A flame retardant MPP power cable sheath and preparation method thereof

By performing cross-linking network processing of surface modification and polyurethane-bound cross-linking network processing of basalt fibers, the dispersion and impact resistance in flame retardant MPP power cable sheath is solved, significantly improving the flame retardant effect and oxidation resistance, satisfying the High-performance power cable sheathing demand.

CN118546463BActive Publication Date: 2024-11-15SHAANXI SHENGXIANG PIPELINE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411016703.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Basalt fibers have problems such as poor dispersion and flowability, low impact strength and oxidation and brittleness in the preparation of flame retardant MPP power cable sheath tubes, which limits its application.

Method used

By modifying the basalt fibers with aminosilane coupling agent, surfactant and dodecylamine-N-acetic acid-N-methylenephosphonic acid, a stable high-density cross-linking network is formed in combination with polyurethane, improving its relationship with polypropylene Compatibility and dispersion of resins, and the flame retardant MPP power cable sheathing was prepared by extrusion process.

Benefits of technology

It significantly improves the flame retardant effect and impact resistance, solves the problem of basalt fibers being easily oxidized and brittle, and meets the needs of high-performance power cable sheaths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of modified polypropylene pipes, and relates to a flame-retardant MPP power cable sheath pipe and a preparation method thereof. The present invention provides a flame-retardant MPP power cable sheath pipe, and its preparation raw materials are composed of a PP substrate, a flame retardant, an antioxidant and a modified inorganic filler; the modified inorganic filler is composed of a modified basalt fiber and a polyurethane; the modified basalt fiber is a basalt fiber that is modified by an aminosilane coupling agent and a surfactant, and then modified by dodecylamine-N-acetic acid-N-methylenephosphonic acid. The modified inorganic filler provided by the present invention realizes that in the preparation process of the modified polypropylene pipe, a stable and high-density cross-linked ion bonding network is formed in the interface area of ​​the composite material with the assistance of polyurethane, and is tightly connected to polypropylene through covalent bonds and hydrogen bonds, effectively improving its flame retardant effect and impact strength, and solving the technical problem that it is prone to oxidation and brittleness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of modified polypropylene pipes and relates to a flame-retardant MPP power cable sheath pipe and a preparation method thereof. Background Art

[0002] Polypropylene has the advantages of high electrical insulation, good heat resistance, low density, low material cost, and strong corrosion resistance, and has been widely used in production and life. Modified polypropylene (MPP) is an important raw material for the preparation of power cable sheath pipes. With the increase in urban infrastructure investment and the rapid development of the power industry, the demand for sheath pipes that play an important protective role in the transmission of power cables has also increased. Since power cables usually need to be laid underground in a trenchless manner, and a certain amount of heat loss is usually generated during the power transmission process, this requires MPP sheath pipes with high strength, corrosion resistance, good thermal conductivity, long service life, and excellent earthquake resistance and resistance to ground settlement. This puts higher requirements on the performance of existing MPP power cable sheath pipes.

[0003] Basalt fiber is a continuous fiber made by melting basalt stone at 1450~1500℃ and then drawing it at high speed through a platinum-rhodium alloy drawing plate. Compared with short fibers such as glass fiber, asbestos, and rock wool, basalt fiber has a higher aspect ratio, is not easily inhaled into the lungs, is safer, and has a pollution-free production process. Basalt fiber does not produce harmful substances at high temperatures, has excellent thermal protection and mechanical properties, and is widely used in fabrics, building materials, and lightweight automotive materials. Because basalt fiber has a greater density and more surface defects than glass fiber, basalt fiber has many defects such as poor dispersion and fluidity when used directly in the preparation of flame-retardant MPP power cable sheaths, low impact strength, and easy oxidation and brittleness, which hinders the application of basalt fiber in this field. Summary of the invention

[0004] The purpose of the present invention is to solve at least one of the above-mentioned technical problems, focusing on how to realize the application of basalt fiber in the preparation of flame-retardant MPP power cable sheath in a simple and low-cost way. To this end, the present invention provides a flame-retardant MPP power cable sheath and a preparation method thereof to solve this need in the art.

[0005] On the one hand, the present invention relates to a flame-retardant MPP power cable sheath tube, the preparation raw materials of which are composed of a PP substrate, a flame retardant, an antioxidant and a modified inorganic filler;

[0006] The modified inorganic filler is composed of modified basalt fiber and polyurethane;

[0007] The modified basalt fiber is prepared by subjecting the basalt fiber to modification treatment with an aminosilane coupling agent and a surfactant, and then to modification with dodecylamine-N-acetic acid-N-methylenephosphonic acid;

[0008] The density of the basalt fiber is 2.65-3.0 g / cm 3 , diameter is 7~25μm, breaking strength is >1200MPA, and elongation at break is 2.4~3.1%.

[0009] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the raw materials for preparation are composed, by weight, of 100 parts of PP substrate, 20 to 25 parts of flame retardant, 1 to 3 parts of antioxidant, and 15 to 25 parts of modified inorganic filler.

[0010] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the mass ratio of the basalt fiber to the polyurethane is 10:3-6.

[0011] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the flame retardant is selected from at least one of hexahydroxymethylmelamine, melamine, ammonium polyphosphate, sodium tetraborate, and polyamide.

[0012] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the antioxidant is one of antioxidant 1010 and antioxidant AO-6.

[0013] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the aminosilane coupling agent is one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, and 3-[2-(2-aminoethylamino)ethylamino]propyl-trimethoxysilane.

[0014] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the surfactant is a cationic surfactant.

[0015] Furthermore, in the flame-retardant MPP power cable sheath provided by the present invention, the cationic surfactant is selected from at least one of dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride.

[0016] On the other hand, the present invention relates to a method for preparing the flame-retardant MPP power cable sheath pipe, which comprises: washing and drying basalt fiber, placing it in a solution containing an aminosilane coupling agent and a surfactant, ultrasonically dispersing it uniformly, reacting it at 60-65° C. for 3-6 hours, drying it, placing it in a dodecylamine-N-acetic acid-N-methylenephosphonic acid solution, reacting it at 70-80° C. for 4-6 hours, washing it with deionized water, drying it, and mixing it with polyurethane to obtain the modified inorganic filler;

[0017] The prepared raw materials are mixed at a temperature of 95-105° C. for 10-20 minutes, and extruded to obtain a flame-retardant MPP power cable sheath tube.

[0018] Furthermore, in the method provided by the present invention, in the solution containing the aminosilane coupling agent and the surfactant, the concentration of the aminosilane coupling agent is 20-30wt%, and the concentration of the surfactant is 5-10wt%;

[0019] The concentration of dodecylamine-N-acetic acid-N-methylenephosphonic acid in the dodecylamine-N-acetic acid-N-methylenephosphonic acid solution is 5-10 wt %.

[0020] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects or advantages:

[0021] The present invention solves many problems existing when basalt fiber is used for the preparation of flame-retardant MPP power cable sheath pipe, improves the compatibility of basalt fiber and polypropylene resin, improves the flame retardant effect and impact strength of flame-retardant MPP power cable sheath pipe, and solves the technical problem that it is easy to oxidize and become brittle. First, the present invention is used to improve the roughness of the surface of basalt fiber and repair its surface defects by surface modification of basalt fiber with aminosilane coupling agent, surfactant and dodecylamine-N-acetic acid-N-methylenephosphonic acid. Secondly, the present invention further modifies the surface of dodecylamine-N-acetic acid-N-methylenephosphonic acid using the characteristics of dodecylamine-N-acetic acid-N-methylenephosphonic acid. When dodecylamine-N-acetic acid-N-methylenephosphonic acid is combined with the material, only one phosphonic acid group is combined with the modified basalt fiber, and the other phosphonic acid group is in a free state. Finally, in the present invention, polyurethane is added to finally prepare the flame-retardant MPP power cable sheath pipe. Based on the above-mentioned surface-modified characteristics, the network formed by the polyurethane and the basalt fiber with free phosphonic acid groups constitute a water-insoluble interpenetrating polymer network, and further form a stable high-density cross-linked ionic bonding network in the interface area of ​​the composite material, and tightly link with polypropylene through covalent bonds and hydrogen bonds, thereby improving the compatibility of basalt fiber and polypropylene resin, making it uniformly dispersed in the material, further improving the flame retardant effect and impact strength of the flame-retardant MPP power cable sheath pipe, and solving the technical problem of its easy oxidation and brittleness. DETAILED DESCRIPTION

[0022] The technical scheme of the present invention is described below in conjunction with the examples, but the present invention is not limited to the following examples. The experimental methods and detection methods described in each example are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified. The "%" indicates mass percentage unless otherwise specified.

[0023] Basalt fiber was purchased from Shandong Hengtai New Material Technology Co., Ltd. with a density of 2.65~3.0g / cm 3 , diameter is 7~25μm, breaking strength is >1200MPA, and elongation at break is 2.4~3.1%.

[0024] Example 1

[0025] This embodiment provides a flame-retardant MPP power cable sheath pipe and a preparation process thereof.

[0026] Step 1: Soak the basalt fiber in an acetone solution at 50°C for 1 hour, then clean it with deionized water, dry it in a vacuum drying oven at room temperature, take it out, and take polyurethane with a mass ratio of 10:3 for use.

[0027] Step 2: Place the basalt fiber obtained in step 1 into a mixed solution of 3-aminopropyltriethoxysilane and dodecyltrimethylammonium chloride (the concentration of 3-aminopropyltriethoxysilane is 20%, the concentration of dodecyltrimethylammonium chloride is 5%, and the solvent is anhydrous ethanol), disperse it evenly by ultrasonication, react at 60°C for 3h, then wash it with deionized water, dry it in a vacuum drying oven at room temperature, and take it out for use.

[0028] Step 3: Place the basalt fiber obtained in step 2 in a 5% dodecylamine-N-acetic acid-N-methylenephosphonic acid solution (solvent is isopropanol), react at 70°C for 4 hours, then wash with deionized water, dry in a vacuum drying oven at room temperature, take out and mix with polyurethane for later use (i.e., obtain a modified inorganic filler).

[0029] Step 4: Take 100 parts of PP substrate, 20 parts of flame retardant (hexahydroxymethyl melamine), 1 part of antioxidant (antioxidant 1010), and 15 parts of modified inorganic filler obtained in step 3 as raw materials, and mix and stir them evenly in a twin-screw extruder (MTS20, Jiangsu Deteng Mechanical and Electrical Equipment Co., Ltd.) at a temperature of 95°C for 10 minutes to prepare the flame-retardant MPP power cable sheath through an extrusion process.

[0030] Example 2

[0031] This embodiment provides a flame-retardant MPP power cable sheath pipe and a preparation process thereof.

[0032] Step 1: Soak the basalt fiber in an acetone solution at 50°C for 1.5 hours, then clean it with deionized water, dry it in a vacuum drying oven at room temperature, take it out, and take polyurethane with a mass ratio of 10:4 for use.

[0033] Step 2: Place the basalt fiber obtained in step 1 into a mixed solution of 3-aminopropyltrimethoxysilane and tetradecyltrimethylammonium chloride (the concentration of 3-aminopropyltrimethoxysilane is 22%, the concentration of tetradecyltrimethylammonium chloride is 7%, and the solvent is anhydrous ethanol), disperse it evenly by ultrasonication, react it at 60°C for 4h, then wash it with deionized water, dry it in a vacuum drying oven at room temperature, and then take it out for use.

[0034] Step 3: Place the basalt fiber obtained in step 2 in a 7% dodecylamine-N-acetic acid-N-methylenephosphonic acid solution (solvent is isopropanol), react at 70°C for 5 hours, then wash with deionized water, dry in a vacuum drying oven at room temperature, take out and mix with polyurethane for later use (i.e., obtain a modified inorganic filler).

[0035] Step 4: Take 100 parts of PP substrate, 22 parts of flame retardant (melamine), 2 parts of antioxidant (antioxidant AO-6), and 20 parts of modified inorganic filler obtained in step 3 as raw materials, mix and stir evenly in a twin-screw extruder (MTS20, Jiangsu Deteng Mechanical and Electrical Equipment Co., Ltd.) at a temperature of 100°C and a time of 15 minutes, and prepare the flame-retardant MPP power cable sheath through an extrusion process.

[0036] Example 3

[0037] This embodiment provides a flame-retardant MPP power cable sheath pipe and a preparation process thereof.

[0038] Step 1: Soak the basalt fiber in an acetone solution at 60°C for 2 hours, then clean it with deionized water, dry it in a vacuum drying oven at room temperature, take it out, and take polyurethane with a mass ratio of 10:3 for later use.

[0039] Step 2: The basalt fiber obtained in step 1 is placed in a mixed solution of 3-aminopropylmethyldiethoxysilane and hexadecyltrimethylammonium chloride (the concentration of 3-aminopropylmethyldiethoxysilane is 30%, the concentration of hexadecyltrimethylammonium chloride is 10%, and the solvent is anhydrous ethanol), and after being dispersed evenly by ultrasound, it is reacted at 65°C for 6h, and then washed with deionized water, dried in a vacuum drying oven at room temperature, and taken out for use.

[0040] Step 3: Place the basalt fiber obtained in step 2 in a 10% dodecylamine-N-acetic acid-N-methylenephosphonic acid solution (solvent is isopropanol), react at 80°C for 6 hours, then wash with deionized water, dry in a vacuum drying oven at room temperature, take out and mix with polyurethane for later use (i.e., obtain a modified inorganic filler).

[0041] Step 4: Take 100 parts of PP substrate, 25 parts of flame retardant (ammonium polyphosphate), 3 parts of antioxidant (antioxidant AO-6), and 20 parts of modified inorganic filler obtained in step 3 as raw materials, and mix and stir them evenly in a twin-screw extruder (MTS20, Jiangsu Deteng Mechanical and Electrical Equipment Co., Ltd.) at a temperature of 105°C for 20 minutes to prepare the flame-retardant MPP power cable sheath through an extrusion process.

[0042] Comparative Example 1

[0043] This comparative example is the same as Example 1, except that no polyurethane is added.

[0044] Comparative Example 2

[0045] This comparative example is the same as Example 1, except that dodecylamine-N-acetic acid-N-methylenephosphonic acid is replaced by phosphonic acid.

[0046] Comparative Example 3

[0047] This comparative example is the same as Example 1, except that dodecyltrimethylammonium chloride is replaced by carboxymethyl cellulose.

[0048] Comparative Example 4

[0049] This comparative example is the same as Example 1, except that the modified inorganic filler is replaced by basalt fiber.

[0050] Test Case

[0051] In this test example, the flame retardant MPP power cable sheath tube prepared as above was tested for flame retardancy, impact strength and oxidation embrittlement resistance.

[0052] The limiting oxygen index (LOI) indicates the volume fraction concentration of oxygen that can just support the combustion of the MPP power cable sheath in a mixture of oxygen and nitrogen. The higher the LOI value, the stronger the flame retardant performance. The limiting oxygen index (LOI, %) of the sample was tested according to ASTM 2863. Elongation at break is the ratio of the elongation of the material from the time of stretching to the time of fracture to the original length before the material breaks, and is an important indicator for evaluating the toughness of the material. A high elongation at break means that the material can undergo a greater degree of plastic deformation before breaking, thereby making the material have better resistance to impact damage. According to the standard of GB / T528-2009, the tensile rate is set to 500mm / min, and the elongation at break (%) of the material is tested. According to the standard of GB / T3512-2001, the accelerated thermal oxidative aging test is carried out at an aging temperature of 100℃, and then the change rate (%) of the elongation at break of the material at different times relative to that without accelerated thermal oxidative aging is measured to judge the oxidation resistance of the material. The flattening test and the drop hammer impact test are carried out according to the standard of DL / T 802.7-2010. The test results are shown in Table 1.

[0053] Table 1: Performance parameters of flame retardant MPP power cable sheath

[0054]

[0055] As shown in Table 1, the LOI of the flame-retardant MPP power cable sheath pipe prepared by the present invention is 41.7-47.8%, while the LOI of Comparative Example 1 without adding polyurethane is 32.6%, the LOI of Comparative Example 2 using phosphonic acid is 34.4%, the LOI of Comparative Example 3 using anionic surfactant is 38.3%, and the LOI of unmodified basalt fiber is 24.6%. The flame-retardant MPP power cable sheath pipe prepared by the present invention has a significant improvement in flame retardant effect by modifying basalt fiber. As shown in Comparative Example 4, when basalt fiber is directly used as filler for flame-retardant MPP power cable sheath pipe, its compatibility with polypropylene resin is poor, and it cannot meet the technical performance requirements specified in DL / T 802.7-2010 standard, and cannot be directly used for cable protection of power cables. The various data of the embodiments are significantly better than those of the comparative examples, indicating that the cross-linked network constructed by the participation of polyurethane, the adsorption mode of dodecylamine-N-acetic acid-N-methylenephosphonic acid and the appropriate surfactant cooperate with each other to improve the flame retardant effect, impact strength and oxidation embrittlement resistance of the MPP power cable sheath.

[0056] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.

Claims

1. A flame retardant MPP power cable sheath pipe, characterized in that: The preparation raw materials are composed of PP substrate, flame retardant, antioxidant and modified inorganic filler; The modified inorganic filler is composed of modified basalt fiber and polyurethane; The modified basalt fiber is prepared by subjecting the basalt fiber to modification treatment with an aminosilane coupling agent and a surfactant, and then to modification with dodecylamine-N-acetic acid-N-methylenephosphonic acid; The density of the basalt fiber is 2.65-3.0 g / cm 3 , diameter is 7~25μm, breaking strength>1200MPA, and breaking elongation is 2.4~3.1%; The basalt fiber is cleaned and dried, placed in a solution containing an aminosilane coupling agent and a surfactant, ultrasonically dispersed evenly, and reacted at 60-65° C. for 3-6 hours. After drying, the basalt fiber is placed in a dodecylamine-N-acetic acid-N-methylenephosphonic acid solution and reacted at 70-80° C. for 4-6 hours. After being washed with deionized water, the fiber is dried and mixed with polyurethane to obtain the modified inorganic filler.

2. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The raw materials for preparation are composed of 100 parts of PP substrate, 20-25 parts of flame retardant, 1-3 parts of antioxidant and 15-25 parts of modified inorganic filler in parts by mass.

3. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The mass ratio of the basalt fiber to the polyurethane is 10:3-6.

4. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The flame retardant is selected from at least one of hexamethylolmelamine, melamine, ammonium polyphosphate and sodium tetraborate.

5. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010 and antioxidant AO-6.

6. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The aminosilane coupling agent is one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane and 3-[2-(2-aminoethylamino)ethylamino]propyl-trimethoxysilane.

7. The flame-retardant MPP power cable sheath according to claim 1, characterized in that: The surfactant is a cationic surfactant.

8. The flame-retardant MPP power cable sheath pipe according to claim 7, characterized in that: The cationic surfactant is selected from at least one of dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride and hexadecyltrimethylammonium chloride.

9. A method for preparing the flame-retardant MPP power cable sheath pipe according to any one of claims 1 to 8, characterized in that: include: The prepared raw materials are mixed at a temperature of 95-105° C. for 10-20 minutes, and extruded to obtain a flame-retardant MPP power cable sheath tube.

10. The method for preparing a flame-retardant MPP power cable sheath pipe according to claim 9, characterized in that: In the solution containing the aminosilane coupling agent and the surfactant, the concentration of the aminosilane coupling agent is 20-30wt%, and the concentration of the surfactant is 5-10wt%; The concentration of dodecylamine-N-acetic acid-N-methylenephosphonic acid in the dodecylamine-N-acetic acid-N-methylenephosphonic acid solution is 5-10 wt %.