Triethylamine gas sensor based on ZnWO4 / ZnO composite material and its preparation method

By using triethylamine gas-sensitive sensors of ZnWO4/ZnO composite materials, the problems of high working temperature and low sensitivity in triethylamine detection in the prior art are solved, and high sensitivity detection at 160°C is achieved, with a wide detection range. Suitable for rapid identification of 0.5~40ppm and simplifies the process.

CN118549495BActive Publication Date: 2024-11-12HENAN XIANGZHI TECH TRANSFER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012134.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In the detection of triethylamine, existing metal oxide semiconductor gas sensors have problems such as high operating temperature, low sensitivity, long response recovery time and poor selectivity.

Method used

Using a triethylamine gas-sensitive sensor based on ZnWO4/ZnO composite material, ZnO fractionated microspheres were added to ammonium metatungstate solution for ultrasonic reaction, prepared by drying and calcining, coated on the surface of insulated ceramic tubes, and simplified by hydrothermal method. Process, reduce operating temperature and increase sensitivity.

Benefits of technology

It realizes high sensitivity detection at 160℃, has a wide detection range and significantly improves sensitivity (Ra/Rg), which is suitable for rapid identification of 0.5~40ppm of triethylamine, and is simple in process and low in cost, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118549495B_ABST
    Figure CN118549495B_ABST
Patent Text Reader

Abstract

The present invention relates to a triethylamine gas sensor based on ZnWO4 / ZnO composite material and a preparation method thereof. The gas sensor comprises an insulating ceramic tube, the two ends of the surface of the insulating ceramic tube are respectively provided with electrodes, a heating wire is passed through the inside of the insulating ceramic tube, the electrodes and the heating wire are respectively connected to the electrodes on the sensor base, the surface of the electrodes and the surface of the insulating ceramic tube between the electrodes are coated with ZnWO4 / ZnO composite material, and the ZnWO4 / ZnO composite material is obtained by adding ZnO graded microspheres to ammonium metatungstate solution, and after ultrasonic reaction, the reactant is dried and calcined. The optimal working temperature of the sensor is only 160°C, and it has good linearity at 0.5~40ppm and high sensitivity (Ra / Rg).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor oxide gas sensors, and in particular to a triethylamine gas sensitive sensor based on a ZnWO4 / ZnO composite material and a preparation method thereof. Background Art

[0002] Triethylamine is a typical colorless, transparent volatile organic compound with a strong pungent odor. It can be used as a catalyst, solvent, dye and preservative. Long-term excessive exposure to triethylamine can damage human health. According to the standards of the Occupational Safety and Health Administration (OSHA), the concentration of triethylamine in the air should not exceed 10ppm by volume. The European Commission also recommends that the occupational exposure threshold of triethylamine is 1ppm. In addition, aquatic products such as fish and shellfish can also release trace amounts of triethylamine. As the freshness of aquatic products decreases, the concentration of released triethylamine gradually increases. Therefore, triethylamine can also be used as a marker to check the freshness of aquatic products.

[0003] Currently, metal oxide semiconductor gas sensors used for triethylamine detection generally have problems such as high operating temperature, low sensitivity, long response recovery time, and poor selectivity. For example, the invention patent with publication number CN113550025B uses zinc tungstate / zinc oxide heterogeneous nanofibers prepared by electrospinning as gas-sensitive materials and laminates them on the sensor substrate. The optimal operating temperature is 350°C. The operating temperature is high, the preparation method is complex, and under the condition of triethylamine gas concentration of 50ppm, the sensitivity (Ra / Rg) is only between 100 and 120. Summary of the invention

[0004] Based on this, the present invention provides a triethylamine gas sensor based on ZnWO4 / ZnO composite material. The optimal operating temperature of the sensor is only 160°C, and it has good linearity in the range of 0.5-40ppm and high sensitivity (Ra / Rg).

[0005] The present invention adopts the following technical scheme: a triethylamine gas sensor based on ZnWO4 / ZnO composite material, comprising an insulating ceramic tube, electrodes are respectively provided at both ends of the surface of the insulating ceramic tube, a heating wire is passed through the interior of the insulating ceramic tube, the electrodes and the heating wire are respectively connected to the electrodes on the sensor base, the surfaces of the electrodes and the surfaces of the insulating ceramic tube between the electrodes are coated with ZnWO4 / ZnO composite material, the ZnWO4 / ZnO composite material is obtained by adding ZnO graded microspheres to an ammonium metatungstate solution, and after ultrasonic reaction, the reactant is dried and calcined.

[0006] As a preferred embodiment, the preparation method of the ZnWO4 / ZnO composite material is as follows: adding ZnO graded microspheres to an ammonium metatungstate solution, washing the product after ultrasonic reaction for 0.5 to 10 hours, then collecting it by centrifugation, drying it at 60 to 90°C, and calcining it in air at 300 to 800°C.

[0007] Furthermore, the preparation method of the ZnO graded microspheres is as follows: zinc nitrate solution, hexamethylenetetramine solution and sodium citrate solution are mixed and stirred evenly, and then a hydrothermal reaction is carried out at 80-150° C. The hydrothermal reaction product is cooled and washed, and then centrifuged and collected, dried at 60-90° C., and then annealed in air at 300-500° C. to obtain the microspheres.

[0008] As a preferred embodiment, zinc nitrate is calculated as zinc nitrate hexahydrate, sodium citrate is calculated as sodium citrate dihydrate, and the molar ratio of zinc nitrate hexahydrate, hexamethylenetetramine, and sodium citrate dihydrate is (1-30):(1-30):1; the mass ratio of ZnO graded microspheres to ammonium metatungstate is 1:(2-40).

[0009] As a preferred implementation, the insulating ceramic tube is an alumina insulating ceramic tube, the electrode is a gold electrode, the heating wire is a nickel-chromium heating wire, and the gold electrode is led out by a platinum wire pin and connected to the electrode on the sensor base.

[0010] Furthermore, the preparation method of the triethylamine gas sensor based on the ZnWO4 / ZnO composite material is as follows: the ZnWO4 / ZnO composite material is ground with ethanol to form a paste slurry, and then a small amount of the slurry is evenly coated on the surface of the insulating ceramic tube with a brush, and the electrode on the surface of the ceramic tube is covered to form a coating film of 15 to 30 μm, and then it is baked and sintered under an infrared lamp; then the sintered insulating ceramic tube is welded to the base, and a heating wire is inserted into the inside of the insulating ceramic tube, and the electrode and the heating wire are respectively welded to the electrode on the base to obtain a gas sensitive element; after the gas sensitive element is aged, the triethylamine gas sensor is obtained.

[0011] As a preferred implementation, the baking time is 10 to 20 minutes, the sintering temperature is 300 to 350° C., and the sintering time is 1 to 2 hours.

[0012] As a preferred implementation, the aging conditions are: aging at 160-280° C. for 2-7 days.

[0013] As a preferred embodiment, the mass volume ratio of the ZnWO4 / ZnO composite material when mixed with ethanol is 6-12 mg:20 μL.

[0014] As a preferred embodiment, the coating thickness of the ZnWO4 / ZnO composite material is 15-30 μm.

[0015] Compared with the prior art, the core advantages of the present invention are:

[0016] (1) The sensitivity is best at 160°C, the operating temperature is much lower than the existing technology, and it has good linearity between 0.5 and 40 ppm. Under the optimal working temperature and different gas concentration conditions, the sensitivity (Ra / Rg) is much higher than the existing technology;

[0017] (2) ZnWO4 / ZnO composite graded microsphere materials can be prepared by the hydrothermal method. The method is simple, low-cost, highly repeatable, and suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The scanning electron microscope morphology images of the ZnO graded microspheres and the ZnWO4 / ZnO composite graded microspheres in the embodiments and comparative examples;

[0019] Figure 2 This is the XRD pattern of ZnWO4 / ZnO composite graded microspheres;

[0020] Figure 3 The working temperature-sensitivity curves of ZnO graded microsphere and ZnWO4 / ZnO composite graded microsphere sensors;

[0021] Figure 4 The response curve of the ZnWO4 / ZnO sensor prepared in Example 1 of the present invention to 0.5-40 ppm triethylamine at the optimal working temperature, and the repeated response curves to 20 ppm and 500 ppb triethylamine;

[0022] Figure 5 The linearity result of the ZnWO4 / ZnO sensor prepared in Example 1 of the present invention at the optimal working temperature;

[0023] Figure 6 The long-term stability and specificity test results of the ZnWO4 / ZnO sensor prepared in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0024] Based on the problems existing in the existing triethylamine gas sensors, the inventors firstly prepared ZnO nanomaterials with different morphologies such as nanorods, nanosheets, nanotubes, and graded microspheres by adding different molding agents using a hydrothermal method, and then composite modified them with ZnWO4 to finally obtain ZnWO4 / ZnO composite nanomaterials. After the above materials were used to prepare triethylamine gas sensors and tested, it was found that the triethylamine gas sensing performance of ZnWO4 / ZnO composite graded microspheres was better. After further research, the following technical scheme was finally determined: Based on The triethylamine gas sensor of ZnWO4 / ZnO composite material comprises an insulating ceramic tube, the two ends of the surface of the insulating ceramic tube are respectively provided with electrodes, a heating wire is inserted into the interior of the insulating ceramic tube, the electrodes and the heating wire are respectively connected to the electrodes on the sensor base, and the difference between the triethylamine gas sensor and the prior art is that the surface of the electrode and the surface of the insulating ceramic tube between the electrodes are coated with ZnWO4 / ZnO composite material, and the ZnWO4 / ZnO composite material is obtained by adding ZnO graded microspheres to ammonium metatungstate solution, and drying and calcining the reactants after ultrasonic reaction. The triethylamine gas sensor not only reduces the working temperature of the gas sensor, but also has a wider and lower detection range, better sensitivity (Ra / Rg), and can quickly and effectively identify triethylamine between 0.5 and 40 ppm.

[0025] In the present invention, the preparation method of the ZnWO4 / ZnO composite material is as follows: adding ZnO graded microspheres into an ammonium metatungstate solution, washing the product after ultrasonic reaction for 0.5 to 10 hours, then collecting the product by centrifugation, drying at 60 to 90° C., and calcining the product in air at 300 to 800° C.

[0026] The preparation method of ZnO graded microspheres is as follows: zinc nitrate solution, hexamethylenetetramine solution and sodium citrate solution are mixed and stirred evenly, and then hydrothermal reaction is carried out at 80-150°C. The hydrothermal reaction product is cooled and washed, and then centrifuged and collected. After drying at 60-90°C, annealing is carried out in air at 300-500°C. The process parameters of the hydrothermal reaction can be selected as follows: hydrothermal reaction at 80°C for 2 hours, hydrothermal reaction at 120°C for 4 hours, and hydrothermal reaction at 150°C for 6 hours, but are not limited thereto.

[0027] In the present invention, the ZnWO4 / ZnO composite material is preferably prepared by the above method, that is, firstly preparing three solutions A, B, and C of zinc nitrate solution, hexamethylenetetramine solution, and sodium citrate solution respectively, then mixing and stirring the three solutions, transferring them to a stainless steel high-pressure reactor containing a polytetrafluoroethylene liner, and then carrying out a hydrothermal reaction for 2 to 6 hours, and then cooling the hydrothermal product to room temperature, washing with deionized water and anhydrous ethanol, collecting by centrifugation at a speed of 3000 to 5000 r / min, drying and annealing the product to obtain ZnO graded microspheres; adding the ZnO graded microspheres to an ammonium metatungstate solution D, after ultrasonic reaction, also washing with deionized water and anhydrous ethanol, collecting by centrifugation at a speed of 3000 to 5000 r / min, drying the product and calcining it to obtain the product.

[0028] In the present invention, the ultrasonic time of ZnO graded microspheres in ammonium metatungstate solution D will have a certain influence on the performance of the gas sensor, and the preferred range is 0.5 to 10 hours, and the more preferred range is 1 to 9 hours. For example, 1 hour, 3 hours, 5 hours, 7 hours, and 9 hours can be selected, and the best is 5 hours. At this time, the sensitivity (Ra / Rg) of the prepared gas sensor is better.

[0029] In the above specific method, zinc nitrate is calculated as zinc nitrate hexahydrate, sodium citrate is calculated as sodium citrate dihydrate, and the molar ratio of zinc nitrate hexahydrate, hexamethylenetetramine and sodium citrate dihydrate is (1-30):(1-30):1, preferably (3-8):(3-8):1; the mass ratio of ZnO graded microspheres to ammonium metatungstate is 1:(2-40), preferably 1:(10-15).

[0030] The preparation method of the triethylamine gas sensor based on the ZnWO4 / ZnO composite material is as follows: grind the ZnWO4 / ZnO composite material with ethanol to form a paste slurry, then use a brush to dip a small amount of the paste and evenly apply it on the surface of the insulating ceramic tube, and cover the electrode on the surface of the ceramic tube to form a coating film of 15-30 μm, and then bake and sinter under an infrared lamp;

[0031] Then, the sintered insulating ceramic tube is welded to the base, and a heating wire is inserted into the inside of the tube. The electrode and the heating wire are respectively welded to the electrode on the base to obtain a gas sensor.

[0032] After aging treatment of the gas sensitive element, the triethylamine gas sensitive sensor is obtained.

[0033] Among them, the baking time is 10~20 minutes, the sintering temperature is 300~350℃, and the sintering time is 1~2 hours; the aging conditions are: aging at 160~280℃ for 2~7 days; the mass volume ratio of ZnWO4 / ZnO composite material and ethanol when mixed is 6~12 mg:20μL.

[0034] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand the present invention more clearly.

[0035] The following embodiments are only used to illustrate the present invention, but are not limited to the scope of the present invention. Based on the specific embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work belong to the protection scope of the present invention.

[0036] In the examples of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; in the examples of the present invention, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art. In the examples of the present invention, the raw materials used are conventional commercial products.

[0037] Example 1

[0038] The embodiment of the present invention provides a triethylamine gas sensor based on ZnWO4 / ZnO composite material and a preparation method thereof, which are specifically as follows:

[0039] 0.8924 g of zinc nitrate hexahydrate was dissolved in 100 mL of deionized water and stirred to obtain solution A; 0.4206 g of hexamethylenetetramine was dissolved in 100 mL of deionized water and stirred to obtain solution B; 0.1680 g of sodium citrate dihydrate was dissolved in 100 mL of deionized water and stirred to obtain solution C;

[0040] The solution A, solution B and solution C were mixed and stirred evenly, transferred to a stainless steel high-pressure reactor with a polytetrafluoroethylene liner, and placed in an oven for hydrothermal reaction at 150 °C for 2 hours;

[0041] The hydrothermal product was cooled to room temperature, washed with deionized water and anhydrous ethanol for 5 times, collected by centrifugation at 5000 r / min, dried at 90 °C for 10 hours, and then air annealed at 400 °C for 2 hours to obtain ZnO graded microspheres.

[0042] 3.5 g of ammonium metatungstate was dissolved in 20 mL of deionized water and stirred to obtain solution D. 0.25 g of ZnO graded microspheres was added to solution D and ultrasonically reacted for 5 hours.

[0043] The above products were washed with deionized water and anhydrous ethanol for 5 times, collected by centrifugation at 5000 r / min, and dried at 90 °C for 10 hours; finally, they were calcined in air at 450 °C for 2 hours to obtain ZnWO4 / ZnO composite hierarchical microsphere sensitive material (labeled as ZnWO4 / ZnO-5).

[0044] The calcined ZnWO4 / ZnO composite graded microsphere sensitive material was mixed evenly with ethanol in a mortar to form a paste slurry. The mixing ratio of the sensitive material to ethanol was 0.5 mg: 1 mL. A small amount of slurry was applied evenly on the surface of the alumina ceramic tube with a brush to cover the gold electrode on the surface of the ceramic tube to form a 25 μm thick sensitive material coating. After coating, the ceramic tube was baked under an infrared lamp for 10 minutes, and then the ceramic tube was sintered at 300 °C for 2 hours;

[0045] The sintered alumina ceramic tube was welded on a six-legged base, and a nickel-chromium heating wire was inserted into the ceramic tube. The gold electrode and the nickel-chromium heating wire were welded to the electrode on the sensor base, respectively, to obtain a triethylamine gas sensor based on ZnWO4 / ZnO composite graded microsphere sensitive material.

[0046] The gas sensor was placed on an aging bench, the heating voltage was adjusted to 4.5 V, and it was aged at 280 °C for 3 days before the gas sensing test was performed.

[0047] Example 2

[0048] The embodiment of the present invention provides a triethylamine gas sensor based on a ZnWO4 / ZnO composite material and a preparation method thereof, which is different from Example 1 in that during the preparation of the ZnWO4 / ZnO composite graded microsphere sensitive material, the ultrasonic reaction time of the ZnO graded microspheres in solution D is 1 hour, and the obtained ZnWO4 / ZnO composite graded microsphere sensitive material is marked as ZnWO4 / ZnO-1. The device preparation method and test method are consistent with those of Example 1.

[0049] Example 3

[0050] The embodiment of the present invention provides a triethylamine gas sensor based on a ZnWO4 / ZnO composite material and a preparation method thereof, which is different from Example 1 in that during the preparation of the ZnWO4 / ZnO composite graded microsphere sensitive material, the ultrasonic reaction time of the ZnO graded microspheres in solution D is 3 hours, and the obtained ZnWO4 / ZnO composite graded microsphere sensitive material is marked as ZnWO4 / ZnO-3. The device preparation method and test method are consistent with those in Example 1.

[0051] Example 4

[0052] The embodiment of the present invention provides a triethylamine gas sensor based on a ZnWO4 / ZnO composite material and a preparation method thereof, which is different from Example 1 in that during the preparation of the ZnWO4 / ZnO composite graded microsphere sensitive material, the ultrasonic reaction time of the ZnO graded microspheres in solution D is 7 hours, and the obtained ZnWO4 / ZnO composite graded microsphere sensitive material is marked as ZnWO4 / ZnO-7. The device preparation method and test method are consistent with those in Example 1.

[0053] Example 5

[0054] The embodiment of the present invention provides a triethylamine gas sensor based on a ZnWO4 / ZnO composite material and a preparation method thereof, which is different from Example 1 in that during the preparation of the ZnWO4 / ZnO composite graded microsphere sensitive material, the ultrasonic reaction time of the ZnO graded microspheres in solution D is 9 hours, and the obtained ZnWO4 / ZnO composite graded microsphere sensitive material is marked as ZnWO4 / ZnO-9. The device preparation method and test method are consistent with those of Example 1.

[0055] Comparative Example 1

[0056] A triethylamine gas sensor based on ZnO material and a preparation method thereof, which is different from Example 1 in that the prepared ZnO graded microspheres are directly used for the preparation and testing of the device.

[0057] Performance Test:

[0058] The ZnO graded microsphere materials and ZnWO4 / ZnO composite materials prepared in the above examples and comparative examples were analyzed. Figure 1 , 2 shown. Figure 1 These are scanning electron microscope morphology images, where a is ZnO, and b is (b) ZnWO4 / ZnO-1; (c) ZnWO4 / ZnO-3; (d) ZnWO4 / ZnO-5; (e) ZnWO4 / ZnO-7; and (f) ZnWO4 / ZnO-9. Figure 2 is the XRD pattern.

[0059] The working temperature and sensitivity of the gas sensors prepared in the above examples and comparative examples were tested. The specific method is as follows: the triethylamine gas sensor is placed in a gas-sensitive test box. In the working temperature range of 120-240°C, the triethylamine gas sensor is switched back and forth between the triethylamine gas of the same concentration of 30 ppm and dry air. The dynamic switching resistance curve under different working temperatures is tested. The duration of each switch is 200 seconds. The sensitivity is defined as: sensitivity = resistance value between two gold electrodes in air / resistance value between two gold electrodes in triethylamine. The results are as follows Figure 3As shown. Figure 3 It can be seen that the sensitivity of the sensors prepared using ZnWO4 / ZnO composite materials is higher than that of the sensors prepared using ZnO graded microsphere materials, and the sensitivity of the sensors prepared using ZnWO4 / ZnO composite materials is the best at 160°C.

[0060] The gas sensor prepared in Example 1 was analyzed for its detection range. The results are as follows: Figure 4 shown. Figure 4 Figures a and b are the dynamic response curves of ZnWO4 / ZnO-5 sensor to 0.5~40ppm at the optimal working temperature of 160℃. Figure 5 This is a linear result. From this result, we can see that the sensor has a good linear relationship in the range of 0.5~40ppm. Figure 4 Figures c and d are the repeated response curves of the ZnWO4 / ZnO-5 sensor to gas concentrations of 20ppm and 500ppb. From the results, it can be seen that the sensor has good response recovery characteristics and its sensitivity remains stable.

[0061] The long-term stability and specificity of the gas sensor ZnWO4 / ZnO-5 prepared in Example 1 were analyzed, wherein the gas concentration was 30 ppm. Figure 5 As shown. Figure 6 Figure a is the long-term stability analysis result obtained by testing every 5 days under the condition of 30 ppm gas concentration. It can be seen from the result that after 30 days, the sensitivity result has hardly decreased, indicating that the sensor has excellent stability. Figure 6 Figure b is the specific analysis result of the sensor in different gases. It can be seen from the results that the sensor only shows extremely high sensitivity to triethylamine, which is about 15 to 70 times the sensitivity of methanol, acetone, formaldehyde, isopropanol, ethanol, and ethylene glycol.

[0062] It is necessary to point out that the above embodiments are limited to further elaboration and explanation of the technical solution of the present invention, and are not further limitations of the technical solution of the present invention. The method of the present invention is only a preferred implementation scheme, and is not used to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A triethylamine gas sensor based on ZnWO4 / ZnO composite material, comprising an insulating ceramic tube, electrodes are provided at both ends of the surface of the insulating ceramic tube, a heating wire is passed through the interior of the insulating ceramic tube, and the electrodes and the heating wire are respectively connected to the electrodes on the sensor base, characterized in that: The preparation method of the triethylamine gas sensor is as follows: ZnWO4 / ZnO composite material and ethanol are mixed at a mass volume ratio of 0.5 mg:1 mL and then ground to form a paste slurry, then a small amount is dipped with a brush and evenly coated on the surface of an insulating ceramic tube, and the electrode on the surface of the ceramic tube is covered to form a 25 μm thick coating, and then baked under an infrared lamp for 10 minutes, and then sintered at 300°C for 2 hours; then the sintered insulating ceramic tube is welded to a base, and a heating wire is inserted into the inside thereof, and the electrode and the heating wire are respectively welded to the electrode on the base to obtain a gas sensitive element; after aging the gas sensitive element, the triethylamine gas sensor is obtained; The preparation method of the ZnWO4 / ZnO composite material is as follows: ZnO graded microspheres are added to an ammonium metatungstate solution, and the product is washed after ultrasonic reaction for 5 hours, and then centrifuged and collected, dried at 60-90°C, and calcined in air at 450°C for 2 hours.

2. The triethylamine gas sensor based on ZnWO4 / ZnO composite material according to claim 1, characterized in that: The preparation method of the ZnO graded microspheres is as follows: zinc nitrate solution, hexamethylenetetramine solution and sodium citrate solution are mixed and stirred evenly, and then a hydrothermal reaction is carried out at 80-150° C. The hydrothermal reaction product is cooled and washed, and then centrifuged and collected, dried at 60-90° C., and then annealed in air at 300-500° C. to obtain the microspheres.

3. The triethylamine gas sensor based on ZnWO4 / ZnO composite material according to claim 2, characterized in that: Zinc nitrate is calculated as zinc nitrate hexahydrate, sodium citrate is calculated as sodium citrate dihydrate, and the molar ratio of zinc nitrate hexahydrate, hexamethylenetetramine and sodium citrate dihydrate is (1-30):(1-30):1; the mass ratio of ZnO graded microspheres to ammonium metatungstate is 1:(2-40).

4. The triethylamine gas sensor based on ZnWO4 / ZnO composite material according to any one of claims 1 to 3, characterized in that: The insulating ceramic tube is an alumina insulating ceramic tube, the electrode is a gold electrode, the heating wire is a nickel-chromium heating wire, and the gold electrode is led out by a platinum wire pin and connected to the electrode on the sensor base.

5. The triethylamine gas sensor based on ZnWO4 / ZnO composite material according to claim 1, characterized in that: Aging conditions: aging at 160~280℃ for 2~7 days.