Environmentally friendly mineral-based gelling agent and preparation method thereof
By using fly ash, coal gangue, slag, modified basalt fibers and modified calcite in mineral-based gelling agents, and using calcium carbide slag, nanomagnesium oxide and NaOH as excitants, mineral-based gels are solved The problem of insufficient mechanical properties of the coagulant significantly improves its compressive strength and compactness.
Patent Information
- Application Number
- CN202410672132.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-28
AI Technical Summary
The mechanical properties of existing mineral-based gelling agents are poor and cannot meet market demand.
Using fly ash, coal gangue, slag, KH792 modified basalt fibers and YDH-171 modified calcium zeolite and other components, combined with calcium carbide slag, nanomagnesium oxide and NaOH as alkaline exciters, environmentally friendly type is prepared by stirring and mixing. Mineral-based gelling agent to improve its density and mechanical properties.
The mechanical properties and compactness of the gelling agent are significantly improved, and the compressive strength of the 7d can reach up to 6.25MPa, meeting the market's demand for the performance of mineral-based gelling agents.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of mineral-based gelling agents, and more specifically, relates to an environmentally friendly mineral-based gelling agent and a preparation method thereof. Background Art
[0002] After the use of minerals, a large amount of solid waste such as slag, fly ash, carbide slag, etc. will be generated. The long-term accumulation of these solid wastes not only occupies a large amount of land resources but also pollutes the surrounding environment. Geopolymer cementitious materials are a new type of green cementitious materials mainly based on industrial solid waste as precursors, prepared by the hydration mechanism based on the alkali excitation effect under the action of alkali activators at room temperature or slightly high temperature. The hydration mechanism of geopolymer is mainly completed by four stages: dissolution and reconstruction, dispersion and migration, concentration and polymerization, and hydration and hardening. This inorganic material is an aluminum-oxygen-silicon three-dimensional network silicate polymer composed of [AlO4] and [SiO4] tetrahedrons with ionic bonds and covalent bonds as the main connectors and van der Waals bonds as complementary connections.
[0003] CN117865532A discloses a method for preparing a freeze-thaw resistant volcanic ash-based polymer activated by composite waste alkali. The geopolymer is a freeze-thaw resistant volcanic ash and blast furnace slag-based geopolymer activated by a triple composite alkali activator of carbide slag, mirabilite and sodium silicate, and has the characteristics of high compressive strength and good freeze-thaw cycle durability. The invention uses an environmentally friendly material preparation method to give full play to the utilization value of solid waste, which can reduce the production cost of the geopolymer. The matrix density of the geopolymer is increased by using carbide slag, mirabilite and sodium silicate as a composite alkali activator, thereby improving the freeze-thaw durability. The triple composite waste alkali system has good alkali activation performance, which can accelerate the geopolymerization process to obtain a dense gel matrix. The geopolymer is used as a substitute for ordinary Portland cement, which can increase the life of buildings in cold environments and has good application prospects.
[0004] CN117964261A discloses a geopolymer made from fly ash bottom slag from garbage incineration and a system process method, including geopolymer made from fly ash bottom slag from garbage incineration, wherein the geopolymer made from fly ash bottom slag from garbage incineration is composed of the following raw materials: 20-60% fly ash bottom slag, 60-20% fly ash; 17% mineral powder; 3% gypsum; 0.8% sodium hydroxide; 2% water glass; 0.3%-0.5% water-binder ratio. The present invention relates to the technical field of hazardous solid waste management. The present invention adopts the cleaning, purification and refining technology of fly ash bottom slag. Based on the calculation of 800 tons / day of garbage incineration: 800*25%=200 tons / day of bottom slag, 800*4%=32 tons / day of fly ash, three slag pools are designed. The 1# slag pool and the 2# slag pool are operated alternately, and the mixed water produced by cleaning enters the 3# pool and then enters the low-temperature evaporation separator to separate water and chlorine. The purified water is circulated to the bottom slag by a pump and continued to be provided for bottom slag cleaning. The separated finished chlorine is made into disinfectants and other products, reducing the intermittent production process of lime water immersion.
[0005] CN117964288A discloses a geopolymer regeneration fireproof mortar reinforced with waste glass powder and a preparation method thereof. The regeneration fireproof mortar concrete comprises the following raw material components: 480-500 parts of cementitious material, 840-1080 parts of recycled fine aggregate, 310-340 parts of alkali activator, 120-360 parts of waste glass powder and 50 parts of water. The preparation method is as follows: the recycled fine aggregate is mixed and stirred with the cementitious material to obtain a dry mixture; the waste glass powder is stirred and pre-treated with the alkali activator to obtain an alkali-activated mixed solution; the alkali-activated mixed solution is added to the dry mixture and stirred to obtain a mortar slurry; the mortar slurry is poured in a mold, and the mortar slurry is compacted and vibrated in layers during the pouring process, and the mold is wrapped after the surface solidifies, and the geopolymer regeneration fireproof mortar is obtained by curing. The present invention completely uses recycled aggregates, and on this basis partially replaces the recycled fine aggregate with waste glass powder, thereby alleviating the problem of resource scarcity caused by excessive exploitation of natural sand. The synergistic reaction of waste glass powder and geopolymer and its filling effect can effectively alleviate the problem of poor performance of recycled mortar and improve the working performance and fire resistance of geopolymer recycled mortar.
[0006] From the above content, it can be seen that the comprehensive performance of mineral-based gelling agents can be improved by recycling mineral waste and adding modifying components or alkali activators. However, the mechanical properties of mineral-based gelling agents are poor and can no longer meet market demand. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide an environmentally friendly mineral-based gelling agent and a preparation method. In parts by weight, the present invention comprises the following components: 20 to 30 parts of fly ash; 15 to 25 parts of coal gangue; 25 to 35 parts of slag; 4 to 8 parts of basalt fiber modified by KH792; 3 to 7 parts of calcium zeolite modified by YDH-171; 5 to 9 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.2 to 0.4: 0.1 to 0.3: 1: 0.4 to 0.6. The present invention can improve the compactness of the gel material and the mechanical properties of the mineral-based gelling agent by adding modified materials and using alkaline activators of specific composition.
[0008] The purpose of the present invention is to provide an environmentally friendly mineral-based gelling agent.
[0009] Another object of the present invention is to provide a method for preparing an environmentally friendly mineral-based gelling agent.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] An environmentally friendly mineral-based gelling agent, comprising the following components by weight:
[0012] 20-30 parts of fly ash;
[0013] 15-25 parts of coal gangue;
[0014] 25-35 parts of slag;
[0015] 4-8 parts of KH792 modified basalt fiber;
[0016] 3-7 parts of YDH-171 modified calcium zeolite;
[0017] 5-9 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.2-0.4: 0.1-0.3: 1: 0.4-0.6.
[0018] Preferably, the particle size of the fly ash is 100-300 μm; the particle size of the fly ash is 50-150 μm.
[0019] Preferably, the particle size of the slag is 150-250 μm; the length of the basalt fiber is 1-5 mm, and the aspect ratio is 100-500:1; and the particle size of the calcium zeolite is 100-300 nm.
[0020] Preferably, the preparation method of the KH792-modified basalt fiber comprises: adding basalt fiber and KH792 to ethanol, heating to 60-80° C. for reaction for 1-3 hours, filtering, washing, and vacuum drying at 80° C. to constant weight to obtain KH792-modified basalt fiber.
[0021] Preferably, the mass ratio of the basalt fiber to KH792 is 10:1-3.
[0022] Preferably, the preparation method of YDH-171 modified calcium zeolite includes: heat treating the calcium zeolite, cooling to room temperature, then ultrasonically dispersing the heat-treated calcium zeolite and YDH-171 in ethanol, heating to 70-90°C for reaction for 1-3h, cooling to room temperature, filtering, washing, and vacuum drying at 80°C to constant weight to obtain YDH-171 modified calcium zeolite.
[0023] Preferably, the mass ratio of the heat-treated calcium zeolite to YDH-171 is 5:1-2.
[0024] Preferably, the heat treatment is performed at 120-140° C. for 3-5 hours.
[0025] Based on the above-mentioned method for preparing an environmentally friendly mineral-based gelling agent, the preparation method comprises the following steps:
[0026] Put fly ash, coal gangue, slag, KH792 modified basalt fiber and YDH-171 modified calcium zeolite into a mixer and stir and mix them, then add alkaline activator, continue stirring for a certain time, and obtain an environmentally friendly mineral-based gelling agent.
[0027] Preferably, the stirring speed is 150-250 r / min, and the stirring is 20-40 min; the continuous stirring time is 10-20 min.
[0028] The present invention has the following beneficial effects:
[0029] The present invention can improve the dispersibility of KH792 modified basalt fiber in the gelling agent and improve the mechanical properties of the gelling agent. By adding modified zeolite, the internal pore structure of the material can be refined, the density of the material can be improved, and the mechanical properties of the gelling agent can be improved. By selecting a specific specific composition, the density of the gel material can be improved and the mechanical properties of the mineral-based gelling agent can be improved. DETAILED DESCRIPTION
[0030] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0031] Main chemical components of fly ash / (wt%)
[0032] CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> MgO <![CDATA[Fe2O3]]> <![CDATA[SO3]]> Loss on ignition 5.8 49.8 24.1 1.4 0.75 2.2 2.7
[0033] Main chemical components of slag / (wt%)
[0034] CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> MgO <![CDATA[Fe2O3]]> <![CDATA[SO3]]> Loss on ignition 38.2 33.2 14.24 9.32 0.69 2.6 0.5
[0035] Chemical composition of carbide slag / (wt%)
[0036] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO <![CDATA[SO3]]> other 3.6 1.78 91.3 1.73 1.59
[0037] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0038] Example 1
[0039] An environmentally friendly mineral-based gelling agent, comprising the following components by weight:
[0040] 25 parts of fly ash; the particle size of the fly ash is 200 μm;
[0041] 20 parts of coal gangue; the particle size of the fly ash is 100 μm;
[0042] 30 parts of slag; the particle size of the slag is 200 μm;
[0043] 6 parts of KH792 modified basalt fiber; the basalt fiber has a length of 3 mm and an aspect ratio of 300:1;
[0044] 5 parts of YDH-171 modified calcium zeolite; the particle size of the calcium zeolite is 200 nm;
[0045] 7 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.3:0.2:1:0.5;
[0046] The preparation method of the KH792-modified basalt fiber comprises: adding 10 g of basalt fiber and 2 g of KH792 to 150 mL of ethanol, heating to 70° C. for reaction for 2 h, filtering, washing, and vacuum drying at 80° C. to constant weight to obtain the KH792-modified basalt fiber.
[0047] The preparation method of YDH-171 modified calcium zeolite comprises: heat treating 100g calcium zeolite at 13°C for 4h, cooling to room temperature, and then ultrasonically dispersing 50g heat-treated calcium zeolite and 15g YDH-171 in ethanol, heating to 80°C for reaction for 2h, cooling to room temperature, filtering, washing, and vacuum drying at 80°C to constant weight to obtain YDH-171 modified calcium zeolite. A preparation method of an environmentally friendly mineral-based gelling agent comprises the following steps:
[0048] Put fly ash, coal gangue, slag, KH792 modified basalt fiber and YDH-171 modified calcium zeolite into a mixer and stir and mix them at a stirring speed of 200 r / min for 30 minutes; then add an alkaline activator and continue stirring for 15 minutes to obtain an environmentally friendly mineral-based gelling agent.
[0049] Example 2
[0050] The difference between Example 2 and Example 1 is that: an environmentally friendly mineral-based gelling agent, calculated by weight, comprises the following components:
[0051] 30 parts of fly ash; the particle size of the fly ash is 300 μm;
[0052] 15 parts of coal gangue; the particle size of the fly ash is 50 μm;
[0053] 35 parts of slag; the particle size of the slag is 250 μm;
[0054] 4 parts of KH792 modified basalt fiber; the basalt fiber has a length of 1 mm and an aspect ratio of 100:1;
[0055] 7 parts of YDH-171 modified calcium zeolite; the particle size of the calcium zeolite is 300nm;
[0056] 5 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.4:0.1:1:0.6.
[0057] Example 3
[0058] The difference between Example 2 and Example 1 is that: an environmentally friendly mineral-based gelling agent, calculated by weight, comprises the following components:
[0059] 20 parts of fly ash; the particle size of the fly ash is 100 μm;
[0060] 25 parts of coal gangue; the particle size of the fly ash is 150 μm;
[0061] 25 parts of slag; the particle size of the slag is 150 μm;
[0062] 8 parts of KH792 modified basalt fiber; the basalt fiber has a length of 5 mm and an aspect ratio of 500:1;
[0063] 3 parts of YDH-171 modified calcium zeolite; the particle size of the calcium zeolite is 100 nm;
[0064] 9 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.2:0.3:1:0.4.
[0065] Comparative Example 1
[0066] The difference between Comparative Example 1 and Example 1 is that an equal amount of basalt fiber is used to replace the KH792 modified basalt fiber.
[0067] Comparative Example 2
[0068] The difference between Comparative Example 2 and Example 1 is that an equal amount of calcium zeolite is used to replace the YDH-171 modified calcium zeolite.
[0069] Comparative Example 3
[0070] The difference between Comparative Example 3 and Example 1 is that an equal amount of KH792-modified basalt fiber is used to replace YDH-171-modified calcium zeolite.
[0071] Comparative Example 4
[0072] The difference between Comparative Example 4 and Example 1 is that an equal amount of carbide slag is used to replace nano magnesium oxide.
[0073] Comparative Example 5
[0074] The difference between Comparative Example 5 and Example 1 is that an equal amount of NaOH is used to replace nano magnesium oxide.
[0075] The mechanical properties of Examples 1-3 and Comparative Example 5 were tested. The specific test results are shown in Table 1:
[0076] Among them, the test standard is: GB / T 17671-2021, using a compressive strength testing machine for 7d compressive strength test
[0077] Table 1
[0078] 7d compressive strength (MPa) 7d compressive strength (MPa) Example 1 6.25 Comparative Example 2 5.84 Example 2 6.12 Comparative Example 3 5.46 Example 3 6.22 Comparative Example 4 5.96 Comparative Example 1 5.88 Comparative Example 5 6.02
[0079] It can be seen from Table 1 that the environmentally friendly mineral-based gelling agent prepared by the present invention has a 7d compressive strength of up to 6.25 MPa. Moreover, from the comparison between Example 1 and Comparative Examples 1-5, it can be seen that the present invention significantly promotes the improvement of the mechanical properties of the environmentally friendly mineral-based gelling agent through modification treatment and interaction between components.
[0080] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An environmentally friendly mineral-based gelling agent, Features: By weight, it includes the following components: 20-30 parts of fly ash; 15-25 parts of coal gangue; 25-35 parts of slag; 4-8 parts of KH792 modified basalt fiber; 3-7 parts of YDH-171 modified calcium zeolite; 5-9 parts of alkaline activator; the alkaline activator is carbide slag, nano magnesium oxide, NaOH and water, and the mass ratio of the carbide slag, nano magnesium oxide, NaOH and water is: 0.2-0.4: 0.1-0.3: 1: 0.4-0.
6.
2. An environmentally friendly mineral-based gelling agent according to claim 1, Features: The particle size of the fly ash is 100-300 μm; the particle size of the fly ash is 50-150 μm.
3. An environmentally friendly mineral-based gelling agent according to claim 1, Features: The particle size of the slag is 150-250 μm; the length of the basalt fiber is 1-5 mm, and the aspect ratio is 100-500:1; and the particle size of the calcium zeolite is 100-300 nm.
4. An environmentally friendly mineral-based gelling agent according to claim 1, Features: The preparation method of the KH792-modified basalt fiber comprises: adding basalt fiber and KH792 to ethanol, heating to 60-80° C. for reaction for 1-3 hours, filtering, washing, and vacuum drying at 80° C. to constant weight to obtain the KH792-modified basalt fiber.
5. An environmentally friendly mineral-based gelling agent according to claim 4, Features: The mass ratio of the basalt fiber to KH792 is 10:1-3.
6. An environmentally friendly mineral-based gelling agent according to claim 1, Features: The preparation method of YDH-171 modified calcium zeolite includes: heat-treating the calcium zeolite, cooling to room temperature, then ultrasonically dispersing the heat-treated calcium zeolite and YDH-171 in ethanol, heating to 70-90°C for reaction for 1-3 hours, cooling to room temperature, filtering, washing, and vacuum drying at 80°C to constant weight to obtain YDH-171 modified calcium zeolite.
7. An environmentally friendly mineral-based gelling agent according to claim 6, Features: The mass ratio of the heat-treated calcium zeolite to YDH-171 is 5:1-2.
8. An environmentally friendly mineral-based gelling agent according to claim 6, Features: The heat treatment is performed at 120-140° C. for 3-5 hours.
9. A method for preparing an environmentally friendly mineral-based gelling agent according to any one of claims 1 to 8, Features: The preparation method comprises the following steps: Put fly ash, coal gangue, slag, KH792 modified basalt fiber and YDH-171 modified calcium zeolite into a mixer and stir and mix them, then add alkaline activator, continue stirring for a certain time, and obtain an environmentally friendly mineral-based gelling agent.
10. A method for preparing an environmentally friendly mineral-based gelling agent according to claim 9, Features: The stirring speed is 150-250 r / min, and the stirring is 20-40 min; the continuous stirring time is 10-20 min.
Citation Information
Patent Citations
Preparation method of freeze-thaw-resistant volcanic ash-based geopolymer excited and synthesized by composite waste alkali
CN117865532A
Geopolymer prepared from waste incineration fly ash bottom slag and system process method
CN117964261A
Waste glass powder reinforced geopolymer regenerated fireproof mortar and preparation method thereof
CN117964288A
Alkali-activated cementing material and preparation method thereof
CN106746781A
Preparation method of mineral fiber reinforced geopolymer-based wood adhesive
CN113122150A