A magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles and a preparation method thereof
Through the synergistic reinforcement of nanometal particles and in-situ self-generated nanoceramic particles in the magnesium-rare earth alloy matrix, the strength-ductility balance problem of traditional magnesium alloys is solved, the yield strength and plasticity are improved, and a magnesium-based composite with high mechanical properties is achieved. Material.
Patent Information
- Application Number
- CN202410979002.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Traditional magnesium alloys have difficulties in the strength-ductility balance. Ti particles form a brittle phase at the magnesium-Al alloy interface, reducing the plasticity of the magnesium alloy, and the poor interfacial bonding of the additional ceramic particles damages the plasticity of the composite material.
Nano-metal particles and in-situ self-generated nano-ceramic particles are used to synergistically strengthen the magnesium-rare earth alloy matrix. Through ultrasonic dispersion, ball milling, sintering and hot extrusion deformation processes, coherent interfaces and uniformly distributed nano-ceramic particles are formed to stimulate dynamic recrystallization and Grain refinement.
It improves the yield strength and plasticity of magnesium-based composite materials, purifies the magnesium alloy matrix, breaks the problem of poor interface bonding that damages plasticity, and realizes magnesium-based composite materials with high mechanical properties.
Smart Images

Figure CN118531278B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of magnesium-based composite materials, and in particular to a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles and a preparation method thereof. Background Art
[0002] Magnesium alloys are widely regarded as advanced structural materials with broad application prospects in rail transportation and aerospace. However, traditional magnesium alloys face the dilemma of strength-ductility balance. An effective strategy to resolve this conflict is to introduce metal reinforcement particles with excellent mechanical properties into the magnesium matrix. Metal particles usually include copper, nickel and titanium particles. However, Cu and Ni tend to form Mg2Cu and Mg2Ni with Mg, which hinders their use as effective reinforcements. Both Ti and Mg have a close-packed hexagonal crystal structure and good wettability. Although they can improve the strength of Mg alloys, Ti particles tend to form a brittle Al3Ti phase at the interface with the Mg-Al alloy, which seriously reduces the plasticity of the magnesium alloy.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The object of the present invention is to provide a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles and a preparation method thereof, so as to solve or improve the above technical problems.
[0005] The present invention can be implemented like this:
[0006] In a first aspect, the present invention provides a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles, the magnesium-based composite material comprising a magnesium-rare earth alloy matrix and a reinforcing material;
[0007] In the magnesium-rare earth alloy matrix, the content of rare earth elements is 5wt%~20wt%;
[0008] The reinforcing material comprises nano metal particles and in-situ self-generated nano ceramic particles; wherein the mass percentage of the nano metal particles in the magnesium-based composite material is 1% to 5%, and the mass percentage of the in-situ self-generated nano ceramic particles in the magnesium-based composite material is 10% to 15%.
[0009] In an optional embodiment, the metal in the nanometal particles includes at least one of Ti, Mo, Cr, V, Nb, Ta, Zr and Hf;
[0010] The in-situ self-generated nano-ceramic particles include at least one of Y2O3, Gd2O3, Nd2O3, Sm2O3, Er2O3, Ce2O3, Pr2O3, La2O3 and Ho2O3.
[0011] In an optional embodiment, the magnesium-based composite material has at least one of the following characteristics:
[0012] Feature 1: In-situ self-generated nano-ceramic particles are precipitated with nano-metal particles as heterogeneous nucleation points;
[0013] Feature 2: The in-situ self-generated nano-ceramic particles and the magnesium-rare earth alloy matrix have a coherent interface;
[0014] Feature 3: The particle size of the in-situ self-generated nano-ceramic particles does not exceed 100nm;
[0015] Feature 4: The grain size of the magnesium-based composite material does not exceed 1 μm;
[0016] Feature 5: The tensile strength of magnesium-based composite materials is not less than 370MPa;
[0017] Feature 6: The yield strength of the magnesium-based composite material is not less than 350MPa;
[0018] Feature 7: The elongation of the magnesium-based composite material is not less than 12%.
[0019] In a second aspect, the present invention provides a method for preparing a magnesium-based composite material as described in any of the aforementioned embodiments, comprising the following steps: ultrasonically dispersing and drying nano-metal powder to obtain energy-injected nano-metal powder; mixing a magnesium-rare earth alloy matrix with the energy-injected nano-metal powder, high-energy ball milling to obtain a ball mill material; and sintering and hot extrusion deforming the ball mill material.
[0020] In an optional embodiment, the mass of the nano metal powder is 1% to 5% of the total mass of the magnesium-rare earth alloy matrix and the nano metal powder;
[0021] The average particle size of nano metal powder is 50nm~80nm;
[0022] The average particle size of the magnesium-rare earth alloy matrix is 60μm~100μm.
[0023] In an optional embodiment, the frequency of ultrasonic dispersion is 30 Hz to 50 Hz, and the time of ultrasonic dispersion is 0.5 h to 2 h.
[0024] In an optional embodiment, the magnesium-rare earth alloy matrix is mixed with the energy-injected nano-metal powder at a rotation speed of 100 r / min to 200 r / min for 5 h to 8 h.
[0025] In an optional embodiment, the rotation speed of the high energy ball mill is 200 r / min to 300 r / min, the ball-to-material ratio of the high energy ball mill is 20:1 to 30:1, and the time of the high energy ball mill is 2h to 4h.
[0026] In an optional embodiment, the sintering temperature is 500° C. to 550° C., the sintering pressure is 30 MPa to 50 MPa, the sintering time is 3 min to 10 min, and air cooling is performed after sintering.
[0027] In an optional embodiment, the temperature of the hot extrusion deformation is 380° C. to 400° C., the extrusion ratio of the hot extrusion deformation is 20:1 to 25:1, and the speed of the hot extrusion deformation is 0.3 m / min to 0.5 m / min.
[0028] The beneficial effects of the present invention include:
[0029] The magnesium-based composite material proposed by the present invention is a magnesium-rare earth alloy matrix with a specific rare earth content reinforced by nano-metal particles and in-situ self-generated nano-ceramic particles, so that the composite material has high yield strength and plasticity at the same time. Among them, the in-situ self-generated nano-ceramic particles and the magnesium alloy matrix are coherent interfaces with good interface bonding, and the in-situ self-generated nano-ceramic particles are evenly distributed on the interface of the magnesium-rare earth alloy matrix, which helps the continuous transfer of loads on the interface and improves the mechanical properties of the composite material. It can also purify the magnesium alloy matrix, breaking the problem that the added ceramic particles damage the plasticity of the composite material due to poor interface bonding. At the same time, the added nano-metal particles and the in-situ endogenous ceramic particles stimulate the occurrence of dynamic recrystallization, which triggers grain refinement. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 This is a longitudinal cross-sectional morphology of the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles prepared in Example 1;
[0032] Figure 2 This is a longitudinal cross-sectional morphology of the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles prepared in Comparative Example 1;
[0033] Figure 3 This is a longitudinal cross-sectional morphology of the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles prepared in Comparative Example 6;
[0034] Figure 4 This is a coherent distribution interface diagram between the in-situ self-generated nano-ceramic particles and the matrix in the magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles prepared in Example 1. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0036] The magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles provided by the present invention and the preparation method thereof are described in detail below.
[0037] The invention provides a magnesium-based composite material synergistically reinforced by nano metal particles and ceramic particles. The magnesium-based composite material comprises a magnesium-rare earth alloy matrix and a reinforcing material.
[0038] In the magnesium-rare earth alloy matrix, the content of rare earth elements is 5wt%~20wt%, such as 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%, etc., and can also be other values within the range of 5wt%~20wt%. In some preferred embodiments, the content of rare earth elements in the magnesium-rare earth alloy matrix is 8wt%~12wt%; in some more preferred embodiments, the content of rare earth elements in the magnesium-rare earth alloy matrix is 10wt%.
[0039] By limiting the content of rare earth elements to the above range, it is possible to effectively refine the grains while reducing costs. In addition, taking the nano-metal particles as nano-Ti particles and the rare earth as Y as an example, if the content of the rare earth element is too little, not only is the generated Y2O3 content low, but also the impurity precipitation phases such as MgO and TiO2 are easily generated, and the composition is not easy to control.
[0040] The reinforcing materials include nano-metal particles and in-situ self-generated nano-ceramic particles.
[0041] It should be noted that commonly used ceramic particles include carbides (such as SiC, TiC and B4C), nitrides (such as Si3N4, AlN and TiN) and oxide particles (such as MgO, Al2O3 and Y2O3). However, the wettability and interfacial bonding between the added SiC ceramic particles and the Mg matrix are low, resulting in low elongation of the corresponding material. The added AlN ceramic particles can easily form clusters at the interface, and a complex process is required to obtain a clean interface. For oxide ceramic particles, excessive addition of oxide ceramic particles at the grain boundary will also lead to deterioration of the interface combination.
[0042] The nano ceramic particles in the present invention are in-situ self-generated nano ceramic particles, which can maintain a good interface combination with the matrix and improve the mechanical properties of the material.
[0043] In the present invention, the mass percentage of the nano metal particles in the magnesium-based composite material can be 1% to 5%, such as 1%, 2%, 3%, 4% or 5%, etc., or any other value within the range of 1% to 5%. The mass percentage of the in-situ self-generated nano ceramic particles in the magnesium-based composite material can be 10% to 15%, such as 10%, 11%, 12%, 13%, 14% or 15%, etc., or any other value within the range of 10% to 15%.
[0044] The metal in the nano-metal particles may illustratively but not limitatively include at least one of Ti, Mo, Cr, V, Nb, Ta, Zr and Hf.
[0045] The in-situ self-generated nano-ceramic particles may illustratively but not limitatively include at least one of Y2O3, Gd2O3, Nd2O3, Sm2O3, Er2O3, Ce2O3, Pr2O3, La2O3 and Ho2O3.
[0046] The particle size of the in-situ self-generated nano-ceramic particles does not exceed 100nm.
[0047] In the magnesium-based composite material proposed by the present invention, the in-situ self-generated nano-ceramic particles use nano-metal particles as heterogeneous nucleation points and use rare earth elements in the matrix and oxygen elements introduced on the surface of the nano-metal particles as raw materials to precipitate nano-ceramic oxides. Among them, the oxygen element is oxygen adsorbed on the surface of the nano-metal particles, which can be introduced by exposing the nano-metal particles to the air after ultrasound. The in-situ self-generated nano-ceramic particles and the magnesium alloy matrix are coherent interfaces with good interface bonding, and the in-situ self-generated nano-ceramic particles are evenly distributed on the interface of the magnesium-rare earth alloy matrix, which helps the continuous transfer of loads on the interface and improves the mechanical properties of the composite material. It can also purify the magnesium alloy matrix, breaking the problem that the added ceramic particles damage the plasticity of the composite material due to poor interface bonding. At the same time, the added nano-metal particles and the in-situ endogenous ceramic particles stimulate the occurrence of dynamic recrystallization and induce grain refinement.
[0048] The improvement of strength of the magnesium-based composite material proposed in the present invention is mainly attributed to the grain refinement strengthening and dispersion strengthening mechanism, and the improvement of ductility is mainly due to the increase of dislocation storage capacity in the ultrafine grain structure, the formation of a coherent interface between the endogenous reinforcement particles and the magnesium matrix, and the conical surface. and<a+c> Activation of the slip system: The pinning of grain boundaries and dislocations by endogenous and external reinforcement particles during deformation can significantly refine the grains.
[0049] In some embodiments, the grain size of the magnesium-based composite material provided by the present invention does not exceed 1 μm, such as 0.76 μm to 0.98 μm.
[0050] The magnesium-based composite material within this range has fine grains, a large number of grain boundaries, and greater resistance to dislocation movement, which is conducive to enhancing the plastic deformation resistance of the magnesium alloy. In addition, the more grains there are, the more metal plastic deformation can be dispersed inside the grains, and the grain boundaries hinder the expansion of cracks, thereby improving the storage energy of the composite material.
[0051] In some embodiments, the tensile strength of the magnesium-based composite material provided by the present invention is not less than 370 MPa, such as 370 MPa to 391 MPa.
[0052] In some embodiments, the yield strength of the magnesium-based composite material provided by the present invention is not less than 350 MPa, such as 351 MPa to 366 MPa.
[0053] In some embodiments, the elongation of the magnesium-based composite material provided by the present invention is not less than 12%, such as 12% to 15%.
[0054] As mentioned above, the magnesium-based composite material provided by the present invention has higher yield strength and plasticity.
[0055] Correspondingly, the present invention also provides a method for preparing the above-mentioned magnesium-based composite material, comprising the following steps: ultrasonically dispersing nano-metal powder and drying it to obtain energy-injected nano-metal powder; mixing a magnesium-rare earth alloy matrix with the energy-injected nano-metal powder, high-energy ball milling, to obtain a ball mill material; and sintering and hot extrusion deforming the ball mill material.
[0056] In some embodiments, the average particle size of the nano metal powder can be 50nm~80nm, such as 50nm, 55nm, 60nm, 65nm, 70nm, 75nm or 80nm, etc., or other values within the range of 50nm~80nm. In some preferred embodiments, the average particle size of the nano metal powder is 55nm~65nm. In some more preferred embodiments, the average particle size of the nano metal powder is 60nm.
[0057] The finer the nano metal powder is, the larger the specific surface area is, the more active atoms there are on the surface, and the easier it is for surface diffusion to be performed. The nano metal powder with an average particle size of 50nm to 80nm adopted in the present invention is highly active, is evenly distributed on the substrate surface, and promotes the formation of ceramic particles at the phase boundary. If the average particle size of the nano metal powder exceeds 80nm, the activity will decrease, and the gaps between particles are large, which is unfavorable for the formation of dense composite materials.
[0058] In some embodiments, the frequency of ultrasonic dispersion can be 30 Hz to 50 Hz, such as 30 Hz, 35 Hz, 40 Hz, 45 Hz or 50 Hz, or any other value within the range of 30 Hz to 50 Hz. The time of ultrasonic dispersion can be 0.5 h to 2 h, such as 0.5 h, 1 h, 1.5 h or 2 h, or any other value within the range of 0.5 h to 2 h.
[0059] By ultrasonically dispersing and drying the nano metal powder before mixing it with the magnesium-rare earth alloy matrix, energy can be injected into the nano metal powder to activate the nano metal powder.
[0060] In some embodiments, the average particle size of the magnesium-rare earth alloy matrix can be 60 μm to 100 μm, such as 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm, etc., or other values within the range of 60 μm to 100 μm. In some preferred embodiments, the average particle size of the magnesium-rare earth alloy matrix can be 75 μm to 85 μm. In some more preferred embodiments, the average particle size of the magnesium-rare earth alloy matrix is 80 μm.
[0061] If the average particle size of the magnesium alloy matrix is less than 60 μm, the magnesium alloy powder has high activity. The material is not only easily oxidized during the preparation process, but also poses a safety risk, which is not conducive to industrial production.
[0062] In some embodiments, the mass of the nano metal powder can be 1% to 5% of the total mass of the magnesium-rare earth alloy matrix and the nano metal powder, such as 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., or other values within the range of 1% to 5%.
[0063] If the mass percentage of nano-metal powder is higher than 5%, it is not conducive to the uniform distribution of nano-metal powder, and the excess nano-metal powder is easy to agglomerate at the phase boundary, which is not conducive to enhancing the strong interface bonding between the particles and the matrix, and the material plasticity is poor.
[0064] In some embodiments, the magnesium-rare earth alloy matrix is mixed with the energy-injected nano-metal powder at a rotation speed of 100 r / min~200 r / min (such as 100 r / min, 150 r / min or 200 r / min, etc.) for 5h~8h (such as 5h, 6h, 7h or 8h, etc.).
[0065] In some embodiments, the rotation speed of the high energy ball mill can be 200r / min~300r / min, such as 200r / min, 250r / min or 300r / min, or other values within the range of 200r / min~300r / min. The ball-to-material ratio of the high energy ball mill can be 20:1 to 30:1, such as 20:1, 25:1 or 30:1, or other values within the range of 20:1 to 30:1. The time of high energy ball milling can be 2h~4h, such as 2h, 2.5h, 3h, 3.5h or 4h, or other values within the range of 2h~4h.
[0066] Through high-energy ball milling, energy can be further injected into the ball-milled material to activate the magnesium matrix.
[0067] In some embodiments, the sintering temperature may be 500°C to 550°C, such as 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, or other values within the range of 500°C to 550°C. The sintering pressure may be 30MPa to 50MPa, such as 30MPa, 35MPa, 40MPa, 45MPa or 50MPa, or other values within the range of 30MPa to 50MPa. The sintering time may be 3min to 10min, such as 3min, 5min or 10min, or other values within the range of 3min to 10min. After sintering, air cooling is performed.
[0068] The above sintering can be carried out by spark plasma sintering. When spark plasma sintering powder is used, many holes or defects will exist in the sintered blank at a sintering temperature below 500°C, and there will be almost no cracks or defects above 500°C, which will help the effective bonding process between the powders. However, the thermal inertia during the spark plasma sintering heating process will cause the actual temperature to exceed the set temperature, and the actual temperature will exceed 550°C or the solidus temperature, so that the powder is partially melted into a semi-solid state.
[0069] During the sintering process, rare earth oxides such as Gd2O3, Y2O3 and Ce2O3 are formed at the interface of Mg-RE powder and accumulate at the bonding interface between metal powders. As the sintering time increases, the thickness of the bonding interface increases, the interface bonding weakens, and at the same time, more solute RE atoms are consumed, resulting in a decrease in the solid solution strengthening effect of the α-Mg matrix. Therefore, the sintering time should not be too long. In addition, if the sintering time is too long, the grain growth is more, which is not conducive to fine grain strengthening.
[0070] In some embodiments, the temperature of the hot extrusion deformation is 380°C to 400°C (such as 380°C, 385°C, 390°C, 395°C or 400°C, etc.), the extrusion ratio of the hot extrusion deformation is 20:1 to 25:1 (such as 20:1, 21:1, 22:1, 23:1, 24:1 or 25:1, etc.), and the speed of the hot extrusion deformation is 0.3m / min to 0.5m / min (such as 0.3m / min, 0.35m / min, 0.4m / min, 0.45m / min or 0.5m / min, etc.).
[0071] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0072] Example 1
[0073] This embodiment provides a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles, and the preparation method thereof includes:
[0074] S1: Ultrasonic dispersion of nano-Ti powder with an average particle size of 60 nm is performed at a frequency of 30 Hz for 1 hour. The nano-Ti powder after ultrasonic dispersion is dried to obtain energy-infused and uniformly dispersed nano-Ti powder.
[0075] S2: The energy-injected and uniformly dispersed nano-Ti powder and a magnesium-rare earth alloy matrix (Mg-10Y powder containing 10 wt% Y) with an average particle size of 80 μm were mixed in a double cone mixer at a mass ratio of 2:98 at a speed of 150 r / min for 6 hours to obtain a mixed powder.
[0076] S3: The powder is subjected to high-energy ball milling to obtain a ball mill material, wherein the ball-to-material ratio is 20:1, the rotation speed is 200 r / min, and the time is 2 h.
[0077] S4: the ball abrasive is subjected to spark plasma sintering treatment, and after sintering, the temperature is cooled to room temperature by air to obtain a sintered part, wherein the sintering temperature is 500° C., the time is 5 min, and the pressure is 40 MPa.
[0078] S5: After the sintered part and the extrusion die are kept at 400° C. for 30 minutes, hot extrusion is performed at an extrusion ratio of 25:1 and an extrusion speed of 0.5 m / min to finally obtain a magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles.
[0079] The magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles prepared in this embodiment includes a magnesium-rare earth alloy matrix and a reinforcing material, wherein the reinforcing material includes nano-Ti particles and in-situ self-generated nano-Y2O3 particles; wherein the mass percentage of the nano-Ti particles in the magnesium-based composite material is 2%, and the mass percentage of the in-situ self-generated nano-Y2O3 particles in the magnesium-based composite material is 10%.
[0080] Example 2
[0081] The difference between this embodiment and embodiment 1 is that the magnesium-rare earth alloy matrix is Mg-10Gd alloy powder containing 10 wt % of Gd.
[0082] Example 3
[0083] The difference between this embodiment and embodiment 1 is that the nano-metal reinforcement particles are nano-metal Mo particles.
[0084] Example 4
[0085] The difference between this embodiment and embodiment 1 is that the frequency of ultrasonic dispersion is 50 Hz and the time is 1 hour. The nano-Ti obtains relatively more injected energy.
[0086] Example 5
[0087] This embodiment provides a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles, and the preparation method thereof includes:
[0088] S1: Ultrasonic dispersion of nano Nb powder with an average particle size of 50 nm is performed at a frequency of 40 Hz for 2 hours. The nano Nb powder after ultrasonic dispersion is dried to obtain energy-infused and uniformly dispersed nano Nb powder.
[0089] S2: The energy-injected and uniformly dispersed nano Nb powder was mixed with a magnesium-rare earth alloy matrix (Mg-5Sm powder containing 5 wt% Sm) having an average particle size of 60 μm in a double cone mixer at a mass ratio of 1:99 at a speed of 100 r / min for 8 h to obtain a mixed powder.
[0090] S3: The powder is subjected to high-energy ball milling to obtain a ball mill material, wherein the ball-to-material ratio is 25:1, the rotation speed is 250 r / min, and the time is 4 hours.
[0091] S4: the ball abrasive is subjected to spark plasma sintering treatment, and after sintering, the temperature is cooled to room temperature by air to obtain a sintered part, wherein the sintering temperature is 520° C., the time is 5 min, and the pressure is 30 MPa.
[0092] S5: After the sintered part and the extrusion die are kept at 380° C. for 30 minutes, hot extrusion is performed at an extrusion ratio of 20:1 and an extrusion speed of 0.3 m / min to finally obtain a magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles.
[0093] Example 6
[0094] This embodiment provides a magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles, and the preparation method thereof includes:
[0095] S1: Ultrasonic dispersion of nano-Cr powder with an average particle size of 80 nm is performed at a frequency of 50 Hz for 0.5 h. The nano-Cr powder after ultrasonic dispersion is dried to obtain energy-infused and uniformly dispersed nano-Cr powder.
[0096] S2: The energy-injected and uniformly dispersed nano-Cr powder and a magnesium-rare earth alloy matrix (Mg-10Ce powder containing 20 wt% Ce) with an average particle size of 100 μm were mixed in a double cone mixer at a mass ratio of 5:95 for 5 hours at a speed of 200 r / min to obtain a mixed powder.
[0097] S3: The powder is subjected to high-energy ball milling to obtain a ball mill material, wherein the ball-to-material ratio is 30:1, the rotation speed is 300 r / min, and the time is 2 h.
[0098] S4: the ball abrasive is subjected to spark plasma sintering treatment, and after sintering, the temperature is cooled to room temperature by air to obtain a sintered part, wherein the sintering temperature is 550° C., the time is 5 min, and the pressure is 50 MPa.
[0099] S5: After the sintered part and the extrusion die are kept at 400° C. for 30 minutes, hot extrusion is performed at an extrusion ratio of 25:1 and an extrusion speed of 0.4 m / min to finally obtain a magnesium-based composite material synergistically reinforced with nano-metal particles and ceramic particles.
[0100] Comparative Example 1
[0101] The difference between this comparative example and Example 1 is that no nano-Ti particles are added, and pure Mg10Y alloy is used.
[0102] Comparative Example 2
[0103] The difference between this comparative example and Example 1 is that the content of rare earth elements in the magnesium-rare earth alloy matrix is 2wt%.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 1 is that the nano metal particles are Cu.
[0106] Comparative Example 4
[0107] The difference between this comparative example and Example 1 is that the reinforcement particles are Ti with an average particle size of 30 μm.
[0108] Comparative Example 5
[0109] The difference between this comparative example and Example 1 is that the average particle size of the magnesium-rare earth alloy matrix is 180 μm.
[0110] Comparative Example 6
[0111] The difference between this comparative example and Example 1 is that the mass of the nano metal powder is 15% of the total mass of the magnesium-rare earth alloy matrix and the nano metal powder.
[0112] Comparative Example 7
[0113] The difference between this comparative example and Example 1 is that the nano-Ti powder in S1 is not injected with energy and is directly mixed with the magnesium-rare earth alloy matrix without ultrasonic treatment.
[0114] Comparative Example 8
[0115] The difference between this comparative example and Example 1 is that the ultrasonic frequency is 100 Hz.
[0116] Comparative Example 9
[0117] The difference between this comparative example and Example 1 is that the sintering time is 20 minutes.
[0118] Comparative Example 10
[0119] The difference between this comparative example and Example 1 is that the extrusion ratio of hot extrusion is 2:1.
[0120] Test example
[0121] ①, the morphology of the magnesium-based composite materials obtained in Example 1, Comparative Example 1 and Comparative Example 6 was tested, the transmission structure of the ceramic Y2O3 in situ precipitated in the examples was characterized, and the grain size of the magnesium-based composite materials obtained in Examples 1 to 6 and Comparative Examples 1 to 10 was tested by electron backscattering, and the obtained grain morphology was statistically analyzed. The results are shown in Figures 1 to 4 And as shown in Table 1.
[0122] Depend on Figures 1 to 3It can be seen that in the 2.0wt% Ti / Mg10Y composite material in Example 1, the precipitated phase is nano-sized and dispersed and evenly distributed; nano-Ti and in-situ precipitated nano-Y2O3 ceramic particles are distributed in the extruded zone area, and rectangular Mg2Y phases are distributed between the extruded zones. In Comparative Example 1, no Y2O3 ceramic precipitated phase was found, and the existing Mg2Y phase was irregular in size and relatively coarse, and its distribution was extremely uneven, which seriously affected the final mechanical properties of the composite material. In Comparative Example 6, the mass fraction of nano-Ti particles is as high as 15wt%. Nano-particles with a high volume fraction are easily agglomerated when added to the magnesium alloy matrix, resulting in a coarse Mg2Y precipitated phase. This phase is a brittle phase, and cracks are easily initiated and extended again, resulting in a decrease in the final mechanical properties.
[0123] Depend on Figure 4 It can be seen that the Y2O3 ceramic particles formed in situ in the 2.0wt% Ti / Mg10Y composite material of Example 1 are only about 30nm in size, showing a regular square morphology, and the orientation of each edge is coherent with the magnesium matrix, showing good interface bonding, which is conducive to the transfer of load on the interface and effectively avoids cracking caused by stress concentration.
[0124] Depend on Figure 1 , Figure 3 As can be seen from Table 1, the grain size of the magnesium-based composite material prepared by the method provided in the embodiment of the present application is basically at the nanometer level, and it contains a large number of grain boundaries, which can effectively hinder the expansion of cracks, greatly improve the storage energy of the material, and have significant effects of fine grain strengthening and precipitation strengthening, resulting in that the strength and plasticity of the composite material can be improved at the same time.
[0125] ②. The magnesium-based composite materials obtained in Examples 1 to 6 and Comparative Examples 1 to 10 were subjected to mechanical property tests, and the results are shown in Table 1.
[0126] Among them, the yield strength, tensile strength and room temperature elongation are tested in accordance with "GB / T 228.1-2021".
[0127] Table 1 Grain size and mechanical properties test results
[0128]
[0129] It can be seen from Table 1 that the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles provided by the present invention can have both high yield strength and plasticity.
[0130] In summary, the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles provided by the present invention has fine grains, high yield strength, tensile strength and elongation. The preparation method of the magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles is simple to operate, low in cost, and can be industrialized.
[0131] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A magnesium-based composite material synergistically reinforced by nano-metal particles and ceramic particles, characterized in that: The magnesium-based composite material comprises a magnesium-rare earth alloy matrix and a reinforcing material; The content of rare earth elements in the magnesium-rare earth alloy matrix is 5wt%~20wt%; The reinforcing material comprises nano-metal particles and in-situ self-generated nano-ceramic particles; wherein the mass percentage of the nano-metal particles in the magnesium-based composite material is 1% to 5%, and the mass percentage of the in-situ self-generated nano-ceramic particles in the magnesium-based composite material is 10% to 15%; The metal in the nano-metal particles includes at least one of Ti, Mo, Cr, V, Nb, Ta, Zr and Hf; The in-situ self-generated nano-ceramic particles include at least one of Y2O3, Gd2O3, Nd2O3, Sm2O3, Er2O3, Ce2O3, Pr2O3, La2O3 and Ho2O3.
2. The magnesium-based composite material according to claim 1, characterized in that: The magnesium-based composite material has at least one of the following characteristics: Feature 1: The in-situ self-generated nano-ceramic particles are precipitated with the nano-metal particles as heterogeneous nucleation points; Feature 2: The in-situ self-generated nano-ceramic particles and the magnesium-rare earth alloy matrix have a coherent interface; Feature 3: The particle size of the in-situ self-generated nano-ceramic particles does not exceed 100 nm; Feature 4: The grain size of the magnesium-based composite material does not exceed 1 μm; Feature 5: The tensile strength of the magnesium-based composite material is not less than 370 MPa; Feature 6: The yield strength of the magnesium-based composite material is not less than 350 MPa; Feature 7: The elongation of the magnesium-based composite material is not less than 12%.
3. A method for preparing a magnesium-based composite material as claimed in claim 1 or 2, characterized in that: The following steps are involved: Ultrasonic dispersion and drying of nano-metal powders are performed to obtain energy-injected nano-metal powders; a magnesium-rare earth alloy matrix is mixed with the energy-injected nano-metal powders, and high-energy ball milling is performed to obtain ball mill material; the ball mill material is sintered and hot extruded; The frequency of ultrasonic dispersion is 30 Hz to 50 Hz, the sintering time is 3 min to 10 min, and the extrusion ratio of hot extrusion deformation is 20:1 to 25:
1.
4. The preparation method according to claim 3, characterized in that: The mass of the nano metal powder is 1% to 5% of the total mass of the magnesium-rare earth alloy matrix and the nano metal powder; The average particle size of the nano metal powder is 50nm~80nm; The average particle size of the magnesium-rare earth alloy matrix is 60 μm to 100 μm.
5. The preparation method according to claim 3, characterized in that: The ultrasonic dispersion time is 0.5h~2h.
6. The preparation method according to claim 3, characterized in that: The magnesium-rare earth alloy matrix and the energy-injected nano-metal powder are mixed at a rotation speed of 100 r / min to 200 r / min for 5 h to 8 h.
7. The preparation method according to claim 3, characterized in that: The rotation speed of the high energy ball mill is 200r / min~300r / min, the ball-to-material ratio of the high energy ball mill is 20:1 to 30:1, and the time of the high energy ball mill is 2h~4h.
8. The preparation method according to claim 3, characterized in that: The sintering temperature is 500°C~550°C, the sintering pressure is 30MPa~50MPa, and air cooling is performed after sintering.
9. The preparation method according to claim 3, characterized in that: The temperature of hot extrusion deformation is 380℃~400℃, and the speed of hot extrusion deformation is 0.3m / min~0.5m / min.