Preparation method of high concentration perfluorosulfonic acid resin solution and perfluorosulfonic acid ion exchange membrane
By heating and homogenizing the perfluorosulfonic acid resin solution, a high-concentration jelly resin solution was prepared, which solved the problems of poor dispersion uniformity and unstable film thickness caused by jelly phenomenon, and achieved the stability and scale of the high-concentration resin solution The thickness deviation of the obtained perfluorosulfonic acid ion exchange film is less than 7%, which is suitable for a variety of electrochemical applications.
Patent Information
- Application Number
- CN202411002023.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The prior art is prone to gel freezing when preparing high-concentration perfluorosulfonic acid resin solutions, resulting in poor dispersion uniformity and unstable film thickness, which affects the performance and repeatability of the ion exchange membrane.
The perfluorosulfonic acid resin solution with a mass fraction of 4% to 6% is heated to 80°C to 120°C to prepare a jelly resin solution with a mass fraction of 20% to 30%, and a solvent is added to homogenize the process to obtain a mass fraction of 15 The high-concentration jelly resin solution of %~25% has a homogenization pressure of 80MPa~100MPa, a time of 4 hours~6 hours, ensuring that the resin particle size is not greater than 1 micron, and finally forming a film on the casting machine.
The accurate concentration control of high-concentration perfluorosulfonic acid resin solution is achieved, and the stability is improved. It is suitable for large-scale production. The thickness deviation of the obtained perfluorosulfonic acid ion exchange film is less than 7%, which is suitable for electrochemicals such as fuel cells and flow batteries. field.
Smart Images

Figure CN118546397B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ion exchange membranes, and in particular to a method for preparing a high-concentration perfluorosulfonic acid resin solution and a perfluorosulfonic acid ion exchange membrane. Background Art
[0002] At present, the preparation methods of perfluorosulfonic acid ion exchange membrane mainly include melt extrusion film forming method and solution film forming method. The preparation process of melt extrusion method is complicated, and the equipment requirements are very high, so the cost of equipment is also very high. Solution film forming method includes solution casting molding method and solution casting method. Casting method is suitable for mass production. Before film formation, it is necessary to prepare resin solution. Ethanol aqueous solution, isopropanol aqueous solution, DMF, 1,2-propylene glycol, etc. can be used to prepare resin solution.
[0003] If DMF is used to prepare the resin solution, it needs to be heated to 180℃~210℃ and kept at a constant temperature for 4 hours to obtain a resin solution with a mass fraction of 5%. In the resin and DMF solution, when the resin content exceeds 6% by mass or the temperature is heated unevenly, jelly will be produced (this is a common phenomenon of polymer solutions): under appropriate conditions, it loses fluidity and becomes an elastic semi-solid state, which is called gel. Gels with a high liquid content are also called jelly. The process of resin solution producing jelly can be regarded as a stage in the sol precipitation process. During gelation, the colloid loses its aggregation stability, but still has dynamic stability. It is a special semi-solid state. The colloidal particles are interconnected to form a network structure. The gaps in the structure are filled with liquid and no precipitation is generated.
[0004] With the jelly solution, its dispersion uniformity becomes worse, the thickness value deviation at each position after film formation is large, the conductivity of the membrane is unstable and the repeatability is poor, which affects the use. Therefore, the dispersion uniformity of perfluorosulfonic acid solution is an important indicator. The preparation of a uniformly dispersed resin solution is a prerequisite for ensuring the good performance of the ion exchange membrane. The solid content of the jelly may be lower than the solid content of the solution, and the jelly has poor fluidity. When the resin content is lower than 15% by mass, a casting machine cannot be used for film formation. The preparation of a high-concentration resin solution with a mass fraction of more than 15% is particularly prone to jelly. The current process is complicated and there is no simple and effective method. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0006] To this end, the first aspect of the present invention provides a method for preparing a high-concentration perfluorosulfonic acid resin solution, comprising:
[0007] Heat a 4% to 6% perfluorosulfonic acid resin solution to 80°C to 120°C to prepare a 20% to 30% jelly resin solution;
[0008] Then, a solvent is added to prepare a jelly resin solution having a mass fraction of 15% to 25%;
[0009] The jelly resin solution with a mass fraction of 15% to 25% is homogenized to obtain a high-concentration perfluorosulfonic acid resin solution.
[0010] Furthermore, the solvent of the perfluorosulfonic acid resin solution includes one of N,N-dimethylformamide, dimethyl sulfoxide or dimethylacetamide.
[0011] Furthermore, the perfluorosulfonic acid resin in the perfluorosulfonic acid resin solution has an EW value of 700-1300, including: new perfluorosulfonic acid resin and / or perfluorosulfonic acid resin recovered by chlor-alkali ion membrane.
[0012] Furthermore, the particle size of the homogenized perfluorosulfonic acid resin is controlled to be no greater than 1 micron.
[0013] Furthermore, the homogenization method includes: a homogenization pressure of 80MPa to 100MPa, and a homogenization time of 4 hours to 6 hours.
[0014] The second aspect of the present invention provides a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0015] The high-concentration perfluorosulfonic acid resin solution prepared by the above-mentioned method for preparing the high-concentration perfluorosulfonic acid resin solution is formed into a film on a casting machine to obtain the perfluorosulfonic acid ion exchange membrane.
[0016] Furthermore, the preparation method also includes: degassing treatment before film formation on a casting machine, and the degassing method includes: placing the high-concentration perfluorosulfonic acid resin solution in a degassing machine and placing it in a vacuum for 8 to 10 hours.
[0017] Furthermore, the film is formed on the casting machine, and the method includes: putting the high-concentration perfluorosulfonic acid resin solution into the casting machine, and obtaining a perfluorosulfonic acid ion exchange membrane of required thickness by controlling the coating thickness.
[0018] Furthermore, the thickness of the perfluorosulfonic acid ion exchange membrane ranges from 25 μm to 125 μm, and the thickness deviation is less than 7%.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] The high-concentration perfluorosulfonic acid resin solution provided by the present invention has a simple preparation method, can accurately control the concentration of the high-concentration perfluorosulfonic acid resin solution, has stable quality, and is suitable for large-scale promotion; the obtained high-concentration perfluorosulfonic acid resin solution is directly used for preparing a perfluorosulfonic acid ion exchange membrane by a tape casting machine, has a simple process, stable quality, and is suitable for large-scale promotion; the obtained perfluorosulfonic acid ion exchange membrane has a thickness deviation of less than 7%, and can be used in electrochemical fields such as fuel cells, liquid flow batteries, water electrolysis to produce hydrogen, electrolysis and electroplating, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A flow chart for preparing a perfluorosulfonic acid ion exchange membrane provided in an embodiment of the present application. DETAILED DESCRIPTION
[0022] In order to better understand the above technical solution, the technical solution of the present invention is described in detail below through specific embodiments.
[0023] A first aspect of an embodiment of the present invention provides a method for preparing a high-concentration perfluorosulfonic acid resin solution, comprising:
[0024] Heat a 4% to 6% perfluorosulfonic acid resin solution to 80°C to 120°C to prepare a 20% to 30% jelly resin solution;
[0025] Then, a solvent is added to prepare a jelly resin solution having a mass fraction of 15% to 25%;
[0026] The jelly resin solution with a mass fraction of 15% to 25% is homogenized to obtain a high-concentration perfluorosulfonic acid resin solution.
[0027] The high-concentration perfluorosulfonic acid resin solution provided in the embodiment of the present invention has a simple preparation method, can accurately control the concentration of the high-concentration perfluorosulfonic acid resin solution, has stable quality, and is suitable for large-scale promotion; the obtained high-concentration perfluorosulfonic acid resin solution is directly used in a casting machine to prepare a perfluorosulfonic acid ion exchange membrane, has a simple process, stable quality, and is suitable for large-scale promotion.
[0028] Specifically, the embodiment of the present invention adopts a two-step method to prepare a high-concentration perfluorosulfonic acid resin solution, that is, first prepare a jelly resin solution with a mass fraction of 20% to 30%, and then add a solvent to the jelly resin solution with a mass fraction of 20% to 30%. Because the accurate proportion of the solvent is added in the second step, the mass fraction of the jelly resin solution can be accurately controlled, and finally a jelly resin solution with an accurate mass fraction of 15% to 25% is prepared. If a jelly resin solution with a mass fraction of 15% to 25% is prepared by directly heating a perfluorosulfonic acid resin solution with a mass fraction of 4% to 6% to 80°C to 120°C and evaporating the solvent, the mass fraction of the generated jelly resin solution will be inaccurate, which will cause uneven film thickness in subsequent film making. Regarding the heating temperature of the perfluorosulfonic acid resin solution, the reason why 80°C to 120°C is selected is that the temperature is lower than 80°C, the solvent evaporates too slowly, and the temperature is higher than 120°C, and a dry film is easily formed in the solution, and the dry film cannot be restored. A 4% to 6% perfluorosulfonic acid resin solution is heated to 80°C to 120°C, and a 20% to 30% jelly resin solution is prepared by comprehensively considering the solution volume, heating power, and heating time. For example, a 5% perfluorosulfonic acid resin solution with a volume of 2L has a heating power of 1KW and a heating time of 2 hours to 4 hours.
[0029] In a feasible embodiment, the solvent of the perfluorosulfonic acid resin solution includes one of N,N-dimethylformamide, dimethyl sulfoxide or dimethylacetamide.
[0030] It is understandable that common solvents for perfluorosulfonic acid resins can be selected, including dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dimethylacetamide (DMAC), etc. We compared the use of the above three solvents to prepare 15%~25% mass fraction of jelly resin solution, and then used the same method to cast the membrane. There was no obvious difference in the performance of the perfluorosulfonic acid ion exchange membrane obtained.
[0031] In a feasible implementation, the perfluorosulfonic acid resin in the perfluorosulfonic acid resin solution has an EW value of 700-1300, including: new perfluorosulfonic acid resin and / or perfluorosulfonic acid resin recovered from chlor-alkali ion membrane.
[0032] Specifically, we compared the use of new perfluorosulfonic acid resin and perfluorosulfonic acid resin recovered by chlor-alkali ion membrane, and found that there was no difference in the use of the recycled perfluorosulfonic acid resin and the new perfluorosulfonic acid resin, and there was no difference in the performance of the perfluorosulfonic acid ion exchange membrane. According to the different application fields of the fluorosulfonic acid ion exchange membrane, the EW value of the perfluorosulfonic acid resin is selected between 700 and 1300.
[0033] In a feasible implementation manner, the particle size of the homogenized perfluorosulfonic acid resin is controlled to be no larger than 1 micron.
[0034] In this technical solution, we have found through multiple casting machine film forming experiments that when homogenized to more than 1 micron, the generated perfluorosulfonic acid ion exchange membrane will have local thick spots, so the particle size of the perfluorosulfonic acid resin after homogenization is controlled to be no more than 1 micron.
[0035] In a feasible implementation manner, the homogenization method includes: a homogenization pressure of 80 MPa to 100 MPa, and a homogenization time of 4 hours to 6 hours.
[0036] In this technical solution, according to theoretical analysis and experimental verification of the effect of the homogenizer, when the pressure of the homogenizer reaches 30Mpa, it begins to work on the liquid-solid dispersion, and when the pressure reaches 60Mpa, the particle size of most materials can reach less than 2 microns; when the pressure reaches 80Mpa or above, the effect is more obvious, and the particle size of the material can reach less than 1 micron, which is mainly used for ultrafine particle crushing; and when the pressure reaches more than 100Mpa, finer particles can be produced. After ultra-high pressure homogenization, the material can obtain a particle size of 0.1 micron to 0.5 micron. At this time, the thickness deviation of the prepared perfluorosulfonic acid ion exchange membrane is easier to be small; taking all factors into consideration, the homogenization pressure is 80MPa~100MPa, the homogenization time is 4 hours~6 hours, and the thickness deviation of the prepared perfluorosulfonic acid ion exchange membrane meets the requirement of less than 7%.
[0037] A second aspect of the embodiments of the present invention provides a perfluorosulfonic acid ion exchange membrane, the preparation method of which includes:
[0038] The high-concentration perfluorosulfonic acid resin solution prepared by the above-mentioned method is used to form a membrane on a casting machine to obtain a perfluorosulfonic acid ion exchange membrane.
[0039] In the embodiment of the present invention, a high-concentration perfluorosulfonic acid resin solution is directly used in a tape casting machine to prepare a perfluorosulfonic acid ion exchange membrane. This method has simple process and stable quality and is suitable for large-scale promotion.
[0040] In a feasible embodiment, the preparation method further includes: degassing treatment before film formation on the casting machine, the degassing method includes: placing the high-concentration perfluorosulfonic acid resin solution in a degassing machine, evacuating to a limit value of -0.1MPa, and leaving it for 8 to 10 hours. This degassing method is simple and practical and can process various solutions.
[0041] In a feasible embodiment, the film is formed on a casting machine, and the method includes: placing a high-concentration perfluorosulfonic acid resin solution into the casting machine, and controlling the coating thickness to obtain a perfluorosulfonic acid ion exchange membrane of a required thickness. Generally speaking, the thickness of the perfluorosulfonic acid ion exchange membrane obtained by control is in the range of 25μm to 125μm. The thickness of the perfluorosulfonic acid ion exchange membrane ranges from 25μm to 125μm, and the thickness deviation is less than 7%.
[0042] A third aspect of the embodiments of the present invention provides an application of a perfluorosulfonic acid ion exchange membrane, which is used in the field of electrochemistry, including but not limited to fuel cells, liquid flow batteries, water electrolysis to produce hydrogen, electrolytic plating, etc.
[0043] Example 1 A perfluorosulfonic acid ion exchange membrane
[0044] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0045] (1) 10L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 120°C using a 1KW heating device for 4 hours to produce 1.67L of 30% jelly resin solution.
[0046] (2) Add DMF solvent to prepare 2 L of 25% jelly resin solution.
[0047] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 25% is obtained.
[0048] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0049] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.200 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 50 microns, and the membrane thickness deviation is 6%.
[0050] Example 2 A method for preparing a perfluorosulfonic acid ion exchange membrane
[0051] See also Figure 1 , a method for preparing a perfluorosulfonic acid ion exchange membrane, comprising:
[0052] (1) 9.2 L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 80°C using a 1 kW heating device for 6 hours to obtain 1.64 L of 28% jelly resin solution.
[0053] (2) Add DMF solvent to prepare 2 L of 23% jelly resin solution.
[0054] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 23% is obtained.
[0055] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0056] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.217 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 50 microns, and the membrane thickness deviation is 5.8%.
[0057] Example 3 A perfluorosulfonic acid ion exchange membrane
[0058] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0059] (1) 8.4 L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 90°C using a 1 kW heating device for 5 hours to obtain 1.62 L of 26% jelly resin solution.
[0060] (2) Add DMF solvent to prepare 2 L of 21% jelly resin solution.
[0061] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 21% is obtained.
[0062] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0063] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.238 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 50 microns, and the membrane thickness deviation is 6.2%.
[0064] Example 4 A perfluorosulfonic acid ion exchange membrane
[0065] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0066] (1) Heat 10 L of 5% by mass perfluorosulfonic acid resin (EW value 1000) in dimethyl sulfoxide (DMSO) to 120°C using a 1 kW heating device for 4 hours to obtain 1.67 L of 30% by mass jelly resin solution.
[0067] (2) Add DMSO solvent to prepare 2 L of 25% jelly resin solution.
[0068] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 25% is obtained.
[0069] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0070] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.200 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 50 microns, and the membrane thickness deviation is 6.4%.
[0071] Example 5 A perfluorosulfonic acid ion exchange membrane
[0072] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0073] (1) 10 L of a 5% by mass perfluorosulfonic acid resin solution in dimethylacetamide (DMAC) with an EW value of 1000 was heated to 120°C using a 1 kW heating device for 4 hours to obtain 1.67 L of a 30% by mass jelly resin solution.
[0074] (2) Add DMAC solvent to prepare 2 L of 25% jelly resin solution.
[0075] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 25% is obtained.
[0076] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0077] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.200 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 50 microns, and the membrane thickness deviation is 6.3%.
[0078] Example 6 A perfluorosulfonic acid ion exchange membrane
[0079] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0080] (1) 7.2 L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 100°C using a 1 kW heating device for 5 hours to obtain 1.57 L of 23% jelly resin solution.
[0081] (2) Add DMF solvent to prepare 2 L of 18% jelly resin solution.
[0082] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 18% is obtained.
[0083] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0084] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.139 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 25 microns, and the membrane thickness deviation is 4.3%.
[0085] Example 7 A perfluorosulfonic acid ion exchange membrane
[0086] See also Figure 1 , a perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0087] (1) 6L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 100°C using a 1KW heating device for 4.5 hours to obtain 1.5L of 20% jelly resin solution.
[0088] (2) Add DMF solvent to prepare 2 L of 15% jelly resin solution.
[0089] (3) Place the jelly resin solution in a homogenizer and homogenize at 90 MPa for 5 hours. After homogenization, the particle size is less than 1 micron, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 18% is obtained.
[0090] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0091] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.694 mm. The thickness of the perfluorosulfonic acid ion exchange membrane obtained is 125 μm, and the membrane thickness deviation is 6.8%.
[0092] Comparative Example 1: A perfluorosulfonic acid ion exchange membrane
[0093] A perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0094] (1) 2L of 5% perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 120°C for 0.5 hours using a 1KW heating device to obtain 0.5L of 25% jelly resin solution. The actual detected concentration was 23.6% with a concentration deviation of 5.6%.
[0095] The concentration of the obtained solution is inconsistent with that of the theoretical solution, and the perfluorosulfonic acid ion exchange membrane cannot be prepared.
[0096] Comparative Example 2: A perfluorosulfonic acid ion exchange membrane
[0097] A perfluorosulfonic acid ion exchange membrane, the preparation method comprising:
[0098] (1) 2 L of 5% by mass perfluorosulfonic acid resin DMF solution with an EW value of 1000 was heated to 120°C for 0.5 h using a 1 kW heating device to obtain 0.33 L of 30% by mass jelly resin solution.
[0099] (2) Add DMF solvent to prepare 0.4 L of 25% mass fraction jelly resin solution.
[0100] (3) Place the jelly resin solution in a homogenizer and homogenize at 70 MPa for 5 hours. After homogenization, the particle size is less than 2 microns, and finally a high-concentration perfluorosulfonic acid resin dispersion solution with a mass fraction of 25% is obtained.
[0101] (4) Place the high-concentration perfluorosulfonic acid resin dispersion solution in a degassing machine, evacuate to the limit value of -0.1MPa, and place it for 8 hours for vacuum degassing.
[0102] (5) The degassed high-concentration perfluorosulfonic acid resin dispersion solution is placed in a tape casting machine to form a film directly. The coating thickness is controlled to be 0.200 mm, and the perfluorosulfonic acid ion exchange membrane thickness is 50 microns. The membrane thickness deviation is 13%, which is far more than the allowable membrane thickness deviation of 7%.
[0103] Results and discussion: The performance of the perfluorosulfonic acid ion exchange membranes prepared in Examples 1 to 7 and Comparative Example 2 is shown in Table 1. Comparative Example 1 did not produce a membrane, and Examples 1 to 7 only differed in thickness or thickness deviation, while the other technical index test data were basically the same. The test method was based on GB / T 20042.3-2022.
[0104] Table 1 Performance of perfluorosulfonic acid ion exchange membranes prepared in Examples 1 to 7 and Comparative Example 2
[0105]
[0106] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.
Claims
1. A method for preparing a high concentration perfluorosulfonic acid resin solution, characterized in that: include: Heat a 4% to 6% perfluorosulfonic acid resin solution to 80°C to 120°C to prepare a 20% to 30% jelly resin solution; Then, a solvent is added to prepare a jelly resin solution having a mass fraction of 15% to 25%; The jelly resin solution with a mass fraction of 15% to 25% is homogenized to obtain a high-concentration perfluorosulfonic acid resin solution; The solvent of the perfluorosulfonic acid resin solution includes one of N,N-dimethylformamide, dimethyl sulfoxide or dimethylacetamide; The particle size of the homogenized perfluorosulfonic acid resin is controlled to be no greater than 1 micron; The homogenization method includes: a homogenization pressure of 80MPa to 100MPa, and a homogenization time of 4 hours to 6 hours.
2. The method for preparing a high concentration perfluorosulfonic acid resin solution according to claim 1, characterized in that: The perfluorosulfonic acid resin in the perfluorosulfonic acid resin solution has an EW value of 700-1300, including: new perfluorosulfonic acid resin and / or perfluorosulfonic acid resin recovered by chlor-alkali ion membrane.
3. A perfluorosulfonic acid ion exchange membrane, characterized in that: The preparation method comprises: The method for preparing a high-concentration perfluorosulfonic acid resin solution according to any one of claims 1 to 2 is used to form a film of the high-concentration perfluorosulfonic acid resin solution on a casting machine to obtain the perfluorosulfonic acid ion exchange membrane.
4. The perfluorosulfonic acid ion exchange membrane according to claim 3, characterized in that: The preparation method further comprises: degassing treatment before film formation on a casting machine, wherein the degassing method comprises: placing the high-concentration perfluorosulfonic acid resin solution in a degassing machine and placing it in a vacuum for 8 to 10 hours.
5. The perfluorosulfonic acid ion exchange membrane according to claim 3, characterized in that: The film is formed on the casting machine, and the method includes: putting the high-concentration perfluorosulfonic acid resin solution into the casting machine, and obtaining a perfluorosulfonic acid ion exchange membrane of required thickness by controlling the coating thickness.
6. The perfluorosulfonic acid ion exchange membrane according to claim 3, characterized in that: The thickness of the perfluorosulfonic acid ion exchange membrane ranges from 25 μm to 125 μm, and the thickness deviation is less than 7%.
Citation Information
Patent Citations
Method for modifying perfluorosulfonic acid proton exchange membrane through gel extrusion casting
CN113078344A
Preparation method of perfluorinated sulfonic acid resin dispersion liquid
CN114276561A
Method for preparing perfluorinated sulfonic acid ionic membrane by gel extruding and flow-flattening film
CN1990527A