that: The phosphorus implantation dosage in step 03 is 3E15~6E15cm -2 The energy is 30~80KeV, the temperature condition of phosphorus advancement is 1000~1100℃, and the time is 30~90min to form N+ regions (103a) and (103b).

5. The method according to claim 1, characterized in that: The boron implantation dose in step 04 is 2E15~5E15cm -2 The energy is 40~100KeV, the temperature condition of boron advancement is 950~1050℃, and the time is 30~90min to form P+ regions (104a), (104b), and (104c).

6. The method according to claim 1, characterized in that: The width of the grooves (109a), (109b), (109c), (113), (109d), and (109e) in step 05 is 2-6 μm, the depth is 0.5-3 μm, and the phosphorus implantation dose is 3E15-6E15 cm -2 The energy is 60~120KeV, the temperature condition of phosphorus advancement is 900~1000℃, and the time is 30~90min to form an N+ region (105).

7. The manufacturing method according to claim 1, characterized in that: The polysilicon thickness in step 06 is 0.4-0.8 μm, and the boron implantation dose is 3E15-5E15 cm -2 , energy is 40~80KeV, temperature condition of rapid thermal annealing is 1000~1050℃, time is 10~30s, forming P+ region (110).

8. The manufacturing method according to claim 1, characterized in that: The silicon surface dielectric layer (106) in step 07 is tetraethoxysilane TEOS, with a thickness of 15000-20000Å.

9. The manufacturing method according to claim 1, characterized in that: After the contact holes are photolithographically formed in step 08, a layer of TI / TIN is deposited.

10. The manufacturing method according to claim 1, characterized in that: The metal sputtered or evaporated on the front side in step 09 is aluminum or aluminum copper or aluminum silicon copper, with a thickness of 2-4 μm, an alloy temperature of 360-430° C., and a time of 25-45 min.

11. The manufacturing method according to claim 1, characterized in that: The back surface in step 10 is thinned to a thickness of 150-200 μm.

Citation Information

Patent Citations

  • Low-voltage ESD protection device and manufacturing method thereof

    CN111710675A

  • Low-capacitance ESD (Electro-Static Discharge) protection device and manufacturing method

    CN115831961A

  • Low-capacitance low-residual-voltage unidirectional ESD (Electro-Static Discharge) protection device and manufacturing method thereof

    CN118073351A

  • Triggered silicon controlled rectifier for RF ESD protection

    US20050173727A1

  • Vertical current controlled silicon on insulator (SOI) device such as a silicon controlled rectifier and method of forming vertical SOI current controlled devices

    US20080308837A1